Anti-reflection film
By adopting a combined structure of a low refractive index layer and a high refractive index layer in the anti-reflective film, and using a combination of silicon, carbon, fluorine and oxide materials, the problem of both hardness and flexibility in flexible displays is solved, and the tension is achieved. Effective suppression of tensile stress and improvement of anti-reflective and scratch resistance.
Patent Information
- Application Number
- CN202380012409.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-01-30
- Filing Date
- 2023-09-13
- Publication Date
- 2024-10-01
AI Technical Summary
When existing anti-reflective films are used in flexible displays, it is difficult to balance hardness and flexibility, and are prone to cracks especially when facing tensile stress.
It adopts a combined structure of a low refractive index layer and a high refractive index layer. The low refractive index layer contains silicon, carbon, fluorine and oxygen. Indium, tin or bismuth is added to form a fluoroalkyl bond through organic fluorine bonds and oxide materials. To disperse the tensile force, and improve the scratch resistance and anti-reflection of the film through laminate structure and sputtering technology.
It is possible to suppress cracks under tensile stress while maintaining anti-reflection and scratch resistance, significantly improving the durability of the flexible display surface.
Smart Images

Figure CN118742829A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an antireflection film. Background Art
[0002] As an antireflection film applied to the surface of a liquid crystal display or the like, it is known that a high refractive index layer and a low refractive index layer are alternately laminated, and the outermost layer of the antireflection film is a low refractive index layer in order to reduce reflection at the air interface (see
[0046] of Patent Document 1).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2022-65437 Summary of the invention
[0006] Problems to be solved by the invention
[0007] Thin films applied to the surface of liquid crystal displays, such as the anti-reflection films of the prior art, need to have sufficient hardness to ensure scratch resistance in addition to their inherent anti-reflection properties. However, when anti-reflection films are applied to flexible displays such as flexible displays, in addition to hardness, they also need to have a pliability (toughness) that does not cause cracks even when tensile stress is applied, and it is difficult to achieve both hardness and pliability.
[0008] An object of the present invention is to provide an antireflection film which has antireflection properties and scratch resistance and can suppress the generation of cracks due to tensile stress.
[0009] Means for solving problems
[0010] The first solution solves the above-mentioned problems by an antireflection film having, as an outermost layer, a low refractive index layer having a refractive index lower than that of the substrate on a surface of the substrate,
[0011] The low refractive index layer contains silicon, carbon, fluorine and oxygen as essential components, and further contains at least one of indium, tin and bismuth as an essential component, has silicon oxide as a main component, and contains an organic fluorine compound.
[0012] The second solution solves the above-mentioned problem by an antireflection film comprising one or more layers of a low refractive index layer having a lower refractive index than that of the substrate and a high refractive index layer having a higher refractive index than that of the substrate, stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer.
[0013] The high refractive index layer contains niobium, carbon, fluorine and oxygen as essential components, and at least one of indium, tin or bismuth as an essential component, has niobium oxide as a main component, and contains an organic fluorine compound, or
[0014] The present invention contains cerium, carbon, fluorine and oxygen as essential components, further contains at least one of indium, tin and bismuth as an essential component, has cerium oxide as a main component, and contains an organic fluorine compound.
[0015] The third solution solves the above-mentioned problem by an antireflection film comprising one or more layers of a low refractive index layer having a lower refractive index than that of the substrate and a high refractive index layer having a higher refractive index than that of the substrate, stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer.
[0016] The low refractive index layer is further provided between the substrate and the high refractive index layer closest to the substrate.
[0017] The low refractive index layer contains silicon, carbon, fluorine and oxygen as essential components, and further contains at least one of indium, tin and bismuth as an essential component, has silicon oxide as a main component, and contains an organic fluorine compound.
[0018] The fourth solution solves the above-mentioned problem by an antireflection film comprising one or more layers of a low refractive index layer having a lower refractive index than that of the substrate and a high refractive index layer having a higher refractive index than that of the substrate, stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer.
[0019] The low refractive index layer is further provided between the substrate and the high refractive index layer closest to the substrate.
[0020] The high refractive index layer contains niobium, carbon, fluorine and oxygen as essential components, and at least one of indium, tin or bismuth as an essential component, has niobium oxide as a main component, and contains an organic fluorine compound, or
[0021] The present invention contains cerium, carbon, fluorine and oxygen as essential components, further contains at least one of indium, tin and bismuth as an essential component, has cerium oxide as a main component, and contains an organic fluorine compound.
[0022] Effects of the Invention
[0023] In the present invention, the carbon and fluorine contained in the low refractive index layer or the high refractive index layer are bonded to each other, and exist in the low refractive index layer or the high refractive index layer in a state of forming an organic fluorine bond such as a fluoroalkyl. If an external force in the tensile direction is applied to the low refractive index layer or the high refractive index layer, the organic fluorine bond expands and contracts, and the force applied to the entire layer is dispersed, thereby suppressing the generation of cracks. In addition, by adding indium, tin or bismuth, the refractive index and transmission characteristics of the layer can be adjusted. In addition, by utilizing the interference generated by the combination of the low refractive index layer and the high refractive index layer, anti-reflection can be ensured, and scratch resistance can be ensured by the oxide of silicon, niobium or cerium. As a result, according to the present invention, in addition to having anti-reflection and scratch resistance, crack generation for tensile stress can also be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a cross-sectional view showing a first embodiment of the antireflection film of the present invention.
[0025] Figure 2 It is a cross-sectional view showing a second embodiment of the antireflection film of the present invention.
[0026] Figure 3 It is a cross-sectional view showing a third embodiment of the antireflection film of the present invention.
[0027] Figure 4 This is a cross-sectional view showing an example of a sputtering device for producing the antireflection film of the present invention. DETAILED DESCRIPTION
[0028] Hereinafter, embodiments of the present invention will be described based on the accompanying drawings. The present invention is an antireflection film formed on the surface of a substrate, including the first to fourth embodiments. The first embodiment is an antireflection film having a low refractive index layer as an outermost layer on the surface of the substrate, the low refractive index layer containing a specific composition, namely silicon, carbon, fluorine and oxygen as essential components, and at least one of indium, tin or bismuth as an essential component. The first embodiment can be typically embodied as Figure 1 The membrane structure shown is therefore Figure 1 The first embodiment will be described below.
[0029] The second solution is an antireflection film, wherein one or more low refractive index layers having a refractive index lower than that of the substrate and high refractive index layers having a refractive index higher than that of the substrate are stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer, and the high refractive index layer contains a specific composition, namely, niobium, carbon, fluorine and oxygen as essential components, and also contains at least one of indium, tin or bismuth as an essential component; or contains cerium, carbon, fluorine and oxygen as essential components, and also contains at least one of indium, tin or bismuth as an essential component. The second solution can be typically embodied as follows Figure 2 or Figure 3 The membrane structure shown in any one of the above is thus Figure 2 The second embodiment will be described below.
[0030] The third embodiment is an antireflection film, wherein one or more layers of a low refractive index layer having a refractive index lower than that of the substrate and a high refractive index layer having a refractive index higher than that of the substrate are stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer, and the low refractive index layer is further provided between the substrate and the high refractive index layer closest to the substrate, wherein the low refractive index layer contains a specific composition, namely silicon, carbon, fluorine and oxygen as essential components, and further contains at least one of indium, tin or bismuth as an essential component. The third embodiment can be typically embodied as follows: Figure 3 The membrane structure shown is therefore Figure 3 The third embodiment will be described below.
[0031] The fourth embodiment is an antireflection film, wherein one or more low refractive index layers having a refractive index lower than that of the substrate and high refractive index layers having a refractive index higher than that of the substrate are stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer, and the low refractive index layer is further provided between the substrate and the high refractive index layer closest to the substrate, and the high refractive index layer contains a specific composition, namely, niobium, carbon, fluorine and oxygen as essential components, and also contains at least one of indium, tin or bismuth as an essential component; or, contains cerium, carbon, fluorine and oxygen as essential components, and also contains at least one of indium, tin or bismuth as an essential component. The fourth embodiment can be typically embodied as Figure 3 The membrane structure shown is therefore Figure 3 The fourth embodiment is described below.
[0032] The substrates of the first to fourth embodiments are not particularly limited, and substrates of various materials such as inorganic glass substrates and other inorganic material substrates, organic glass substrates and other plastic material substrates, stainless steel and other metal material substrates can be used. Among them, inorganic material substrates or plastic material substrates are often used as a part of optical elements, so when the anti-reflection film of the present invention is applied to these inorganic material substrates or plastic material substrates, especially flexible substrates, the effect is remarkable.
[0033] 《First Implementation Method》
[0034] Figure 1 2 is a cross-sectional view showing the first embodiment of the anti-reflection film of the present invention. The anti-reflection film 2 of this embodiment is a thin film formed on the surface of the substrate 1, and is a low refractive index layer 21 showing a refractive index n1 lower than the refractive index n0 of the substrate 1. The low refractive index layer 21 of this embodiment is directly formed on the surface of the substrate 1 and is formed as the outermost layer. The film thickness of the low refractive index layer 21 of this embodiment is not particularly limited. It should be noted that in this specification, the outermost layer refers to a layer formed on the outermost side when observed from the substrate 1, and a layer on the outermost side is not formed with a thin film.
[0035] The low refractive index layer 21 having a refractive index n1 lower than the refractive index n0 of the substrate 1 means that, for example, when the refractive index n0 of the substrate 1 made of inorganic glass is 1.52, the refractive index n1 of the low refractive index layer 21 of the present embodiment is less than 1.52.
[0036] In particular, the low refractive index layer 21 of the present embodiment is a film containing silicon (Si), carbon (C), fluorine (F) and oxygen (O) as essential components, and also containing at least any one of indium (In), tin (Sn) or bismuth (Bi). The mixing ratio of silicon, carbon, fluorine and oxygen as essential components is not particularly limited. Indium, tin, and bismuth can contain at least one as an essential component, so more than two kinds can be included. In addition, the mixing ratio of these indium, tin, and bismuth is not particularly limited. As an example of the low refractive index layer 21 of the present embodiment, a film with silicon oxide as the main component and a part of which is substituted by an organic fluorine compound and containing a trace amount of indium, tin or bismuth can be exemplified.
[0037] The low refractive index layer 21 formed on the surface of the substrate 1 can be formed by a sputtering method in which the target is set to silicon oxide-polytetrafluoroethylene containing indium. The target comprises silicon oxide (SiO2), polytetrafluoroethylene ((C2F4)n), and indium (In), so that silicon (Si), carbon (C), fluorine (F), oxygen (O), and indium (In) are contained in the sputtered film as necessary components. It should be noted that if tin (Sn) and / or bismuth (Bi) are contained in addition to the indium contained in the target, and the target is used for sputtering treatment, then in the obtained film, tin and / or bismuth are contained in addition to indium instead of indium. When making a sputtered target, the strength of the target can be improved by using indium, tin or bismuth as a sintering aid.
[0038] <<Second Implementation Method>>
[0039] Figure 2 2 is a cross-sectional view showing the second embodiment of the anti-reflection film of the present invention. The anti-reflection film 2 of the present embodiment is a thin film formed on the surface of a substrate 1, and one or more layers of low refractive index layers 21 showing a refractive index n1 lower than the refractive index n0 of the substrate 1 and high refractive index layers 22 showing a refractive index n2 higher than the refractive index n0 of the substrate 2 are stacked in such a way that the low refractive index layer 21 becomes the outermost layer. Here, the pair of low refractive index layers 21 and high refractive index layers 22 can be a pair of stacking or a plurality of pairs of stacking. The film thickness and film thickness ratio of the low refractive index layer 21 and the high refractive index layer 22 of the present embodiment are not particularly limited.
[0040] The low refractive index layer 21 showing a refractive index n1 lower than the refractive index n0 of the substrate 1 means that, for example, when the refractive index n0 of the substrate 1 made of inorganic glass is 1.52, the refractive index n1 of the low refractive index layer 21 of the present embodiment is less than 1.52. In addition, the high refractive index layer 22 showing a refractive index n2 higher than the refractive index n0 of the substrate 1 means that, for example, when the refractive index n0 of the substrate 1 made of inorganic glass is 1.52, the refractive index n2 of the high refractive index layer 22 of the present embodiment exceeds 1.52.
[0041] In particular, the high refractive index layer 22 of the present embodiment contains niobium (Nb), carbon, fluorine and oxygen as essential components, and also contains at least one of indium, tin or bismuth as an essential component, or contains cerium (Ce), carbon, fluorine and oxygen as essential components, and also contains at least one of indium, tin or bismuth as an essential component. The mixing ratio of niobium, carbon, fluorine and oxygen as essential components, or the mixing ratio of cerium, carbon, fluorine and oxygen is not particularly limited. Indium, tin and bismuth can contain at least one as an essential component, so more than two kinds can be included. In addition, the mixing ratio of these indium, tin and bismuth is not particularly limited. As an example of the high refractive index layer 22 of the present embodiment, a film with niobium oxide as the main component and a part of it being replaced by an organic fluorine compound and containing a trace amount of indium, tin or bismuth can be exemplified. In addition, a film with cerium oxide as the main component and a part of it being replaced by an organic fluorine compound and containing a trace amount of indium, tin or bismuth can be exemplified.
[0042] The low refractive index layer 21 of this embodiment may be a thin film containing silicon, carbon, fluorine, and oxygen as essential components and further containing at least one of indium, tin, and bismuth, but is not limited thereto and may have other compositions.
[0043] The antireflection film 2 of this embodiment can be used Figure 4 The sputtering device 3 shown uses silicon oxide-polytetrafluoroethylene containing indium as the first target and niobium or niobium oxide (or cerium or cerium oxide) as the second target, and forms a film by radical assisted sputtering (RAS) using oxygen as a radical source.
[0044] Here, it is explained Figure 4 The antireflection film 2 of the present invention is preferably formed by using Figure 4The film is formed by sputtering using the sputtering device 3 shown in the figure. In particular, in addition to the effect of adjusting the refractive index of the film, indium, tin or bismuth can improve the strength of the target material by being used as a sintering aid for the sputtering target material. As a result, sputtering can be performed at high power, which can improve the productivity of the film forming process. It should be noted that as other film forming methods, for example, CVD (Chemical Vapor Deposition) method, ALD (Atomic Layer Deposition) method, PLD (Pulsed Laser Deposition) method, vacuum evaporation method, etc. can also be used for film formation.
[0045] Figure 4 1 is a cross-sectional view showing an example of a sputtering device for forming an anti-reflection film 2 of the present invention. The sputtering device 3 of this example is a device capable of implementing a radical assisted sputtering (RAS) method, and is provided with a vacuum chamber 31 which is a substantially rectangular hollow body. An exhaust pipe and a vacuum pump (not shown) are connected to the vacuum chamber 31, and the interior of the vacuum chamber 31 can be set and maintained at a predetermined vacuum degree. In addition, a cylindrical substrate holder 32 is rotatably provided inside the vacuum chamber 31, and a substrate 1 as a film forming object is held on its outer peripheral surface.
[0046] Two sputtering sources 33, 34 and a plasma source 35 are arranged around a substrate holder 32 disposed inside a vacuum chamber 31. Each sputtering source 33, 34 includes an electrode such as a magnetron sputtering electrode, and a target is mounted on the surface of each electrode during film formation. AC power supplies 331, 341 are connected to each electrode via a transformer that adjusts electric energy, and, for example, an AC voltage of about 1k to 100kHz is applied. The plasma source 35 of this example includes: a housing 351 fixed in a manner to block an opening formed on the wall surface of the vacuum chamber 31; and a dielectric module 352 including an antenna fixed to the housing 351. The dielectric module 352 including an antenna is connected to a high-frequency power supply 353. In addition, the antenna receives power from the high-frequency power supply 353 to generate an induced electric field inside the vacuum chamber 31, thereby generating plasma.
[0047] A film forming process area 332 is formed on the front surface of the sputtering source 33, and a film forming process area 342 is formed on the front surface of the sputtering source 34. One film forming process area 332 is surrounded by a partition wall 333 protruding from the inner wall of the vacuum chamber 31 toward the substrate holder 32, and is divided into four independent spaces that can be ensured inside the vacuum chamber 31. The other film forming process area 342 is also surrounded by a partition wall 343 protruding from the inner wall of the vacuum chamber 31 toward the substrate holder 32, and is divided into four independent spaces that can be ensured inside the vacuum chamber 31.
[0048] Similarly, a reaction process area 354 is formed on the front surface of the plasma source 35. The reaction process area 354 is also surrounded by partition walls 355 protruding from the inner wall of the vacuum chamber 31 toward the substrate holder 32 in the same manner as the film forming process areas 332 and 342, and a space independent of the film forming process areas 332 and 342 is ensured inside the vacuum chamber 31. In the sputtering device 3 of this example, the processes in the film forming process areas 332 and 342 and the reaction process area 354 are configured to be independently controllable.
[0049] It should be noted that each sputtering source 33, 34 is connected to a sputtering gas supply system, and the flow rate of the supplied sputtering gas is adjusted by a mass flow controller and introduced into each film forming process area 332, 342 through a pipe. In addition, a reaction treatment gas supply system 356 is connected to the plasma source 35, and the flow rate of the supplied reaction treatment gas is adjusted by a mass flow controller and introduced into the reaction process area 354 through a pipe. Figure 4 In the figure, reference numeral 36 denotes a load lock chamber, which is disposed adjacent to the vacuum chamber 31 and is used for switching the atmosphere pressure to carry in and carry out substrates before and after processing.
[0050] In order to use the sputtering device 3 of this configuration, Figure 2 The low refractive index layer 21 and the high refractive index layer 22 are stacked on the surface of the substrate 1 shown in the figure. First, silicon oxide-polytetrafluoroethylene containing indium as a target material for the low refractive index layer 21 is installed at the electrode of one sputtering source 33, and niobium or niobium oxide (or cerium or cerium oxide) as a target material for the high refractive index layer 22 is installed at the electrode of another sputtering source 34. Then, the interior of the vacuum chamber 31 is set to, for example, 10 -1 ~10 -5 Under a high vacuum of about Pa, while the substrate holder 32 holding the substrate 1 is rotated at a constant speed, an inert gas as a sputtering gas is supplied to the two film forming process areas 332 and 342 , and oxygen gas as a reaction gas is supplied to the reaction process area 354 .
[0051] Furthermore, when the low refractive index layer 21 is formed on the surface of the substrate 1, power from the AC power supply is supplied to one sputtering source 33 of the target material (silicon oxide-polytetrafluoroethylene containing indium) on which the low refractive index layer 21 is mounted. Thus, the low refractive index layer 21 is formed on the surface of the substrate 1 by the sputtering process in one film forming process area 332. The film forming process is continued for a predetermined time to form the low refractive index layer 21 of a predetermined film thickness, and thus the supply of power from the AC power supply to one sputtering source 33 is stopped.
[0052] Next, power from an AC power source is supplied to another sputtering source 34 on which a target material (niobium or niobium oxide (or cerium or cerium oxide)) of a high refractive index layer 22 is mounted, and power from a high frequency power source is supplied to a plasma source 35, whereby an intermediate thin film of the high refractive index layer 22 is formed on the surface of the substrate 1 through a continuous sputtering process in a film forming process area 342, and the intermediate thin film is converted into an ultra-thin film through a subsequent plasma exposure process in a reaction process area 354. Furthermore, by repeatedly performing a sputtering process and a plasma exposure process, a next ultra-thin film is deposited on the ultra-thin film, and such a process is repeated until the final high refractive index layer 22 is formed.
[0053] 《Third Implementation Method》
[0054] Figure 3 2 is a cross-sectional view showing the third embodiment of the anti-reflection film of the present invention. The anti-reflection film 2 of this embodiment is a thin film formed on the surface of a substrate 1, and one or more layers of low refractive index layers 21 showing a refractive index n1 lower than the refractive index n0 of the substrate 1 and high refractive index layers 22 showing a refractive index n2 higher than the refractive index n0 of the substrate 2 are stacked in a manner such that the low refractive index layer 21 becomes the outermost layer, and further, a low refractive index layer 21 is also provided between the substrate 1 and the high refractive index layer 22 closest to the substrate 1 side. Here, the pair of low refractive index layers 21 and high refractive index layers 22 can be a pair of stacking or a plurality of pairs of stacking. The film thickness and film thickness ratio of the low refractive index layer 21 and the high refractive index layer 22 of this embodiment are not particularly limited.
[0055] The low refractive index layer 21 showing a refractive index n1 lower than the refractive index n0 of the substrate 1 means that, for example, when the refractive index n0 of the substrate 1 made of inorganic glass is 1.52, the refractive index n1 of the low refractive index layer 21 of the present embodiment is less than 1.52. In addition, the high refractive index layer 22 showing a refractive index n2 higher than the refractive index n0 of the substrate 1 means that, for example, when the refractive index n0 of the substrate 1 made of inorganic glass is 1.52, the refractive index n2 of the high refractive index layer 22 of the present embodiment exceeds 1.52.
[0056] Regarding the composition of the low refractive index layer 21 and the high refractive index layer 22 constituting the anti-reflection film 2 of the present embodiment, at least the low refractive index layer 21 is a thin film containing silicon, carbon, fluorine and oxygen as essential components, and also containing at least any one of indium, tin or bismuth; or, at least the high refractive index layer 22 is a thin film containing niobium, carbon, fluorine and oxygen as essential components, and also containing at least any one of indium, tin or bismuth as an essential component, or, it can be a thin film containing cerium, carbon, fluorine and oxygen as essential components, and also containing at least any one of indium, tin or bismuth as an essential component.
[0057] That is, when one or more low-refractive index layers 21 constituting the anti-reflection film 2 are thin films containing silicon, carbon, fluorine, and oxygen as essential components and at least one of indium, tin, or bismuth, the composition of the high-refractive index layer 22 is not particularly limited. In addition, when one or more high-refractive index layers 22 constituting the anti-reflection film 2 are thin films containing niobium, carbon, fluorine, and oxygen as essential components and at least one of indium, tin, or bismuth as essential components, or containing cerium, carbon, fluorine, and oxygen as essential components and at least one of indium, tin, or bismuth as essential components, the composition of the low-refractive index layer 21 is not particularly limited.
[0058] As an example of the low refractive index layer 21 of the present embodiment, a film having silicon oxide as a main component, a part of which is substituted by an organic fluorine compound, and containing a trace amount of indium, tin or bismuth can be exemplified. In addition, as an example of the high refractive index layer 22 of the present embodiment, a film having niobium oxide as a main component, a part of which is substituted by an organic fluorine compound, and containing a trace amount of indium, tin or bismuth can be exemplified. In addition, a film having cerium oxide as a main component, a part of which is substituted by an organic fluorine compound, and containing a trace amount of indium, tin or bismuth can be exemplified.
[0059] The antireflection film 2 of this embodiment can be used as in the second embodiment described above. Figure 4 The sputtering device 3 shown uses silicon oxide-polytetrafluoroethylene containing indium as the first target and niobium or niobium oxide (or cerium or cerium oxide) as the second target, and forms a film by a radical assisted sputtering method (RAS method) using oxygen as a radical source.
[0060] Example
[0061] Hereinafter, the present invention will be described by giving examples that further embody the present invention. However, the numerical values and specific examples of the structure shown below do not limit the present invention.
[0062] 《Example 1》
[0063] A sputtering device (RAS-1100C manufactured by Shincolon Corporation) was used on one surface of a polycarbonate substrate 1 (Technolloy C000 manufactured by Escarbo Sheet Co., Ltd., with a thickness of 125 μm and a refractive index n0 of 1.59 at a wavelength of 550 nm). The target material was set to silicon oxide-polytetrafluoroethylene containing indium (the weight ratio of silicon oxide to polytetrafluoroethylene was 7:1, and the content of indium was 1 wt%), and the power density of the target material was set to 1.7 W / cm 2 The atmosphere gas was set to 100% argon, and the film forming pressure of the vacuum chamber was set to 0.7 Pa. Figure 1The antireflection film 2 having the film structure shown was formed. The low refractive index layer 21 constituting the obtained antireflection film 2 had a thickness of 291 nm, and the refractive index n1 of the low refractive index layer 21 at a wavelength of 550 nm was 1.453.
[0064] The reflectivity, heat crack resistance, hardness (nanoindenter), and tensile strength of the obtained anti-reflection film 2 were measured, and elemental analysis was further performed. The reflectivity was measured using a spectrophotometer (U4100 manufactured by Hitachi High-Technologies Corporation). Regarding heat crack resistance, a low-temperature dryer (DX300 manufactured by Yamato Scientific) was used to perform heat treatment at a specified temperature and time, and then a polarizing microscope (ECLIPSE LV100 manufactured by Nikon Corporation) was used to observe the surface. The hardness was measured using a nanoindenter (TI Premier manufactured by Bruker Corporation). Regarding tensile strength, a tensile tester (ISC-2 / 100 manufactured by TG シートン Corporation) was used to fix the two ends of a test piece of 80mm×10mm size to a tensile tester, and the two ends were stretched at a speed of 5mm / min in a manner that automatically stopped after reaching a specified tensile length. After the test, a polarizing microscope (ECLIPSELV100 manufactured by Nikon Corporation) was used to observe the surface. The elemental analysis was performed using an energy dispersive X-ray spectrometer (EDX) attached to a scanning electron microscope (JSM-6700F manufactured by JEOL).
[0065] 《Example 2》
[0066] On one surface of a polyethylene terephthalate substrate 1 (Lumirror T60 manufactured by Toray Industries, Ltd., thickness 100 μm, refractive index n0=1.66 at a wavelength of 550 nm), a low refractive index layer 21 was formed using a sputtering device (RAS-1100C manufactured by Shinkolon Corporation), with the target being silicon oxide-polytetrafluoroethylene containing indium (the weight ratio of silicon oxide to polytetrafluoroethylene being 7:1, and the content of indium being 1 wt%), and the power density of the target being 1.7 W / cm 2 The atmosphere gas was set to 100% argon, the film forming pressure of the vacuum chamber was set to 0.7 Pa, and when the high refractive index layer 22 was formed, the target material was set to cerium oxide-polytetrafluoroethylene containing indium (the weight ratio of cerium oxide to polytetrafluoroethylene was 7:1, and the content of indium was 1 wt%), and the power density of the target material was set to 4.4 W / cm 2 The atmosphere gas is set to 100% argon, and the film forming pressure of the vacuum chamber is set to 1.0 Pa. On this basis, the number of pairs of low refractive index layers 21 and high refractive index layers 22 is 2. Figure 2The anti-reflection film 2 of the film structure shown is formed. The film thicknesses of the low refractive index layer 21 and the high refractive index layer 22 constituting the obtained anti-reflection film 2 are 13nm, 32nm, 113.9nm, and 81.3nm, respectively, from the substrate side, and the refractive index n1 of the low refractive index layer 21 at a wavelength of 550nm is 1.453, and the refractive index n2 of the high refractive index layer 22 at a wavelength of 550nm is 2.136.
[0067] The reflectivity, heat crack resistance, hardness (nanoindenter), and tensile strength of the obtained antireflection film 2 were measured by the same method as in Example 1, and elemental analysis was further performed. The measurement results of these physical properties are shown in Table 1.
[0068] 《Example 3》
[0069] When forming a low refractive index layer 21 on one surface of a polycarbonate substrate 1 (Technolloy C000 manufactured by Escarbo Sheet Co., Ltd., with a thickness of 125 μm and a refractive index n0 of 1.59 at a wavelength of 550 nm), a sputtering device (RAS-1100C manufactured by Shincolon Co., Ltd.) was used, the target material was set to silicon oxide-polytetrafluoroethylene containing indium (the weight ratio of silicon oxide to polytetrafluoroethylene was 7:1, and the content of indium was 1 wt%), and the power density of the target material was set to 1.7 W / cm 2 The atmosphere gas was set to 100% argon, the film forming pressure of the vacuum chamber was set to 0.7 Pa, and when the high refractive index layer 22 was formed, the target material was set to metal niobium, and the power density of the target material was set to 5.2 W / cm 2 The atmosphere gas is set to a gas with an oxygen / argon ratio of 30%, and the film forming pressure of the vacuum chamber is set to 0.3 Pa. On this basis, the number of pairs of low refractive index layers 21 and high refractive index layers 22 is 2. Figure 3 The anti-reflection film 2 of the film structure shown is formed. The film thicknesses of the low refractive index layer 21 and the high refractive index layer 22 constituting the obtained anti-reflection film 2 are 40.4nm, 13.9nm, 42.1nm, 113.9nm, and 81.3nm, respectively, from the substrate side, and the refractive index n1 of the low refractive index layer 21 at 550nm is 1.453, and the refractive index n2 of the high refractive index layer 22 at 550nm is 2.356.
[0070] The reflectivity, heat crack resistance, hardness (nanoindenter), and tensile strength of the obtained antireflection film 2 were measured by the same method as in Example 1, and elemental analysis was further performed. The measurement results of these physical properties are shown in Table 1.
[0071] Comparative Example 1
[0072] On one surface of a polycarbonate substrate 1 (Technolloy C000 manufactured by Escarbo Sheet Co., Ltd., thickness 125 μm, refractive index n0=1.59 at a wavelength of 550 nm), a low refractive index layer 21 was formed using a sputtering device (RAS-1100C manufactured by Shincolon Co., Ltd.), with a target material of metallic silicon and a power density of the target material of 3.4 W / cm 2 The atmosphere gas was set to a gas with an oxygen / argon ratio of 11%, the film forming pressure of the vacuum chamber was set to 0.4 Pa, and when the high refractive index layer 22 was formed, the target material was set to metal niobium, and the power density of the target material was set to 5.2 W / cm 2 The atmosphere gas is set to a gas with an oxygen / argon ratio of 30%, and the film forming pressure of the vacuum chamber is set to 0.3 Pa. On this basis, the number of pairs of low refractive index layers 21 and high refractive index layers 22 is 2. Figure 3 The anti-reflection film 2 of the film structure shown is formed. The film thicknesses of the low refractive index layer 21 and the high refractive index layer 22 constituting the obtained anti-reflection film 2 are 40.4nm, 13.9nm, 42.1nm, 113.9nm, and 81.3nm, respectively, from the substrate side, and the refractive index n1 of the low refractive index layer 21 at a wavelength of 550nm is 1.469, and the refractive index n2 of the high refractive index layer 22 at a wavelength of 550nm is 2.356.
[0073] The reflectivity, heat crack resistance, hardness (nanoindenter), and tensile strength of the obtained antireflection film 2 were measured by the same method as in Example 1, and elemental analysis was further performed. The measurement results of these physical properties are shown in Table 1.
[0074] [Table 1]
[0075] Example 1 Example 2 Example 3 Comparative Example 1 Reflectivity 2.0 0.1 0.23 0.24 Heat crack resistance ○ (Substrate deformation) ○ × Nanoindenter(GPa) 4.4 11 4.9 6.1 Tensile crack resistance 2% ○ ○ ○ × Tensile crack resistance 5% ○ × ○ × Detection element (Si) Detected Detected Detected Detected Detection element (C) Detected Detected Detected Detected Detection element (O) Detected Detected Detected Detected Detection element (Nb) Not detected Not detected Detected Detected Detection element (Ce) Not detected Detected Not detected Not detected Detection element (F) Detected Detected Detected Not detected Detection element (In) Detected Detected Detected Not detected
[0076] Investigation
[0077] Regarding heat crack resistance, the reflective films of Examples 1 and 3 are superior to those of Comparative Example 1. It should be noted that the heat resistance temperature of the substrate 1 (made of PET) of the reflective film of Example 2 is lower than the test temperature, and the substrate 1 deformed during heating, so it could not be evaluated. Regarding the hardness evaluation using a nanoindenter, Examples 1 to 3 and Comparative Example 1 all showed results of more than 4 GPa, which means they have sufficient hardness. In particular, the hardness of the reflective film of Example 2 is the highest result. It is speculated that this is because the film hardness of CeO2 is higher than that of SiO2 and Nb2O5, so the performance of the CeO2 film is obvious when forming an anti-reflective film. Regarding tensile crack resistance, the reflective films of Examples 1 to 3 did not produce cracks, while the reflective film of Comparative Example 1 produced cracks after being stretched by 2%.
[0078] From the above results, it was confirmed that the reflective films of Examples 1 to 3 not only have antireflection properties and scratch resistance, but also can suppress the occurrence of cracks due to tensile stress.
[0079] Description of Reference Numerals
[0080] 1…Substrate
[0081] 2…Anti-reflective film
[0082] 21…Low refractive index layer
[0083] 22…High refractive index layer
[0084] 3…Sputtering device
[0085] 31…Vacuum chamber
[0086] 32…Substrate rack
[0087] 33, 34…Sputtering source
[0088] 331, 341…AC power supply
[0089] 332, 342…Film forming process area
[0090] 333, 343... next door
[0091] 35…Plasma source
[0092] 351…Housing
[0093] 352…Dielectric module
[0094] 353…High frequency power supply
[0095] 354…Reaction process area
[0096] 355…Next door
[0097] 356…Reaction treatment gas supply system
Claims
1. An antireflection film having, as an outermost layer, a low refractive index layer having a refractive index lower than that of the substrate on the surface of the substrate, The low refractive index layer contains silicon, carbon, fluorine and oxygen as essential components, further contains at least one of indium, tin or bismuth as an essential component, has silicon oxide as a main component, and contains an organic fluorine compound.
2. The antireflection film according to claim 1, wherein A high refractive index layer having a refractive index higher than that of the substrate is provided between the substrate and the low refractive index layer as the outermost layer, The high refractive index layer contains niobium, carbon, fluorine and oxygen as essential components, and further contains at least one of indium, tin or bismuth as an essential component, or The present invention contains cerium, carbon, fluorine and oxygen as essential components, and further contains at least one of indium, tin and bismuth as an essential component. 3 . The antireflection film according to claim 2 , further comprising the low refractive index layer between the substrate and the high refractive index layer.
4. An antireflection film, comprising one or more layers of a low refractive index layer having a refractive index lower than that of the substrate and a high refractive index layer having a refractive index higher than that of the substrate, stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer, The high refractive index layer contains niobium, carbon, fluorine and oxygen as essential components, and at least one of indium, tin or bismuth as an essential component, has niobium oxide as a main component, and contains an organic fluorine compound, or The present invention contains cerium, carbon, fluorine and oxygen as essential components, further contains at least one of indium, tin and bismuth as an essential component, has cerium oxide as a main component, and contains an organic fluorine compound. 5 . The antireflection film according to claim 4 , further comprising the low refractive index layer between the substrate and the high refractive index layer closest to the substrate.
6. The antireflection film according to claim 4, wherein: The low refractive index layer contains silicon, carbon, fluorine, and oxygen as essential components, and further contains at least one of indium, tin, and bismuth as an essential component.
7. An antireflection film, comprising one or more layers of a low refractive index layer having a refractive index lower than that of the substrate and a high refractive index layer having a refractive index higher than that of the substrate, stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer, The low refractive index layer is further provided between the substrate and the high refractive index layer closest to the substrate. The low refractive index layer contains silicon, carbon, fluorine and oxygen as essential components, further contains at least one of indium, tin or bismuth as an essential component, has silicon oxide as a main component, and contains an organic fluorine compound.
8. An antireflection film, comprising one or more layers of a low refractive index layer having a refractive index lower than that of the substrate and a high refractive index layer having a refractive index higher than that of the substrate, stacked on the surface of the substrate in such a manner that the low refractive index layer becomes the outermost layer, The low refractive index layer is further provided between the substrate and the high refractive index layer closest to the substrate. The high refractive index layer contains niobium, carbon, fluorine and oxygen as essential components, and at least one of indium, tin or bismuth as an essential component, has niobium oxide as a main component, and contains an organic fluorine compound, or The present invention contains cerium, carbon, fluorine and oxygen as essential components, further contains at least one of indium, tin and bismuth as an essential component, has cerium oxide as a main component, and contains an organic fluorine compound.
9. The antireflection film according to any one of claims 1 to 8, wherein The substrate is made of glass material or plastic material.
Citation Information
Patent Citations
Antireflection film and image display unit
JP2022065437A