Solder material

By adding Cu to the solder materials of Sn, Sb, Ag and Ni, the Young's modulus and creep characteristics of the solder are improved, and the problem of cracks in the solder joint at high temperatures is solved, which significantly improves the reliability and durability of the semiconductor device. .

CN119095691APending Publication Date: 2024-12-06FUJI ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036047.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-07
Filing Date
2023-10-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In a high temperature environment, cracks are easily generated by the solder joint between the semiconductor element and the laminated substrate, resulting in a rise in resistance and a decrease in reliability. The existing solder materials cannot effectively suppress the occurrence of cracks at high temperatures.

Method used

By adding a specific amount of Cu to the solder material containing Sn, Sb, Ag and Ni, Young's modulus and creep characteristics are improved, and the elongation and wetting of the solder joints are enhanced, thereby improving the high temperature reliability of the solder. sex.

Benefits of technology

The elongation and creep characteristics of the solder material at high temperatures are significantly improved, cracks in the joints are suppressed, and the reliability and durability of the semiconductor device are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095691A_ABST
    Figure CN119095691A_ABST
Patent Text Reader

Abstract

Provided is a solder material having excellent elongation at break in a high-temperature environment. Provided are: a solder material containing 5.0 mass% to 10.0 mass% (inclusive) of Sb, 2.0 mass% to 6.0 mass% (inclusive) of Ag, 0.1 mass% to 0.5 mass% (inclusive) of Ni, and 3.0 mass% to 8.0 mass% (inclusive) of Cu, with the remainder comprising Sn and unavoidable impurities; the solder joint part is provided with a joint layer formed by melting the solder material, and the semiconductor device is provided with the joint part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solder material and, in particular, to a solder material having improved elongation at break in a high temperature environment and being suitable for bonding semiconductor elements. Background Art

[0002] Power semiconductor modules are widely used in fields that require efficient power conversion. For example, the scope of application is expanding in power electronics fields such as industrial equipment, electric vehicles, and home appliances. These power semiconductor modules have built-in switching elements and diodes, and Si (silicon) semiconductors and SiC (silicon carbide) semiconductors are used for the elements. These semiconductor elements are bonded to the laminated substrate by bonding materials, and solder materials are used as bonding materials.

[0003] In recent years, due to environmental issues, lead-free solders that do not contain lead have been used as substitutes for Sn-Pb solders. As solder materials used in power semiconductor modules such as IGBT modules, even among the various combinations of lead-free solders currently known, Sn-Ag lead-free solders are widely used because they have a good balance in terms of solder wettability, mechanical properties, thermal resistance, etc. and are also actually used in products.

[0004] A solder composition is known, which is composed of 0.01 wt% to 0.5 wt% Ni, more than 2 wt% to 5 wt% Cu, and Sn as the remainder, and may further contain at least one component selected from the group consisting of Ag, In, Zn, Sb, Ge, and P (see, for example, Patent Document 1). The solder composition disclosed in Patent Document 1 is considered to suppress the disconnection of the conductor caused by the melting corrosion of the conductor containing Cu as the main component, and has characteristics similar to those of the conventional Sn-Pb solder composition.

[0005] A solder alloy is known, which has an alloy combination consisting of 9.0% to 33.0% Sb, more than 4.0% and less than 11.0% Ag, more than 2.0% and less than 6.0% Cu, and the remainder Sn in terms of mass % (for example, refer to Patent Document 2). The solder alloy disclosed in Patent Document 2 is believed to suppress chip cracking during cooling, improve the heat dissipation characteristics of the solder joint, and exhibit high bonding strength at high temperatures.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-324257

[0009] Patent Document 2: International Publication No. WO2020 / 122253 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] Due to the recent high current and high temperature driving of power semiconductor modules, cracks have become a problem at the solder joints between semiconductor elements and laminated substrates. It is believed that the cracks are caused by thermal stress. When cracks occur in the solder joints, the resistance rises, which leads to further temperature rise. In the past, the strength and Young's modulus of solder materials at room temperature have been improved, but it cannot be said that they are sufficient for use in high temperature environments.

[0012] Solutions for solving problems

[0013] The inventors of the present invention have conducted intensive research and found that the reliability of the solder joint can be improved by improving the creep characteristics and elongation at break at a high temperature of about 175°C. Specifically, the inventors of the present invention have come up with the following scheme: by adding a predetermined amount of Cu to a solder material containing Sn, Sb, Ag, and Ni, the Young's modulus is made equivalent at high temperatures, and the creep characteristics and elongation at break are improved, thereby improving the reliability of the module.

[0014] That is, according to one embodiment, the present invention relates to a solder material containing 5.0 mass % to 10.0 mass % Sb, 2.0 mass % to 6.0 mass % Ag, 0.1 mass % to 0.5 mass % Ni, and 3.0 mass % to 8.0 mass % Cu, with the remainder consisting of Sn and unavoidable impurities.

[0015] The solder material preferably contains 4.5 mass % or more and 8.0 mass % or less of Cu.

[0016] In any of the above solder materials, it is preferred that Sb be contained in an amount of 6.0 mass % to 8.5 mass %.

[0017] In any of the above solder materials, it is preferred that Ag be contained in an amount of 3.0 mass % to 6.0 mass %.

[0018] The arbitrary solder material is preferably a solder material used for bonding semiconductor elements.

[0019] According to another embodiment, the present invention relates to a solder joint portion including: a solder joint layer formed by melting any of the above-mentioned solder materials; and a joined body having a metal layer on a surface in contact with the solder joint layer.

[0020] According to another embodiment, the present invention relates to a semiconductor device, comprising a semiconductor element joined to a stacked substrate and a conductive connecting component joined to the semiconductor element, wherein the semiconductor device has a solder joint between the stacked substrate and the semiconductor element, or between the semiconductor element and the conductive connecting component.

[0021] According to another embodiment, the present invention relates to a semiconductor device, comprising a semiconductor element joined to a stacked substrate and a cooler joined to a surface of the stacked substrate opposite to a surface joined to the semiconductor element, wherein the semiconductor device has the solder joint portion between the stacked substrate and the cooler.

[0022] Effects of the Invention

[0023] According to the present invention, a solder material having improved elongation at break and creep elongation at break at high temperatures, excellent stress relaxation effect, and high wettability can be provided. In addition, even in semiconductor devices used in high temperature environments and generating large currents of up to several thousand amperes, the solder material can be ideally used for joining semiconductor elements, and cracks in the joining portion can be suppressed, thereby contributing to improving the reliability of the semiconductor device. Hereinafter, in this specification, elongation at break and creep elongation at break are sometimes referred to as "elongation characteristics". BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a conceptual cross-sectional view showing a cross-sectional structure of a semiconductor device according to one embodiment of the present invention.

[0025] Figure 2A It is a figure which shows the shape of the test piece used in an Example.

[0026] Figure 2B yes Figure 2A Cross-sectional view at line XX.

[0027] Figure 3 This is a graph showing the relationship between the Cu content in the solder material and the normalized elongation at break.

[0028] Figure 4 This is a graph showing the relationship between the Cu content in the solder material and the normalized creep rupture elongation. DETAILED DESCRIPTION

[0029] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the present invention is not limited to the embodiments described below.

[0030] [First embodiment: solder material]

[0031] According to a first embodiment, the present invention is a solder material, which is an alloy containing 5.0 mass % to 10.0 mass % Sb, 2.0 mass % to 6.0 mass % Ag, 0.1 mass % to 0.5 mass % Ni, and 3.0 mass % to 8.0 mass % Cu, with the remainder being Sn and unavoidable impurities.

[0032] In the solder material of the first embodiment, the inevitable impurities mainly refer to Cu, Ni, Zn, Fe, Al, As, Cd, Au, In, P, Pb, etc. The upper limit of the content of each element treated as an inevitable impurity varies depending on the main components of the solder material and is specified by international standards. For example, the upper limit of the amount of inevitable impurities in the solder material involved in this embodiment can be a value specified by the international standards of Sn-Ag solder and Sn-Sb solder. In addition, the solder material of the first embodiment is a lead-free solder alloy that does not contain lead.

[0033] The content of Sb is set to more than 5.0 mass % and less than 10.0 mass %. By containing Sb in this range, the Sn phase is solid solution strengthened, forming a Sn-Sb phase, so that it will not break, and the elongation characteristics (creep characteristics) are improved. Therefore, it is not easy to produce cracks and peeling in the solder joint, which is preferred. If the content of Sb is less than 5.0 mass %, the solid solution strengthening of Sb to the Sn layer cannot fully play a role, there is a deformation of Sn, and the creep characteristics deteriorate. If the content of Sb exceeds 10.0 mass %, then due to the coarsening of the compound of Sn and Sb, that is, SbSn, stress concentration is caused, which becomes the main cause of fracture, and there is a disadvantage that the creep characteristics are reduced. The content of Sb is more preferably set to more than 5.5 mass % and less than 8.5 mass %, or more than 5.5 mass % and less than 7.0 mass %, or more than 6.0 mass % and less than 8.5 mass %. If it is set to the above-mentioned combination range, the Sn-Sb phase is close to the peritectic combination, the wettability is improved, and the solid solution strengthening achieved by adding Sb can be maximized, which is also preferred from the perspective of reducing voids and creep properties. The Sb content is more preferably set to 6.0 mass % or more and 7.0 mass % or less. This is because it becomes a peritectic combination within this range.

[0034] The content of Ag is set to be greater than 2.0 mass % and less than 6.0 mass %. By containing Ag in this range, the pinning effect on dislocation movement is maintained even at a high temperature of 175°C, and the wettability is also excellent. Therefore, there is an advantage that the initial porosity is low and it is easy to ensure the quality of bonding. If the content of Ag is less than 2.0 mass %, the dispersion amount of the Ag3Sn phase is small, and there is a disadvantage that local deformation is easily caused during deformation in a high temperature environment of 175°C, and if the content of Ag exceeds 6.0 mass %, there may be disadvantages such as reduced wettability and increased melting point. The content of Ag is more preferably set to be greater than 3.0 mass % and less than 6.0 mass %. By containing Ag in this range, the Sn-Ag phase is close to the eutectic combination, so the wettability is improved. In addition, since the fine Sn-Ag phase is uniformly dispersed around the Sn phase, it is preferred from the perspective of bonding and creep properties. In addition, since it can have uniform properties, it is also preferred from the perspective of manufacturing. The content of Ag is more preferably set to 3.5 mass % or more and 5.0 mass % or less. By containing Ag in this range, the Sn-Ag phase is closer to the eutectic combination, so as described above, it is more preferred from the perspective of creep characteristics and manufacturing. The content of Ag is further preferably set to 3.7 mass % or more and 5.0 mass % or less. Since it is basically a eutectic combination within the above range, it is further preferred from the perspective of bonding, creep characteristics and manufacturing as described above.

[0035] The content of Ni is set to more than 0.1% by mass and less than 0.5% by mass. By containing Ni in this range, especially in the case of Cu bonding purposes, the product of the solder / Cu substrate interface changes from Cu6Sn to (Cu, Ni)6Sn, and the deterioration of the toughness (elongation characteristics) of the joint after high temperature aging is suppressed. In addition, if the content of Ni that can be expected to be suppressed by the improvement of strength brought by the refinement of grains and the deviation of mechanical properties brought by polycrystallization is less than 0.1% by mass, it is sometimes impossible to give full play to the above-mentioned effect. If the content of Ni exceeds 0.5% by mass, it is worried that the melting point will rise. The content of Ni is more preferably set to more than 0.15% by mass and less than 0.4% by mass. If it is set to this range, the toughness is improved and cracks are not easy to occur. In addition, the amount of initial voids generated is small when bonding over a large area, so it is preferred.

[0036] The content of Cu is set to be more than 3.0 mass % and less than 8.0 mass %. By containing Cu in this range, it is possible to impart sliding characteristics to the solder material. Therefore, there are the following advantages: after being applied with stress, sliding deformation is caused, creep characteristics are improved, and then stress relaxation effect is produced. By containing more than 3.0 mass % of Cu, the failure mode is changed to sliding starting from the grain boundary, which can improve the creep characteristics by at least 40%. If the content of Cu is less than 3.0 mass %, sufficient sliding characteristics cannot be imparted to the solder material. If more than 8.0 mass % of Cu is contained, it is believed that a hard structure of the CuSn system will be excessively generated, and the creep characteristics will be reduced. In addition, from the viewpoint of wettability, the content of Cu is also set to less than 8.0 mass %.

[0037] The content of Cu is preferably set to 4.5 mass % or more and 8.0 mass % or less. By containing Cu in this range, the creep properties at high temperature, especially at 175°C, can be improved by more than 2 times compared with when Cu is not contained (according to Figure 4 The creep characteristics can be increased by 2.5 times or more by setting the Cu content to 5.2 mass % or more and 7.8 mass % or less ( Figure 4 ). In addition, the creep characteristics can be increased by 3.0 times or more by setting the Cu content to 5.9 mass % or more and 7.0 mass % or less ( Figure 4 ). In addition, by setting the Cu content to 4.8 mass % or more and 5.3 mass % or less, when processed into a predetermined shape, there are few deformations such as burrs and local unevenness, and plastic processing is easy. In other words, as a solder material, it also has excellent processability, and as a bonding layer, it has high mechanical strength.

[0038] In the case where a Ni-containing layer (plating, etc.) is applied to the joined portion, Cu as a component of the solder material sometimes reacts with Ni dissolved into the solder and is consumed. The Ni-containing layer refers to a layer containing more than 50% by mass of Ni, which can be either a base material or a layer containing Ni or a Ni alloy formed by a film forming method such as plating. Specifically, for example, it can also be a NiP plating containing more than 0 and less than 10% by mass of P. In addition, in the case where the joined portion is a Cu layer, Sn as a component of the solder material sometimes reacts with Cu dissolved into the solder and is consumed. Therefore, in the case of a joining application containing a Ni layer or a Cu layer, the content range of Cu in the solder material is preferably set to 5.1% by mass and less than 8.0% by mass, preferably set to 5.2% by mass and less than 7.5% by mass. In addition, the Cu layer of the joined portion can be any material containing more than 50% by mass of Cu, including Cu or a Cu alloy.

[0039] Furthermore, if Bi is added to the solder material of the first embodiment having the above composition, a low melting point phase is generated, the mechanical strength is reduced, and Bi is easily oxidized, so it is not preferable in some cases. In particular, adding 2% by mass or more of Bi is not preferable. In addition, if Zn is added, it is easily oxidized, so wettability is sometimes deteriorated and it is not preferable. In particular, adding 2% by mass or more of Zn is not preferable.

[0040] In this specification, the creep property of the solder material is defined by the value of strain × stress required until the solder material breaks, which can also be called strain energy. The strain energy required until the solder material breaks is called creep rupture elongation. In this specification, creep rupture elongation refers to the value of elongation until rupture when a constant load (constant stress) is applied to a test piece at a specific temperature. In the following specification, unless otherwise specified, creep rupture elongation refers to creep rupture elongation at 175°C. In addition, the test piece uses a small test piece with a marked portion diameter of 1mm and a marked portion length of 2.4mm, and the constant load is set to 7N (8.92MPa). This load is determined so that the deformation rate of the solder joint layer can be applied to the test piece in the thermal cycle test of the semiconductor device to which the solder material involved in this embodiment is applied. Specifically, since the constant load is set to 7N, it is possible to apply 1.0×10 -5 ~5.0×10 -5 (1 / s) or so. In addition, the conditions for the thermal cycle test applying the above deformation rate are: high temperature is 150°C, low temperature is -55°C, holding time is 60 minutes, and temperature change is 7°C / minute. By evaluating the creep rupture elongation, the stress relaxation characteristics and fatigue characteristics can be evaluated. It is believed that the greater the value of the creep rupture elongation, the better the stress relaxation characteristics and fatigue characteristics. In addition, in the above-mentioned measurement method, since the test is carried out with a constant load, the creep characteristics (strain energy) and the creep rupture elongation are proportional to each other and can be treated equally.

[0041] The solder material of the present invention can be prepared by melting each raw material selected from Sn, Sb, Ag, Ni and Cu, or a master alloy containing each raw material in an electric furnace according to a common method. It is preferable to use each raw material having a purity of 99.99 mass % or more.

[0042] In addition, the solder material of the above composition can be processed into a plate-shaped preform material, or formed into a powder and processed into a paste solder together with a flux. In the case of processing into a powder and making a paste solder together with a flux, the particle size (particle diameter) of the solder powder is preferably distributed in the range of 10 μm to 100 μm, and more preferably in the range of 20 μm to 50 μm. Regarding the average particle size, for example, when measured using a common laser diffraction / scattering particle size distribution measuring device, it can be set to 25 μm to 50 μm. As the flux, any flux can be used, and in particular, rosin-based flux can be preferably used.

[0043] The solder material of this embodiment has excellent elongation at break and creep properties at high temperatures of about 175°C to 200°C, and can be preferably used for joining components in electronic devices, particularly for joining the back electrode of a semiconductor element to an electrode of a laminate substrate.

[0044] [Second embodiment: Solder joint]

[0045] According to a second embodiment, the present invention is a solder joint portion including: a solder joint layer formed by melting the solder material according to the first embodiment; and a joined body having a metal layer on a surface in contact with the solder joint layer.

[0046] The solder bonding layer constituting the solder bonding portion of the present embodiment can be a layer obtained by melting the solder material of the first embodiment. The thickness, shape, etc. of the solder material used to form the solder bonding layer can be appropriately set by a person skilled in the art according to the purpose and use, and are not particularly limited. As an example, in the bonding between the surface of a semiconductor element and a wiring member such as a lead frame, it is preferably 50 μm or more, but is not limited to this range. In the bonding between the back electrode of the semiconductor element and the conductive plate of the laminated substrate, the thickness of the solder bonding layer can be set to about 200 μm to 300 μm, preferably about 200 μm to 250 μm, but is not limited to this range. In addition, in the bonding between the laminated substrate and the heat sink, it is preferably about 400 μm to 500 μm.

[0047] The joined body constituting the solder joint portion of the present embodiment is a member having a metal layer on the surface in contact with the solder joint layer. The type of metal constituting the metal layer is not particularly limited, but generally speaking, the joined body may be a member having an electrode, and the electrode may be composed of Cu, Ni, Al, Ti, Au, Ag or an alloy thereof. The joined body may also be a member having a plated film containing these metals on the surface in contact with the solder joint layer.

[0048] A solder material of a specified shape and thickness is arranged in contact with the metal layer of the body to be joined, and heated at a specified temperature, thereby forming a solder joint. The joining atmosphere can be set to a nitrogen atmosphere, or the joining can be performed in an active atmosphere such as hydrogen or formic acid. In particular, when using plate solder, it is preferred to use a gas such as hydrogen or formic acid that has a reducing effect. When joining under these active gas atmospheres with a reducing effect, it is preferably set to a temperature at which the gas effectively reduces the oxide, for example, 250°C to 300°C. In addition, the joining temperature of the plate solder and the paste solder can also be set to the melting point (Tm) of the solder material + (50°C ± 10°C). In actual joining, the joining is performed with a temperature distribution of more than a few degrees Celsius, so by ensuring a certain temperature and time, a stable joining quality can be obtained. Thereafter, the molten solder is solidified by cooling at a specified temperature drop rate to form a solder joint layer. The heating rate of the heat treatment can be set to about 1°C / second, and the cooling rate is preferably 5°C / second or more, more preferably 8°C / second or more and 15°C / second or less. By setting the heating rate and cooling rate of the heat treatment to this range, the grains are refined and each phase is precipitated more uniformly, thereby reducing the deviation in quality.

[0049] The solder joint involved in the second embodiment can constitute a part of an electronic device. As electronic devices, electrical power equipment such as inverters, megawatt-class solar equipment, fuel cells, elevators, cooling devices, and vehicle-mounted semiconductor devices can be cited, but are not limited to these. Typically, the electronic device is a semiconductor device. The joint in the semiconductor device can be a chip bonding joint, a joint between a conductive plate and a heat sink, a joint between terminals, a joint between terminals and other components, or any other joint. In particular, it can be a joint for large current flow, but is not limited to these. The semiconductor device is described in detail in the third embodiment.

[0050] The solder joint according to the second embodiment is excellent in stress relaxation characteristics at high temperatures, and therefore is less likely to crack, resulting in a highly reliable solder joint.

[0051] [Third Embodiment: Semiconductor Device]

[0052] According to a third embodiment, the present invention is a semiconductor device including a semiconductor element bonded to a laminated substrate, the semiconductor device having a solder bonding layer formed by melting the solder material of the first embodiment. In other words, the semiconductor device of the third embodiment has the solder bonding portion of the second embodiment, and the bonded body of the solder bonding portion is a semiconductor element and / or any member constituting the semiconductor device.

[0053] Figure 1This is a conceptual cross-sectional view of a power semiconductor module as an example of a semiconductor device involved in the present embodiment. The illustrated power semiconductor module has a stacked structure in which the back electrode of a semiconductor element 11 is bonded to a stacked substrate 12 via a bonding layer 10, and the stacked substrate 12 is bonded to a heat sink 13 via a bonding layer 17. A housing 16 having built-in external terminals 15 is adhered to the heat sink 13. The surface electrode of the semiconductor element 11 and the electrode of the stacked substrate 12 are connected by a lead frame 18 as a conductive connecting member. In addition, the semiconductor element 11 and the external terminal 15 are connected by an aluminum wire 14. A sealing material 20 is filled in a space formed by the housing 16 and the heat sink 13 in a manner in contact with the semiconductor element 11, the stacked substrate 12, the lead frame 18, and the aluminum wire 14 as a conductive connecting member. Figure 1 In the embodiment, the following embodiment is used as an example for explanation: a bonding layer 10 formed by melting the solder material of the first embodiment is provided between the back electrode of the semiconductor element 11 and the laminated substrate 12, and between the surface electrode of the semiconductor element 11 and the lead frame 18. However, the solder material of the first embodiment can be used for bonding any part of the semiconductor device, and the present invention is not limited to the illustrated embodiment.

[0054] The semiconductor element 11 is a power chip such as an IGBT (Insulated Gate Bipolar Transistor) or a diode chip, and can be a Si device or a wide-bandgap semiconductor device such as a SiC device, a GaN device, a diamond device, or a ZnO device. In addition, these devices can also be used in combination. For example, a hybrid module using Si-IGBT and SiC-SBD can be used. The number of semiconductor elements mounted can be one or more.

[0055] The laminated substrate 12 can be composed of an insulating substrate 122, a first conductive plate 121 formed on one main surface thereof, and second conductive plates 123a and 123b formed on the other main surface. As the insulating substrate 122, a material with excellent electrical insulation and thermal conductivity can be used. As the material of the insulating substrate 122, for example, Al2O3, AlN, SiN, etc. can be cited. In particular, in high-voltage applications, it is preferred to use a material that takes into account both electrical insulation and thermal conductivity. AlN and SiN can be used, but are not limited to these. As the first conductive plate 121 and the second conductive plate 123a and 123b, metal materials such as Cu and Al with excellent processability can be used. In addition, for the purpose of rust prevention, the conductive plate can also be Cu and Al that are surface-treated by Ni plating and have a Ni-containing layer containing Ni or Ni alloy on the surface. As a specific Ni-containing layer formed by Ni plating, a layer containing NiP and a layer containing NiB can be cited, but are not limited to these. As a method for configuring the first conductive plate 121 and the second conductive plates 123a, 123b on the insulating substrate 122, a direct copper bonding method (Direct Copper Bonding method) or a brazing method (Active Metal Brazing method) can be cited. In the illustrated embodiment, two second conductive plates 123a, 123b are non-continuously provided on the insulating substrate 122, one second conductive plate 123a functions as an electrode bonded to the semiconductor element 11, and the other second conductive plate 123b functions as an electrode connected to the lead frame 18. However, the number and connection method of the first conductive plate and the second conductive plate are not limited to the illustrated embodiment.

[0056] The lead frame 18 is a conductive connecting member that connects the semiconductor element 11 to the second conductive plate 123b and the like. Specifically, the lead frame 18 can be bonded to the surface electrode of the electrode of the semiconductor element 11 located on the opposite side of the electrode (back electrode) in contact with the laminated substrate 12 using, for example, a bonding layer 10 formed by melting the solder material of the first embodiment. In addition, the lead frame 18 can also be bonded to the wiring portion such as the second conductive plate 123b using a bonding layer 17 of a solder material and the like. The lead frame 18 can be a metal such as copper or an alloy containing copper. It is also possible to form a Ni or Ni alloy layer (NiP alloy, NiB alloy, etc.) as a Ni-containing layer, or to form a Cr or Cr alloy layer on the surface of the lead frame 18 by plating or the like. In this case, the film thickness of the Ni or Ni alloy layer, or the Cr or Cr alloy layer can be set to about 20 μm or less. In addition, the lead frame can also be connected to a take-out terminal (not shown). A wire may be used as a conductive connection member for connecting the semiconductor element 11 and the second conductive plate 123b etc. When bonding is performed by wire bonding, solder material may not be used.

[0057] As the heat sink 13, a metal such as copper or aluminum having excellent thermal conductivity is used. In addition, in order to prevent corrosion, the heat sink 13 may be coated with Ni or a Ni alloy (NiP alloy, NiB alloy, etc.) as a Ni-containing layer by a plating method or the like. The heat sink may also be a cooler having functions such as water cooling or air cooling. It is also possible to be a semiconductor device in which the housing 16 is mounted on the laminated substrate 12 but the heat sink 13 is not mounted on the housing 16.

[0058] The bonding layer 10 that bonds the surface electrode of the semiconductor element 11 to the lead frame 18, and the bonding layer 10 that bonds the back electrode of the semiconductor element 11 to the second conductive plate 123a can be formed using the solder material of the first embodiment. In the past, cracks in these joints would become a problem, so by using the solder material of the first embodiment, the reliability of these bonding layers can be improved. The bonding layer 17 between other components such as the second conductive plate 123b and the heat sink 13 can also be formed using the solder material of the first embodiment, but can be formed using any lead-free solder. For example, Sn-Ag-Cu system, Sn-Sb system, Sn-Sb-Ag system, Sn-Cu system, Sn-Sb-Ag-Cu system, Sn-Cu-Ni system, Sn-Ag system, etc. can be used, but are not limited to these. Alternatively, a connecting material containing tiny metal particles such as a sintered body of nanosilver particles can also be used to form a bonding layer. In addition, the arrangement of the bonding layer 10 formed by melting the solder material of the first embodiment and the arbitrary bonding layer 17 in the semiconductor device shown in the figure is an example. The semiconductor device of the third embodiment of the present invention only needs to have a bonding layer formed by melting the solder material of the first embodiment between any components constituting the device. Therefore, the bonding layer between the laminated substrate 12 and the heat sink 13 can also be a bonding layer formed by melting the solder material of the first embodiment.

[0059] The housing 16 can be made of a thermoplastic resin such as polyphenylene sulfide (PPS) or polybutylene terephthalate (PBT).

[0060] The sealing material 20 may be a thermosetting resin cured product obtained by curing a thermosetting resin composition. The thermosetting resin cured product includes a thermosetting resin main agent and an inorganic filler, and may optionally include a curing agent, a curing accelerator, and an additive.

[0061] The main thermosetting resin is not particularly limited, and examples thereof include epoxy resins, phenolic resins, maleimide resins, cyanate resins, oxazine resins, etc. Among them, epoxy resins having at least two or more epoxy groups in one molecule are particularly preferred because of their high dimensional stability, water resistance, chemical resistance, and electrical insulation. Specifically, aliphatic epoxy resins, alicyclic epoxy resins, or mixtures thereof are preferably used. In addition, as a sealing resin, since heat resistance and high insulation are necessary, a thermosetting resin is preferred, and in particular, an epoxy resin is preferred because it is highly elastic.

[0062] Aliphatic epoxy resin refers to an epoxy compound in which the carbon to which the epoxy group is directly bonded is the carbon constituting the aliphatic hydrocarbon. Thus, even if the compound contains an aromatic ring in the main skeleton, the compound satisfying the above conditions is also classified as an aliphatic epoxy resin. As aliphatic epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD ​​type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, cresol novolac type epoxy resin, trifunctional or more multifunctional epoxy resin, etc. can be cited, but are not limited to these. They can be used alone or two or more of them can be mixed and used. In addition, the glass transition temperature of naphthalene type epoxy resin and trifunctional or more multifunctional epoxy resin is high, so it is also called high heat resistant epoxy resin. By including these high heat resistant epoxy resins, heat resistance can be improved.

[0063] Alicyclic epoxy resin refers to an epoxy compound in which two carbon atoms constituting the epoxy group constitute an alicyclic compound. Examples of alicyclic epoxy resins include monofunctional epoxy resins, difunctional epoxy resins, trifunctional or higher multifunctional epoxy resins, etc., but are not limited to these. Alicyclic epoxy resins can also be used alone or in a mixture of two or more different alicyclic epoxy resins. In addition, if the alicyclic epoxy resin is mixed with an acid anhydride curing agent and cured, the glass transition temperature becomes higher. Therefore, if the alicyclic epoxy resin is mixed with an aliphatic epoxy resin for use, high heat resistance can be achieved.

[0064] The thermosetting resin main agent used in the sealing material 20 can also be a mixture of the above-mentioned aliphatic epoxy resin and alicyclic epoxy resin. The mixing ratio in the case of mixing can be arbitrary, and the mass ratio of the aliphatic epoxy resin to the alicyclic epoxy resin can be about 2:8 to 8:2, but can also be about 3:7 to 7:3, and is not limited to a specific mass ratio. In a preferred embodiment, the thermosetting resin main agent used in the sealing material 20 is a mixture of bisphenol A epoxy resin and alicyclic epoxy resin in a mass ratio of 1:1 to 1:4.

[0065] The inorganic filler can be a metal oxide or a metal nitride, for example, fused silica, silicon dioxide (silicon oxide), aluminum oxide, aluminum hydroxide, titanium dioxide, zirconium oxide, aluminum nitride, talc, clay, mica, glass fiber, etc., but not limited to these. Through these inorganic fillers, the thermal conductivity of the sealing material 20 can be improved and the thermal expansion coefficient can be reduced. These inorganic fillers can also be used alone, but two or more can also be mixed. In addition, the inorganic filler can be either a micron filler or a nanofiller, and two or more inorganic fillers with different particle sizes and / or types can also be mixed and used. In particular, it is preferred to use an inorganic filler with an average particle size of about 0.2μm to 20μm. When the total mass of the thermosetting resin main agent and the curing agent that can be optionally included is set to 100 parts by mass, the amount of the inorganic filler added in the sealing material 20 is preferably 100 parts by mass to 600 parts by mass, and more preferably 200 parts by mass to 400 parts by mass. If the inorganic filler content is less than 100 parts by mass, the thermal expansion coefficient of the sealing material 20 increases, and peeling and cracking may occur easily. If the content is more than 600 parts by mass, the viscosity of the composition increases, and extrusion moldability may deteriorate.

[0066] In the thermosetting resin composition constituting the sealing material 20, as an optional component, a curing agent may also be included. As a curing agent, as long as it can react with a thermosetting resin main agent, preferably with an epoxy resin main agent and solidify, it is not particularly limited, but an anhydride curing agent is preferably used. As an anhydride curing agent, for example, aromatic anhydrides can be cited, specifically, phthalic anhydride, pyromellitic anhydride, trimellitic anhydride, etc. can be cited. Alternatively, cyclic aliphatic anhydrides can be cited, specifically, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, etc. can be cited, or aliphatic anhydrides can be cited, specifically, succinic anhydride, polyadipic anhydride, polysebacic anhydride, polyazepine anhydride, etc. can be cited. The mixing amount of the curing agent is preferably set to be 50 mass parts or more and 170 mass parts or less relative to 100 mass parts of the main agent of the thermosetting resin (epoxy resin), and more preferably set to be 80 mass parts or more and 150 mass parts or less. If the mixing amount of the curing agent is less than 50 mass parts, the glass transition temperature is sometimes reduced due to insufficient crosslinking, and if it is more than 170 mass parts, it is sometimes accompanied by a reduction in moisture resistance, high heat deformation temperature, and heat stability. In addition, in the case of using bisphenol A type epoxy resin alone as a thermosetting resin main agent, or using a mixture of bisphenol A type epoxy resin and the high heat-resistant epoxy resin illustrated before, sometimes not using a curing agent can improve heat resistance and is therefore more preferred. For example, in the case of setting the total mass of the thermosetting resin main agent to 100%, the mixing ratio of the high heat-resistant epoxy resin can be 10 mass % or more and 50 mass %, more preferably 10 mass % or more and 25 mass % or less. If it is this range, heat resistance is also improved, and thickening will not be added in addition, so it is preferred.

[0067] In the thermosetting resin composition constituting the sealing material 20, a curing accelerator can also be added as an optional component. As the curing accelerator, imidazole or its derivatives, tertiary amines, boric acid esters, Lewis acids, organic metal compounds, organic acid metal salts, etc. can be appropriately mixed. The amount of the curing accelerator added is preferably set to 0.01 mass parts or more and 50 mass parts or less relative to 100 mass parts of the thermosetting resin main agent, and more preferably set to 0.1 mass parts or more and 20 mass parts or less.

[0068] The thermosetting resin composition constituting the sealing material 20 may further contain optional additives within a range that does not hinder its characteristics. As additives, for example, flame retardants, pigments for coloring the resin, plasticizers for improving crack resistance, and silicone elastomers can be cited, but are not limited to these. These optional components and their addition amounts can be appropriately determined by those skilled in the art according to the specifications required by the semiconductor device and / or the sealing material.

[0069] The sealing material 20 may be a one-layer structure composed of one resin having the composition exemplified above, or may be a structure including two or more layers. A layer of a thermoplastic resin or silicone rubber may be further provided on the one or more thermosetting resin layers.

[0070] In addition, in order to illustrate the present invention, Figure 1 The cross-sectional structure of a specific module is shown and described in the figure, but the structure of the semiconductor device is not limited to the method shown in the figure. For example, the conductive connecting member can also be only one of the lead frame, the lead, and the implant pin, or it can have two or more of them. In addition, it can also be a shell-less semiconductor device without a shell. In addition, for example, it can also be set as the following semiconductor device: it also has a printed circuit board connected to the surface electrode of the semiconductor element through the implant pin, and the printed circuit board is insulated and sealed.

[0071] Regarding the manufacture of the semiconductor device, for example, the semiconductor element 11 is bonded to the heat sink 13 and the laminated substrate 12 using the solder material of the first embodiment. Next, the housing 16 is mounted and fixed to the heat sink 13 using a resin or the like. Thereafter, the lead frame 18 is bonded and the wire bonding using the aluminum wire 14 is performed. Depending on the structure of the semiconductor device, the implant pin and the printed circuit board can also be optionally bonded. Next, the thermosetting resin composition constituting the sealing material 20 is injected into the housing 16 and heat-cured. The heat-curing process can be set as a two-stage curing, for example, when epoxy resin is used as the main agent of the thermosetting resin, it is heated at 90°C to 120°C for 1 hour to 2 hours to become a semi-cured state. Thereafter, it is further heated at 175°C to 185°C for 1 hour to 2 hours, thereby enabling full curing. However, it is not limited to a specific temperature and time, and there are also cases where it is not necessary to set it as a two-stage curing. The caseless semiconductor device can be manufactured by bonding the laminate substrate and the semiconductor element with the solder material of the first embodiment, mounting conductive connection members such as a lead frame and aluminum wire, placing them in a mold, and filling them with a sealing material.

[0072] In the semiconductor device of the third embodiment, the semiconductor element, the laminated substrate, or the cooler are bonded by the solder material of the first embodiment. Therefore, cracks are unlikely to occur, and a highly reliable device can be formed.

[0073] Example

[0074] The present invention will be described in more detail below with reference to the following examples, but the present invention is not limited to the following examples.

[0075] [Example]

[0076] (1) Evaluation of mechanical properties of solder materials

[0077] A sample was produced by adding 0 to 8 mass % of Cu to an alloy containing 6 mass % of Sb, 4 mass % of Ag and 0.25 mass % of Ni, with the remainder consisting of Sn and inevitable impurities. As the mechanical properties of the sample, the elongation at break, Young's modulus and creep rupture elongation at 175°C were evaluated.

[0078] Based on JIS Z2241:2011 metal material tensile test method, the stress-strain curve of the tensile test was obtained, the Young's modulus was calculated based on the slope of the curve, and the elongation at break (%) was calculated based on the strain at break (when the stress becomes 0). Figure 2A The shape of the test piece is shown in Figure 2B Shown in Figure 2A Cross-sectional view at line XX. Figure 2A The length L1 of the test piece used was 12.0 mm, the length L2 of both ends was 3.9 mm, and the diameter of both ends was 2mm, the length L3 of the marking part is 2.4mm, and the diameter The dumbbell-shaped specimen is 1 mm. At a strain rate of 2.0×10 -3 A tensile test was conducted at a speed of 1 / s and a temperature of 175°C using a micro tensile tester (manufactured by Saginomiya Seisakusho, model: LMH-207).

[0079] Based on JIS Z2271:2010 creep and creep rupture test methods for metal materials, the creep curve was obtained, and the creep rupture elongation was obtained from the elongation at rupture. The same test piece as the tensile test was used for the test piece. For the creep rupture test, the same equipment as the tensile test was used at a constant load of 7N (8.92MPa) and a temperature of 175°C.

[0080] exist Figure 3 The relationship between the Cu content in the solder material and the normalized elongation at break is shown in FIG. The normalized elongation at break is a relative value when the elongation at break when the Cu content is 0 is set to 1. Figure 3 , indicating that the value of the elongation at break increases when the Cu content is in the range of 3 mass % or more and 8 mass % or less.

[0081] exist Figure 4 The relationship between the Cu content in the solder material and the normalized creep rupture elongation is shown in FIG. The normalized creep rupture elongation is a relative value when the creep rupture elongation when the Cu content is 0 is set to 1. Figure 4, compared with the case where the Cu content is 0, when the Cu content is 3 mass% or more, the normalized creep rupture elongation increases by more than 40%. In addition, the creep characteristics become the maximum in the range of Cu content of 5 mass% to 7 mass%, and the normalized creep rupture elongation becomes more than twice as large as the case where the Cu content is 0. When the Cu content exceeds 7 mass%, the creep characteristics decrease, but as long as the Cu content is 8 mass% or less, the normalized creep rupture elongation is maintained at a state where the normalized creep rupture elongation increases by more than 40% compared with the case where the Cu content is 0.

[0082] Even when the Cu content in the solder material was changed from 0 mass % to 8 mass %, the value of the normalized Young's modulus hardly changed (not shown in the graph).

[0083] (2) Reliability evaluation of semiconductor devices

[0084] Solder materials of samples 1 to 18 having the compositions shown in Tables 1 and 2 below were prepared. The following power semiconductor modules were manufactured: Figure 1 The joint between the Si semiconductor element of the semiconductor element 11 shown and the laminated substrate 12 having a first conductive plate 121 and a second conductive plate 123a and 123b made of Cu is provided with a solder joint layer 10 formed by melting the solder material. Regarding the joining conditions, the holding temperature is set to 260°C to 290°C and the holding time is set to 100 seconds to 160 seconds in a N2 reducing environment. The solder between the laminated substrate and the semiconductor element is applied using a metal mask having an opening of 3.2 mm square and a thickness of 200 μm. The paste solder used in this embodiment uses a general flux with rosin as the main component. In addition, for the paste solder, a solder obtained by kneading the rosin-based flux and a solder powder with a particle size of 25 μm to 45 μm in a mass ratio of 1:1 is used.

[0085] [T j Evaluation of P / C tolerance]

[0086] By T j Power cycle tolerance (T j The reliability of power semiconductor modules is evaluated by the power cycle test. vjThe condition of operating the device at 75°C for 1 second (setting the current value to 150°C) and pausing for 9 to 15 seconds (setting the current value to 75°C) is set as one cycle. The number of cycles until the current or voltage shows abnormality is set as the P / C tolerance. Regarding the evaluation criteria for P / C tolerance, the case of more than 50k cycles is set as A, the case of more than 40k cycles and less than 50k cycles is set as B, the case of more than 25k cycles and less than 40k cycles is set as C, and the case of less than 25k cycles is set as D.

[0087] [Evaluation of Wettability]

[0088] The surface tension was measured using a Wilhelmy wetting tester (manufactured by RHESCA; SAT-5100, in accordance with JIS Z3198-4). This is the following measurement method: the contact angle is obtained based on the force applied to the periphery of the front end of the test piece in contact with the liquid surface when the test piece is lifted after being immersed in the liquid. Regarding the test conditions, the immersion temperature was 270°C, and a 5×30×0.3mm test piece of phosphorus deoxidized copper (C1220) was used and coated with an appropriate amount of rosin-based flux to implement the test. The immersion speed was set to 5mm / sec, the immersion depth was set to 2mm, and the immersion time was set to 10sec. Regarding the evaluation criteria, a surface tension of less than 500mN / m is set to A, a surface tension of 500mN / m or more and less than 525mN / m is set to B, and a surface tension of 525mN / m or more is set to D. In addition, the surface tension of evaluation A is less than 500mN / m, which is the surface tension of Sn3.0Ag0.5Cu (a solder material containing 3% by mass of Ag, 0.5% by mass of Cu, and the rest of Sn and inevitable impurities) which is a general solder material in industry. When the surface tension is less than 500mN / m, no defects such as voids are observed at the solder joint and its interface, which is preferred. When the surface tension is greater than 500mN / m and less than 525mN / m, although there is no problem in practical use, sometimes tiny voids of about 1.0mm are generated, so the judgment is set to B. On the other hand, when the surface tension is greater than 525mN / m (D), voids are easily generated at the joint and its interface during module assembly (after solder bonding), and the void diameter and generation rate are both increased. When the surface tension is 525 mN / m or more, the maximum void diameter exceeds 1.5 mm when observed by ultrasonic testing (SAT), which leads to a decrease in module reliability, and is therefore not preferable.

[0089] The following Tables 1 and 2 show the composition of the solder material used as the evaluation sample, the T j P / C tolerance and determination results, as well as evaluation results of the wettability of solder materials.

[0090] [Table 1]

[0091]

[0092] According to the results of samples 1 to 6, when the Cu content was 3.2 mass% to 8 mass%, the life of the semiconductor module was extended by more than about 1.5 times. It is estimated that this is because the creep characteristics became more than 1.3 times. In addition, when the Cu content was 5.2 mass% to 8 mass%, the life of the semiconductor module was extended by more than about 1.7 times. It is estimated that this is because the creep characteristics were improved by more than 2.0 times.

[0093] On the other hand, in the power semiconductor module in which the solder material of sample 8 with reduced Sb is used for the bonding layer, cracks are observed in the Sn phase of the solder bonding layer after the power cycle test. It is speculated that this is the result of the weakening of the solid solution strengthening effect due to insufficient addition of Sb, which results in damage in the Sn part. Since the amount of Sb is small, stress relaxation caused by the deformation of Sn is preferentially exhibited. It is believed that a higher content of Sb is preferred. The solder material of sample 9 with increased Sb cannot be said to have good wettability, and there are parts where voids are observed. In the power semiconductor module in which the solder material of sample 12 is used for the bonding layer, tiny cracks of about 30μm to 50μm are observed centered on the Sn phase of the solder bonding layer. When the content of Ag is 2% by mass or more, Ag3Sn densely dispersed in the solder structure suppresses local deformation (deformation of the Sn phase), so it is considered to be preferred. In addition, it was confirmed from sample 10 that when Ag is more, extremely tiny voids with a diameter of about 1.0mm are generated. Although there is no problem in practical use, it is considered that the P / C tolerance is slightly reduced compared with Sample 11 due to the presence of the voids.

[0094] It is confirmed from Table 1 that by using a solder material containing Sb, Ag, Ni, and Cu within a specified range to form a solder joint layer, a highly reliable power semiconductor module with a P / C tolerance of 50k cycles or more can be obtained. It can be considered that under the composition within the specified range, the slip exhibited by the addition of Cu during the P / C test improves the stress relaxation effect of the solder material, thereby improving the tolerance.

[0095] [Table 2]

[0096]

[0097] In Table 2, "-" indicates poor wettability, and it is difficult to implement the P / C test due to voids in the initial structure and scattered solder balls (solder solidification). According to Table 2, in the power semiconductor module using the solder materials of samples 13 to 16 for the bonding layer, cracks were observed in the grain boundaries of the Sn phase (grain boundaries of β-Sn) of the solder bonding layer after the power cycle test. Since Cu6Sn5 was not generated in the structure of samples 13 and 14, the creep characteristics were not improved due to the improvement of the slip characteristics. Although Cu6Sn5 was generated in samples 15 and 16, it was sparsely distributed, so it is believed that the effect of adding Cu was not fully exerted. As a result, cracks occurred in the grain boundaries of β-Sn in samples 13 to 16, and the life was reached. In samples 17 and 18, the Ag content deviated from the eutectic combination (3.5 mass% or more and 5.0 mass% or less), thereby reducing the wettability, so it is believed that voids and solder balls were generated. In the solder joint of Sample 18, AgSn compounds such as Ag3Sn were excessively generated, resulting in an inhomogeneous structure.

[0098] The solder alloy of the present invention can be applied to general welding parts. In particular, it can be ideally used for components that generate large amounts of heat, such as power semiconductor devices such as LED elements and power diodes. The solder alloy of the present invention has excellent elongation at break and creep properties (creep elongation at break) at high temperatures, thereby improving the reliability of the solder joint. In particular, an increase in tolerance was confirmed in P / C tests using IGBT modules. The increase in resistance caused by the generation of cracks, which is a problem during high-temperature operation, can be eliminated by improving the elongation at break and creep properties.

[0099] Description of Reference Numerals

[0100] 10: bonding layer; 11: semiconductor element; 12: laminated substrate; 121: first conductive plate; 122: insulating substrate; 123a, 123b: second conductive plate; 13: heat sink; 14: aluminum wire; 15: external terminal; 16: housing; 17: bonding layer; 18: lead frame; 20: sealing layer.

Claims

1. A solder material comprising 5.0 mass % to 10.0 mass % of Sb, 2.0 mass % to 6.0 mass % of Ag, 0.1 mass % to 0.5 mass % of Ni, and 3.0 mass % to 8.0 mass % of Cu, with the remainder being Sn and unavoidable impurities.

2. The solder material according to claim 1, wherein The solder material contains 4.5 mass % or more and 8.0 mass % or less of Cu.

3. The solder material according to claim 1, wherein The solder material contains 6.0 mass % or more and 8.5 mass % or less of Sb.

4. The solder material according to claim 2, wherein The solder material contains 6.0 mass % or more and 8.5 mass % or less of Sb.

5. The solder material according to claim 1, wherein The solder material contains 3.0 mass % or more and 6.0 mass % or less of Ag.

6. The solder material according to claim 2, wherein The solder material contains 3.0 mass % or more and 6.0 mass % or less of Ag.

7. The solder material according to claim 3, wherein The solder material contains 3.0 mass % or more and 6.0 mass % or less of Ag.

8. The solder material according to claim 1, wherein The solder material is used for bonding semiconductor elements.

9. A solder joint, comprising: A solder bonding layer formed by melting the solder material according to claim 1; as well as The body to be joined includes a metal layer on a surface in contact with the solder joining layer.

10. A semiconductor device comprising a semiconductor element bonded to a laminate substrate and a conductive connection member bonded to the semiconductor element, wherein: The semiconductor device includes the solder joint according to claim 9 between the multilayer substrate and the semiconductor element or between the semiconductor element and the conductive connecting member.

11. A semiconductor device comprising a semiconductor element bonded to a laminate substrate and a cooler bonded to a surface of the laminate substrate opposite to a surface to which the semiconductor element is bonded, wherein: The semiconductor device includes the solder joint according to claim 9 between the multilayer substrate and the cooler.