Method for removing extracellular antibiotic resistance gene by sulfurized nano zero-valent iron

By using sulfide nanoscale zero-valent iron with controllable hydrophilicity, hydrophobicity and electron transfer ability, the double helix structure of the resistance gene is destroyed and bond breaking is solved, which solves the problems in the existing technology of poor antibiotic resistance gene removal effect and difficulty in inhibiting natural transformation. problems, achieving the effect of efficiently removing and reducing health risks.

CN118745017AInactive Publication Date: 2024-10-08ZHEJIANG UNIV

Patent Information

Application Number
CN202410745354.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies are not effective in removing antibiotic resistance genes from groundwater, and nanoscale zero-valent iron is easily passivated and has poor electron selectivity, making it difficult to effectively inhibit the natural transformation of resistance genes.

Method used

Sulfated nanoscale zero-valent iron with controllable hydrophilicity, hydrophobicity and electron transfer ability is used to adjust the surface properties of the material by changing the dosage of sulfur reagent, destroying the double helix structure of the resistance gene and inducing bond breaking, thereby removing the resistance gene and reducing its Natural transformation ability.

Benefits of technology

Significantly improves the removal efficiency of resistance genes and inhibits their natural transformation ability, reducing environmental and human health risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004886258960000011
    Figure HDA0004886258960000011
  • Figure HDA0004886258960000012
    Figure HDA0004886258960000012
  • Figure HDA0004886258960000021
    Figure HDA0004886258960000021
Patent Text Reader

Abstract

The invention discloses a method for removing extracellular antibiotic resistance genes by using sulfurized nano zero-valent iron, in particular to a method for achieving the purpose of efficiently removing the extracellular antibiotic resistance genes of underground water by regulating and controlling the sulfur content of the sulfurized nano zero-valent iron and changing the physicochemical properties of the sulfurized nano zero-valent iron, and relates to the field of underground water pollution treatment. According to the method, ferric chloride, sodium borohydride and sodium hydrosulfite are used for synthesizing sulfurized nano zero-valent iron with different sulfur contents, so that the hydrophilic-hydrophobic property and electron transfer performance of the surface of a material are regulated and controlled, and various antibiotic resistance genes are efficiently removed and the natural transformation capability of extracellular antibiotic resistance genes is reduced under an anaerobic condition; and the health risk of antibiotic resistance in underground water is reduced from the two aspects of concentration and environmental behavior.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of groundwater pollution control, and in particular to a method for removing extracellular antibiotic resistance genes by using sulfide nano zero-valent iron. Background Art

[0002] Antibiotic resistance genes (ARGs) are a new pollutant, and the drug resistance caused by them has been listed by the World Health Organization as one of the major public health threats in the 21st century. Antibiotic resistance genes are not only widely detected in various environmental media, but can also spread through vertical gene transfer and horizontal gene transfer. Extracellular antibiotic resistance genes are widely present in natural water bodies and can spread in the environment through natural transformation pathways. Groundwater, as a source of drinking water, contains a large number of antibiotic resistance genes, which pose a threat to human health.

[0003] At present, traditional antibiotic resistance gene treatment processes (ultraviolet, chlorination, ozonation, etc.) have disadvantages such as poor removal effect, generation of disinfection byproducts, and promotion of horizontal gene transfer, and are not suitable for groundwater pollution remediation. Nano zero-valent iron, as a widely used groundwater in-situ remediation material, has good adsorption affinity for extracellular antibiotic resistance genes, but nano zero-valent iron is easy to react with water for hydrogen evolution, and has disadvantages such as easy passivation and poor electron selectivity. Sulfidation can increase the hydrophobicity of the material to inhibit the hydrogen evolution reaction, improve electron selectivity, and at the same time improve the electron transfer performance, thereby increasing the reaction activity. Theoretical studies have shown that these properties can promote the removal of resistance genes. On the one hand, due to the instability of hydrogen bonds and base stacking in the double helix structure of deoxyribonucleic acid, it is easier to be destroyed on the hydrophobic surface. On the other hand, electrons can induce the scission of nucleotide bonds in aqueous solution. Therefore, the preparation of hydrophobic and excellent electron transfer performance of sulfided nano zero-valent iron is the key to the treatment of extracellular antibiotic resistance gene pollution in groundwater. Summary of the invention

[0004] The purpose of the present invention is to address the deficiencies of the prior art and provide a method for removing extracellular antibiotic resistance genes using sulfide nano zero-valent iron.

[0005] The objective of the present invention is achieved through the following technical scheme: a method for removing extracellular antibiotic resistance genes by using sulfide nano zero-valent iron, the method specifically comprising: adding sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability to a water body containing extracellular antibiotic resistance genes, fully reacting under anaerobic conditions, and simultaneously completing the removal of the extracellular antibiotic resistance genes in the water body and the reduction of the natural conversion ability of the extracellular antibiotic resistance genes.

[0006] Furthermore, the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability is prepared by the following method:

[0007] (1) Take 57.93 g of ferric chloride and dilute to 1 L with ultrapure water to obtain a concentration of 20 g / L of Fe 3+ Reserve solution, let stand for 6 to 24 hours;

[0008] (2) 6.8 g of sodium borohydride and 0.1-0.6 g of sodium dithionite are added to 200 ml of deionized water and dissolved to obtain a sulfur solution;

[0009] (3) Add 100 ml of Fe 3+ The sulfur solution prepared in step (2) was dripped into the Fe solution at a rate of 5 to 15 ml / min under nitrogen atmosphere and stirring at 200 to 400 rpm. 3+ solution until the sulfur solution is completely dripped;

[0010] (4) subsequently using a magnet to separate the solid from the liquid to obtain a solid; washing the solid three times with oxygen-free deionized water, vacuum drying at 50 to 70° C. for 6 to 12 hours to obtain a dry solid; and slowly oxidizing the dry solid in a vacuum drying oven for 1 to 3 hours to obtain a surface-oxidized solid;

[0011] (5) Grinding the surface oxidized solid obtained in step (4) into a powder to obtain sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability.

[0012] Furthermore, the concentration of the extracellular antibiotic resistance gene in the water body is 10 3 ~10 10 Number of copies per microliter.

[0013] Furthermore, the addition concentration of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability is 0.1 to 1 g / L.

[0014] Furthermore, the temperature of the water body is 20-30°C.

[0015] Furthermore, the sufficient reaction time is greater than 10 minutes.

[0016] Furthermore, the extracellular antibiotic resistance gene is an extracellular tetM antibiotic resistance gene, an extracellular sul2 antibiotic resistance gene, an extracellular Bla TEM antibiotic resistance gene, extracellular addA antibiotic resistance gene or extracellular cat antibiotic resistance gene.

[0017] The beneficial effects of the present invention are as follows: by changing the dosage of the sulfur reagent, the surface hydrophilicity and electron transfer performance of the sulfide nano zero-valent iron are changed; on the one hand, the hydrophobic surface can destroy the double helix structure of the resistance gene, induce the exposure of the base, thereby changing its morphology, thereby inhibiting its natural transformation ability; on the other hand, through electron transfer, the resistance gene is induced to break bonds, thereby achieving the purpose of effective removal rather than simple adsorption: in summary, these two properties enhance the removal of the extracellular antibiotic resistance gene by the material, and inhibit its natural transformation behavior in the environment, further reducing the risk of the spread of the extracellular antibiotic resistance gene in the environment and the health risk to the human body. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A graph showing the change in extracellular tetM antibiotic resistance gene concentration as a function of reaction time when the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example remove extracellular tetM antibiotic resistance gene;

[0019] Figure 2 The normalized apparent rate constant of the extracellular tetM antibiotic resistance gene when the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example remove the extracellular tetM antibiotic resistance gene;

[0020] Figure 3 This is a graph showing the decrease in the natural transformation efficiency of the extracellular tetM antibiotic resistance gene after being treated with the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example;

[0021] Figure 4 A relationship diagram of the added sulfur-iron molar ratio and the measured sulfur-iron molar ratio of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example;

[0022] Figure 5 The water contact angle diagrams of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example;

[0023] Figure 6 The Nyquist diagrams and their equivalent circuit models and fitted equivalent resistance diagrams of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example, wherein: Figure 6(a) is the Nyquist plot and its equivalent circuit model diagram of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example, Figure 6 (b) is a fitted equivalent resistance diagram of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example;

[0024] Figure 7 A graph showing the relationship between the normalized apparent rate constant and the material properties of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example;

[0025] Figure 8 The UV-visible absorption spectra of the resistance gene in the supernatant after the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Example 1 and the nano zero-valent iron prepared in the comparative example were treated, wherein: Figure 8 (a) is a UV-visible absorption spectrum of the resistance gene in the supernatant after being treated with the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Example 1, Figure 8 (b) is the UV-visible absorption spectrum of the resistance gene in the supernatant after treatment with nano zero-valent iron prepared in the comparative example;

[0026] Fig. 9 The electrophoresis diagram of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Example 1 and the nano zero-valent iron prepared in the comparative example after being treated with a plasmid carrying a resistance gene, wherein: Fig. 9 (a) is the electrophoresis diagram of the plasmid carrying the resistance gene after being treated with the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Example 1, Fig. 9 (b) is the electrophoresis diagram of the plasmid carrying the resistance gene after being treated with nano zero-valent iron prepared in the comparative example;

[0027] Fig.10 A graph showing the change in extracellular tetM antibiotic resistance gene concentration as a function of reaction time when the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example are used to remove extracellular tetM antibiotic resistance genes in groundwater matrix;

[0028] Fig.11 This is a diagram showing the removal effect of five different extracellular antibiotic resistance genes in groundwater matrix by the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Example 1;

[0029] Fig.12This is a diagram showing the continuous removal effect of the extracellular tetM antibiotic resistance gene in the groundwater matrix by the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability prepared in Example 1. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0032] The present invention provides a method for removing extracellular antibiotic resistance genes by using sulfide nano zero-valent iron. The method specifically comprises: adding sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability into a water body containing the extracellular antibiotic resistance genes, fully reacting under anaerobic conditions, and simultaneously completing the removal of the extracellular antibiotic resistance genes in the water body and the reduction of the natural conversion ability of the extracellular antibiotic resistance genes.

[0033] The sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability is prepared by the following method:

[0034] (1) Take 57.93 g of ferric chloride and dilute to 1 L with ultrapure water to obtain a concentration of 20 g / L of Fe 3+ Reserve solution, let stand for 6 to 24 hours;

[0035] (2) 6.8 g of sodium borohydride and 0.1-0.6 g of sodium dithionite are added to 200 ml of deionized water and dissolved to obtain a sulfur solution;

[0036] (3) Add 100 ml of Fe 3+ The sulfur solution prepared in step (2) was dripped into the Fe solution at a rate of 5 to 15 ml / min under nitrogen atmosphere and stirring at 200 to 400 rpm. 3+ solution until the sulfur solution is completely dripped;

[0037] (4) subsequently using a magnet to separate the solid from the liquid to obtain a solid; washing the solid three times with oxygen-free deionized water, vacuum drying at 50 to 70° C. for 6 to 12 hours to obtain a dry solid; and slowly oxidizing the dry solid in a vacuum drying oven for 1 to 3 hours to obtain a surface-oxidized solid;

[0038] (5) Grinding the surface oxidized solid obtained in step (4) into a powder to obtain sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability.

[0039] The concentration of the extracellular antibiotic resistance gene in the water body is 10 3 ~10 10 Number of copies per microliter.

[0040] The addition concentration of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability is 0.1-1 g / L.

[0041] The temperature of the water body is 20-30°C.

[0042] The sufficient reaction time is greater than 10 minutes.

[0043] The extracellular antibiotic resistance gene is an extracellular tetM antibiotic resistance gene, an extracellular sul2 antibiotic resistance gene, an extracellular Bla TEM antibiotic resistance gene, extracellular addA antibiotic resistance gene or extracellular cat antibiotic resistance gene.

[0044] Example 1 Preparation of a sulfide nanometer zero-valent iron (0.056-SNZVI) with controllable hydrophilicity and electron transfer ability

[0045] (1) Take 57.93 g of ferric chloride and dilute to 1 L with ultrapure water to obtain a concentration of 20 g / L of Fe 3+ Reserve solution, let stand for 12h;

[0046] (2) 6.8 g of sodium borohydride and 0.43 g of sodium dithionite were added to 200 ml of deionized water and dissolved to obtain a sulfur solution;

[0047] (3) Add 100 ml of Fe 3+ The sulfur solution prepared in step (2) was dripped into the Fe solution at a rate of 10 ml / min under nitrogen atmosphere and stirring at 350 rpm. 3+ solution until the sulfur solution is completely dripped;

[0048] (4) Subsequently, a magnet is used to separate the solid from the liquid to obtain a solid; the solid is washed three times with oxygen-free deionized water, and vacuum dried at 60° C. for 8 hours to obtain a dry solid; and the dry solid is slowly oxidized in a vacuum drying oven for 2 hours to obtain a surface-oxidized solid;

[0049] (5) Grinding the surface oxidized solid obtained in step (4) into a powder to obtain sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability.

[0050] The measured sulfur-iron molar ratio of the sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability prepared in Example 1 is 0.056, so it is recorded as 0.056-SNZVI; the surface property of 0.056-SNZVI is hydrophobic and has strong electron transfer ability.

[0051] Example 2 Preparation of a sulfide nanometer zero-valent iron (0.028-SNZVI) with controllable hydrophilicity and electron transfer ability

[0052] (1) Take 57.93 g of ferric chloride and dilute to 1 L with ultrapure water to obtain a concentration of 20 g / L of Fe 3+ Reserve solution, let stand for 12h;

[0053] (2) 6.8 g of sodium borohydride and 0.22 g of sodium dithionite were added to 200 ml of deionized water and dissolved to obtain a sulfur solution;

[0054] (3) Add 100 ml of Fe 3+ The sulfur solution prepared in step (2) was dripped into the Fe solution at a rate of 10 ml / min under nitrogen atmosphere and stirring at 350 rpm. 3+ solution until the sulfur solution is completely dripped;

[0055] (4) Subsequently, a magnet is used to separate the solid from the liquid to obtain a solid; the solid is washed three times with oxygen-free deionized water, and vacuum dried at 60° C. for 8 hours to obtain a dry solid; and the dry solid is slowly oxidized in a vacuum drying oven for 2 hours to obtain a surface-oxidized solid;

[0056] (5) Grinding the surface oxidized solid obtained in step (4) into a powder to obtain sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability.

[0057] The measured sulfur-iron molar ratio of the sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability prepared in Example 2 is 0.028, so it is recorded as 0.028-SNZVI; the surface property of 0.028-SNZVI is hydrophobic, and the electron transfer ability is strong.

[0058] Example 3 Preparation of a sulfide nano-zero-valent iron (0.017-SNZVI) with controllable hydrophilicity and electron transfer ability

[0059] (1) Take 57.93 g of ferric chloride and dilute to 1 L with ultrapure water to obtain a concentration of 20 g / L of Fe 3+ Reserve solution, let stand for 12h;

[0060] (2) 6.8 g of sodium borohydride and 0.11 g of sodium dithionite were added to 200 ml of deionized water and dissolved to obtain a sulfur solution;

[0061] (3) Add 100 ml of Fe 3+ The sulfur solution prepared in step (2) was dripped into the Fe solution at a rate of 10 ml / min under nitrogen atmosphere and stirring at 350 rpm. 3+ solution until the sulfur solution is completely dripped;

[0062] (4) Subsequently, a magnet is used to separate the solid from the liquid to obtain a solid; the solid is washed three times with oxygen-free deionized water, and vacuum dried at 60° C. for 8 hours to obtain a dry solid; and the dry solid is slowly oxidized in a vacuum drying oven for 2 hours to obtain a surface-oxidized solid;

[0063] (5) Grinding the surface oxidized solid obtained in step (4) into a powder to obtain sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability.

[0064] The measured sulfur-iron molar ratio of the hydrophobic and electron-transfer-capable sulfide nano-zero-valent iron prepared in Example 3 is 0.017, so it is recorded as 0.017-SNZVI; the surface property of 0.017-SNZVI is hydrophilic, and the electron-transfer capacity is relatively weak.

[0065] Comparative Example 1 Preparation of Nano Zero-Valent Iron (NZVI)

[0066] (1) Take 57.93 g of ferric chloride and dilute to 1 L with ultrapure water to obtain a concentration of 20 g / L of Fe 3+ Reserve solution, let stand for 12h;

[0067] (2) taking 6.8 g of sodium borohydride, adding it to 200 ml of deionized water, and dissolving it to obtain a sodium borohydride solution;

[0068] (3) Add 100 ml of Fe 3+ The stock solution and 100 ml of deionized water were added to the Fe solution at a rate of 10 ml / min under nitrogen atmosphere and stirring at 350 rpm. 3+ solution until the sodium borohydride solution is completely dropped;

[0069] (4) Subsequently, a magnet is used to separate the solid from the liquid to obtain a solid; the solid is washed three times with oxygen-free deionized water, and vacuum dried at 60° C. for 8 hours to obtain a dry solid; and the dry solid is slowly oxidized in a vacuum drying oven for 2 hours to obtain a surface-oxidized solid;

[0070] (5) Grinding the surface oxidized solid obtained in step (4) into powder to obtain nano zero-valent iron (NVZI) with hydrophilicity and weak electron transfer ability; the surface properties of NVZI are hydrophilicity and weak electron transfer ability.

[0071] Application Example 1

[0072] 10 mg of sulfide nano zero-valent iron (0.056-SNZVI, 0.028-SNZVI and 0.017-SNZVI) with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and nano zero-valent iron (NZVI) prepared in the comparative example were respectively placed in 170 ml serum bottles; the serum bottles were then transferred to an anaerobic glove box, and 100 ml of 10 6 The deoxygenated deionized water contained extracellular tetM antibiotic resistance gene (eARGs-tetM) at a copy number / μL (copies / μL); the deoxygenated deionized water was obtained by nitrogen aeration for 30 minutes to simulate the anoxic environment in groundwater; and then covered with a Mininert polytetrafluoroethylene valve.

[0073] The serum bottles were placed on a horizontal oscillator at 190 rpm and 25°C. 0.2 ml of liquid was taken from the serum bottle at a preset time point, filtered using a 0.22 μm water filter membrane, and the concentration of the remaining resistance gene in the liquid was detected using a real-time fluorescence quantitative PCR instrument. The measured results were as follows: Figure 1 and Figure 2 shown.

[0074] Figure 1 The graph is a graph showing the change in extracellular tetM antibiotic resistance gene concentration as the reaction time changes when the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example remove the extracellular tetM antibiotic resistance gene. Figure 1 It can be seen that with the increase of the sulfur-iron ratio, the removal effect of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability on the extracellular tetM antibiotic resistance gene increases, and is significantly greater than the effect of nano zero-valent iron. In addition, the sulfide nano zero-valent iron (0.056-SNZVI) with hydrophobic surface properties and strong electron transfer ability obtained in Example 1 has the best effect.

[0075] Figure 2 The normalized apparent rate constants of the removal of extracellular tetM antibiotic resistance genes by the sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano-zero-valent iron prepared in the comparative example. Figure 2It can be seen that the reaction activity of sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability in removing extracellular tetM antibiotic resistance gene increases with the increase of sulfur-iron ratio, and the normalized apparent rate constant of sulfide nano zero-valent iron (0.056-SNZVI) with hydrophobic surface properties and strong electron transfer ability obtained in Example 1 is 22 times that of NZVI, indicating that its reaction activity is significantly improved.

[0076] Application Example 2

[0077] 10 mg of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example were respectively placed in a 50 ml headspace bottle, and then 10 ml of 10 9.8 The invention relates to a method for preparing a novel nanostructured carbon foam containing deoxygenated deionized water containing extracellular tetM antibiotic resistance gene (ARGs-tetM) at a concentration of 100 copies / μL; the air in the headspace bottle is then evacuated, nitrogen is introduced, and the cover is immediately covered with a Mininert polytetrafluoroethylene valve; the deoxygenated deionized water is obtained by nitrogen aeration for 30 minutes; the headspace bottle is placed on an upside-down oscillator, 0.2 ml of liquid is taken at a preset time, and filtered using a 0.22-micron water filter membrane; after diluting 5 times, a transformation experiment is carried out using competent Escherichia coli DH5α as a transformation receptor.

[0078] Take 1 μl of supernatant and 100 μl of competent Escherichia coli DH5α in a 2 ml centrifuge tube and gently mix them, place them in an ice water bath for 30 minutes, heat shock them in a 42°C water bath for 90 minutes, then place them on ice for 2 minutes, and finally add 900 μl of lysate broth (LB) medium and culture them at 37°C for 1 hour (180 rpm); after the culture is completed, spread 100 μL of the bacterial solution on an LB agar plate containing tetracycline (10 mg / L), and count the resulting colonies after culturing at 37°C for 36 hours.

[0079] Figure 3 The figure shows the decrease in the natural transformation efficiency of the extracellular tetM antibiotic resistance gene after being treated with the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example. Figure 3It can be seen that the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability and nano zero-valent iron can generally inhibit the natural transformation process of extracellular antibiotic resistance genes after treatment; however, after being treated with sulfide nano zero-valent iron (0.056-SNZVI) with hydrophobic surface properties and strong electron transfer ability for 5 minutes, its natural transformation process can be completely inhibited. Compared with the treatment effect of nano zero-valent iron, the efficiency is greatly improved. The natural transformation ability of extracellular antibiotic resistance genes can be reduced in a short time, and environmental health risks can be reduced. The sulfide nano zero-valent iron prepared by the present invention has outstanding substantial characteristics and significant progress compared with nano zero-valent iron.

[0080] Application Example 3

[0081] The added sulfur-iron molar ratios of the sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 were 0.035, 0.070 and 0.140, respectively, and the measured sulfur-iron molar ratios were 0.017, 0.028 and 0.056, respectively; the added sulfur-iron molar ratio and the measured sulfur-iron molar ratio of the nano-zero-valent iron prepared in the comparative example were both 0; the added sulfur-iron molar ratio and the actual sulfur-iron molar ratio were linearly fitted to obtain the relationship between the two, as shown in FIG. Figure 4 As shown. Figure 4 It can be seen that the measured sulfur-iron molar ratio ([S / Fe] 实测 ) and the molar ratio of sulfur and iron added ([S / Fe] 投加 ) is [S / Fe] 实测 =0.39×[S / Fe] 投加 , R 2 =0.996.

[0082] Application Example 4

[0083] Using the water contact angle test, the hydrophilicity and hydrophobicity of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the hydrophilicity and hydrophobicity of the nano zero-valent iron prepared in the comparative example were tested. The test results are as follows: Figure 5 As shown. Figure 5 It can be seen that the water drop angle of the sulfide nano zero-valent iron with different sulfur contents prepared by the present invention increases with the increase of sulfur content, indicating that its hydrophobicity increases. The water drop angle of 0.056-SNZVI obtained in Example 1 is the largest and the most hydrophobic.

[0084] Application Example 5

[0085] Electrochemical impedance spectroscopy analysis was performed on the hydrophilicity and hydrophobicity of the sulfide nano zero-valent iron with controllable electron transfer capacity prepared in Examples 1 to 3 and the hydrophilicity and hydrophobicity of the nano zero-valent iron prepared in the comparative example, and the Nyquist plot was drawn. The fitted equivalent resistance was obtained by equivalent circuit fitting, as shown in FIG. Figure 6 As shown (where Figure 6 (a) is the Nyquist diagram and equivalent circuit fitting illustration. Figure 6 (b) is the fitted equivalent resistance). Figure 6 (a) and Figure 6 As can be seen from (b), the fitted equivalent resistance of the sulfide nano zero-valent iron with different sulfur contents prepared by the present invention decreases with the increase of sulfur content, indicating an increase in its electron transfer performance. The fitted equivalent resistance of 0.056-SNZVI is the smallest and its electron transfer ability is the strongest.

[0086] Combination Figure 2 , Figure 4 , Figure 5 , Figure 6 (a) and Figure 6 (b) It can be found that the hydrophilicity and electron transfer resistance of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example have a good correlation with their removal of extracellular antibiotic resistance genes (in order of R 2 =0.73, R 2 =0.92), and taking sulfur content as a comprehensive indicator, its linear fitting correlation increased to R 2 =0.94, such as Figure 7 As shown. In summary, unlike the conventional method of removing resistance genes by generating reactive oxygen species, this method can directly regulate the hydrophilicity and electron transfer properties of the material surface, and achieve efficient removal of multiple extracellular antibiotic resistance genes under anaerobic conditions and reduce the natural transformation ability of extracellular antibiotic resistance genes, thereby reducing the health risks of antibiotic resistance in groundwater from the two aspects of concentration and environmental behavior. This has inspiring significance for the preparation, synthesis and regulation of materials in the future.

[0087] Application Example 6

[0088] 10 mg of the hydrophobic and electron-transfer-capable sulfide nano-zero-valent iron prepared in Example 1 and the nano-zero-valent iron prepared in the comparative example were respectively placed in a 50 ml headspace bottle, and then 10 ml of 10 9.8 The invention relates to a method for preparing a novel nanostructured carbon foam film comprising: adding deoxygenated deionized water containing extracellular tetM antibiotic resistance gene (ARGs-tetM) at a concentration of 100 copies / μL; then evacuating the air in the headspace bottle, flushing with nitrogen, and then covering it with a Mininert polytetrafluoroethylene valve; the deoxygenated deionized water is obtained by nitrogen aeration for 30 minutes; placing the headspace bottle on an upside-down oscillator, taking 0.2 ml of liquid at a preset time, and filtering it with a 0.22-micron water filter membrane; and testing the ultraviolet-visible absorption spectrum of the supernatant between 240 and 280 nm.

[0089] Figure 8The UV-visible absorption spectra of the resistance gene in the supernatant after being treated with the sulfide nano zero-valent iron (0.056-SNZVI) with strong hydrophobicity and electron transfer ability prepared in Example 1 and the nano zero-valent iron (NZVI) prepared in the comparative example, wherein: Figure 8 (a) is the UV-visible absorption spectrum of the resistance gene in the supernatant after being treated with the sulfide nano zero-valent iron (0.056-SNZVI) with strong hydrophobicity and electron transfer ability prepared in Example 1, Figure 8 (b) is the UV-visible absorption spectrum of the resistance gene in the supernatant after treatment with nano zero-valent iron (NZVI) prepared in the comparative example. Figure 8 (a) It can be seen that the UV-visible absorption spectrum of the supernatant after treatment with 0.056-SNZVI prepared in Example 1 has obvious hyperchromic effect (increase in absorbance value) and blue shift phenomenon (spectrum moves toward short wavelength), indicating that 0.056-SNZVI induces the exposure of bases in the double helix structure of the resistance gene and causes structural damage; Figure 8 (b) It can be seen that after the NZVI prepared in Comparative Example 1 was treated, the UV-visible absorption spectrum of the supernatant only had a slight color enhancement effect, and no blue shift occurred: the hydrophobic surface induced the exposure and structural changes of the resistance gene bases.

[0090] Application Example 7

[0091] 10 mg of the hydrophobic and electron-transfer-capable sulfide nano-zero-valent iron prepared in Example 1 and the nano-zero-valent iron prepared in the comparative example were respectively placed in a 50 ml headspace bottle, and then 10 ml of 10 9.8 The invention relates to a method for preparing a novel nanostructured carbon foam bottle comprising: adding deoxygenated deionized water containing 100 copies / μL of the extracellular tetM antibiotic resistance gene (ARGs-tetM); then evacuating the air in the headspace bottle, flushing with nitrogen, and covering it with a Mininert polytetrafluoroethylene valve; the deoxygenated deionized water is obtained by aeration with nitrogen for 30 minutes; placing the headspace bottle on an upside-down oscillator, taking 0.2 ml of liquid at a preset time, and filtering it with a 0.22-micron water filter membrane; and observing the changes in the supernatant carrying the resistance gene plasmid using agarose gel electrophoresis.

[0092] Fig. 9 The electrophoretic diagram of the sulfide nano zero-valent iron (0.056-SNZVI) with strong hydrophobicity and electron transfer ability prepared in Example 1 and the nano zero-valent iron (NZVI) prepared in the comparative example after treatment with the resistance gene plasmid, wherein: Fig. 9 (a) is the electrophoresis diagram of the plasmid carrying the resistance gene after being treated with the sulfide nano zero-valent iron (0.056-SNZVI) with strong hydrophobicity and electron transfer ability prepared in Example 1, Fig. 9(b) is the electrophoresis diagram of the plasmid carrying the resistance gene after being treated with nano zero-valent iron (NZVI) prepared in the comparative example. Fig. 9 (a) shows the change of the conformation of the plasmid carrying the resistance gene after being treated with the sulfide nano zero-valent iron (0.056-SNZVI) having strong hydrophobicity and electron transfer ability prepared in Example 1; Fig. 9 (b) shows the changes in the conformation of the plasmid carrying the resistance gene after being treated with the nano zero-valent iron (NZVI) prepared in the comparative example. Fig. 9 (a) It can be seen that after being treated with 0.056-SNZVI prepared in Example 1, the supercoiled morphology of the plasmid in the supernatant was almost completely transformed into an open ring morphology, indicating that one of the double helical chains of the plasmid was broken at one or more locations; Fig. 9 (b) It can be seen that the comparative example NZVI can also induce changes in plasmid morphology because it also has electron transfer properties. However, compared with the 0.056-SNZVI prepared in Example 1, which has a stronger electron transfer ability, it only induces morphological changes in part of the plasmid: the ring-opening process reveals the existence of bond breaking behavior. At the same time, the change in brightness also shows that the 0.056-SNZVI prepared in Example 1 achieves rapid removal of plasmids compared to the comparative example NZVI.

[0093] In summary, Application Examples 6 and 7 show that by utilizing this method, the double helix structure of the resistance gene can be destroyed, the bases can be exposed, and the bonds can be broken, thereby achieving the purpose of efficiently removing and inhibiting the natural transformation ability.

[0094] Application Example 8

[0095] 10 mg of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example were respectively placed in a 170 ml serum bottle, transferred to an anaerobic glove box, and then 100 ml of 10 6 Deoxygenated groundwater containing 100 copies / μL of the extracellular tetM antibiotic resistance gene; the deoxygenated groundwater was obtained by nitrogen aeration for 30 minutes to simulate the anoxic environment in groundwater; and then covered with a Mininert polytetrafluoroethylene valve.

[0096] The serum bottle was placed on a horizontal oscillator at 190 rpm and 25°C. 0.2 ml of liquid was taken from the serum bottle at a preset time point, filtered using a 0.22 μm water filter membrane, and the concentration of the remaining resistance gene in the liquid was detected using a real-time fluorescence quantitative PCR instrument. The measured results were as follows: Fig.10 shown.

[0097] Fig.10The graph of the change in extracellular tetM antibiotic resistance gene concentration as a function of reaction time when the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer capacity prepared in Examples 1 to 3 and the nano zero-valent iron prepared in the comparative example are used to remove extracellular tetM antibiotic resistance genes in groundwater matrix. Fig.10 It can be seen that in the groundwater matrix, with the increase of sulfur-iron ratio, the removal effect of sulfide nano-zero-valent iron on the extracellular tetM antibiotic resistance gene increases, which is significantly greater than the effect of nano-zero-valent iron, and the sulfide nano-zero-valent iron (0.056-SNZVI) with hydrophobic surface properties and strong electron transfer ability has the best effect.

[0098] Application Example 9

[0099] 10 mg of the sulfide nano-zero-valent iron (0.056-SNZVI) with controllable hydrophilicity and electron transfer capacity prepared in Example 1 was taken into a 170 ml serum bottle, which was transferred to an anaerobic glove box, and 100 ml of 10 6 copies / μL of extracellular antibiotic resistance genes (extracellular tetM antibiotic resistance gene, extracellular sul2 antibiotic resistance gene, extracellular Bla TEM Antibiotic resistance gene, extracellular addA antibiotic resistance gene and extracellular cat antibiotic resistance gene) in deoxygenated groundwater; the deoxygenated groundwater was obtained by nitrogen aeration for 30 minutes, intending to simulate the anoxic environment in groundwater; and then covered with a Mininert polytetrafluoroethylene valve.

[0100] The serum bottle was placed on a horizontal oscillator at 190 rpm and 25°C. 0.2 ml of liquid was taken from the serum bottle at a preset time point, filtered using a 0.22 μm water filter membrane, and the concentration of the remaining resistance gene in the liquid was detected using a real-time fluorescence quantitative PCR instrument. The measured results were as follows: Fig.11 shown.

[0101] Fig.11 The sulfide nano-zero-valent iron (0.056-SNZVI) with controllable hydrophilicity and electron transfer capacity prepared in Example 1 was used to inhibit five different extracellular antibiotic resistance genes (extracellular tetM antibiotic resistance gene, extracellular sul2 antibiotic resistance gene, extracellular Bla TEM The removal effect diagram of antibiotic resistance genes, extracellular addA antibiotic resistance genes and extracellular cat antibiotic resistance genes. Fig.11 As shown, 0.056-SNZVI has a good removal effect and removal rate for five extracellular antibiotic resistance genes, indicating the universality of sulfide nano-zero-valent iron in removing extracellular antibiotic resistance genes.

[0102] Application Example 10

[0103] 10 mg of the hydrophobic and electron-transfer-capable sulfide nano-zero-valent iron (0.056-SNZVI) prepared in Example 1 was placed in a 170 ml serum bottle, which was transferred to an anaerobic glove box, and 100 ml of 10 6 Deoxygenated groundwater containing extracellular tetM antibiotic resistance genes (ARGs-tetM) at 300 copies / μL; the deoxygenated groundwater was obtained by nitrogen aeration for 30 minutes to simulate the anoxic environment in groundwater; and then covered with a Mininert polytetrafluoroethylene valve.

[0104] The serum bottle was placed on a horizontal oscillator at 190 rpm and 25°C. Every 10 minutes, 0.2 ml of liquid was taken from the serum bottle, filtered with a 0.22 μm water filter membrane, and a certain amount of ARGs-tetM stock solution was added to increase the concentration to 10. 6 copies / μL; 10 minutes as one cycle, a total of 20 cycles were performed; the concentration of the remaining resistance gene in the liquid was detected by real-time fluorescence quantitative PCR instrument, and the measured results were as follows Fig.12 shown.

[0105] Fig.12 The figure shows the continuous removal effect of the extracellular tetM antibiotic resistance gene in groundwater matrix by the sulfide nano zero-valent iron (0.056-SNZVI) with controllable hydrophilicity and electron transfer capacity prepared in Example 1. Fig.12 As shown, 0.056-SNZVI has a continuous and stable removal effect on antibiotic resistance genes. The concentration of antibiotic resistance genes after treatment is stabilized at 0-10 copies / μL, and the removal rate reaches 99.999%, indicating that in practical applications it can stably remove a large number of extracellular antibiotic resistance genes and has good environmental application potential.

[0106] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for removing extracellular antibiotic resistance genes by using sulfide nano-zero-valent iron, characterized in that: The method specifically comprises: adding sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability to a water body containing extracellular antibiotic resistance genes, allowing the reaction to fully proceed under anaerobic conditions, and simultaneously completing the removal of the extracellular antibiotic resistance genes in the water body and the reduction of the natural conversion ability of the extracellular antibiotic resistance genes.

2. The method for removing extracellular antibiotic resistance genes by sulfide nano-zero-valent iron according to claim 1, characterized in that: The sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability is prepared by the following method: (1) Take 57.93 g of ferric chloride and dilute to 1 L with ultrapure water to obtain a concentration of 20 g / L of Fe 3+ Reserve solution, let stand for 6 to 24 hours; (2) 6.8 g of sodium borohydride and 0.1-0.6 g of sodium dithionite are added to 200 ml of deionized water and dissolved to obtain a sulfur solution; (3) Add 100 ml of Fe 3+ The sulfur solution prepared in step (2) was dripped into the Fe solution at a rate of 5 to 15 ml / min under nitrogen atmosphere and stirring at 200 to 400 rpm. 3+ solution until the sulfur solution is completely dripped; (4) subsequently using a magnet to separate the solid from the liquid to obtain a solid; washing the solid three times with oxygen-free deionized water, vacuum drying at 50 to 70° C. for 6 to 12 hours to obtain a dry solid; and slowly oxidizing the dry solid in a vacuum drying oven for 1 to 3 hours to obtain a surface-oxidized solid; (5) Grinding the surface oxidized solid obtained in step (4) into a powder to obtain sulfide nano-zero-valent iron with controllable hydrophilicity and electron transfer ability.

3. The method for removing extracellular antibiotic resistance genes by using sulfide nano-zero-valent iron according to claim 1, characterized in that: The concentration of the extracellular antibiotic resistance gene in the water body is 10 3 ~10 10 Number of copies per microliter.

4. The method for removing extracellular antibiotic resistance genes by using sulfide nano-zero-valent iron according to claim 1, characterized in that: The addition concentration of the sulfide nano zero-valent iron with controllable hydrophilicity and electron transfer ability is 0.1-1 g / L.

5. The method for removing extracellular antibiotic resistance genes by using sulfide nano-zero-valent iron according to claim 1, characterized in that: The temperature of the water body is 20-30°C.

6. The method for removing extracellular antibiotic resistance genes by using sulfide nano-zero-valent iron according to claim 1, characterized in that: The sufficient reaction time is greater than 10 minutes.

7. The method for removing extracellular antibiotic resistance genes by using sulfide nano-zero-valent iron according to claim 1, characterized in that: The extracellular antibiotic resistance gene is an extracellular tetM antibiotic resistance gene, an extracellular sul2 antibiotic resistance gene, an extracellular Bla TEM antibiotic resistance gene, extracellular addA antibiotic resistance gene or extracellular cat antibiotic resistance gene.

Citation Information

Patent Citations

  • Production of nanoscale zero-valent iron subjected to vulcanization modification and application in treatment of antibiotic resistance genes

    CN110862137A

  • Vulcanized nano zero-valent iron with controllable sulfur content and form as well as preparation method and application of vulcanized nano zero-valent iron

    CN114799199A

  • Iron-based nano material for in-situ remediation of heavy metal combined pollution of underground water in mining area as well as preparation method and application of iron-based nano material

    CN117401785A

Cited By

  • Method for rapidly starting dye-organic wastewater anaerobic co-metabolism system based on S-nZVI

    CN119390239A