A method for preparing low specific surface area white carbon black for reinforcing butyl rubber

By preparing primary silica via precipitation and combining it with acyl chlorinated lignin treatment, the problem of poor dispersibility of silica in butyl rubber was solved. This resulted in high dispersibility and good compatibility of low specific surface area silica in butyl rubber, improving the strength, abrasion resistance, and low-temperature resistance of the vulcanized rubber.

CN118754141BActive Publication Date: 2024-11-22SHANDONG LINK SCI & TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411244179.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

In the preparation of butyl rubber matrix, the high specific surface area of ​​silica results in poor dispersion in butyl rubber, which weakens the reinforcing ability and reduces wear resistance and low temperature resistance.

Method used

Primary silica was prepared by precipitation method, cationic surfactant was added and two-stage aging was carried out, combined with acyl chlorinated lignin treatment, to improve the dispersibility of primary silica and its compatibility with butyl rubber.

Benefits of technology

The resulting silica has a low specific surface area and high dispersibility, which improves the strength and abrasion resistance of the vulcanized rubber and ensures its low-temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a method for preparing low specific surface area white carbon black for reinforcing butyl rubber, belonging to the technical field of white carbon black; the preparation method comprises the steps of preparing primary white carbon black, preparing chlorinated lignin, and grafting; the grafting step comprises the steps of adding primary white carbon black and chlorinated lignin into dimethyl sulfoxide, heating the mixture to 60-64°C at a rate of 1.7-2.3°C / min, reacting the mixture for 6.3-6.7h, stirring the mixture while reacting the mixture at a rate of 136-145rpm, filtering and washing the mixture after the reaction, drying the mixture at 25-20°C for 5.3-5.7h, and drying the mixture at 38-34°C for 8.4-8.6h to obtain the white carbon black; the white carbon black obtained by the method has good reinforcing performance for butyl rubber while reducing the specific surface area, and the obtained vulcanized rubber has high strength, good wear resistance and good low temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of white carbon black, and in particular relates to a method for preparing white carbon black with low specific surface area for reinforcing butyl rubber. Background Art

[0002] White carbon black is a general term for white powdery X-ray amorphous silicic acid and silicate products, mainly referring to precipitated silica, fumed silica and ultrafine silica gel, and also including powdered synthetic aluminum silicate and calcium silicate. White carbon black is a porous substance, and its composition can be expressed by SiO2·nH2O, where nH2O exists in the form of surface hydroxyl groups. It is soluble in caustic alkali and hydrofluoric acid, insoluble in water, solvents and acids other than hydrofluoric acid, resistant to high temperatures, tasteless and odorless, and has good electrical insulation.

[0003] In the prior art, when preparing tire tread rubber with a butyl rubber matrix, white carbon black is usually used to reinforce the butyl rubber. However, white carbon black with a high specific surface area agglomerates in the butyl rubber matrix and has poor dispersibility, resulting in a weakened reinforcing ability of white carbon black.

[0004] Therefore, providing a method for preparing low specific surface area white carbon black for reinforcing butyl rubber has become a new research and development direction.

[0005] CN103466640A discloses a method for reducing the BET specific surface area of ​​white carbon black prepared by a sulfuric acid precipitation method, which specifically reduces the specific surface area of ​​white carbon black prepared by a sulfuric acid precipitation method by increasing the mass concentration of water glass to 20%-35% and the aging pH value to 4-10;

[0006] The white carbon black produced by the method of this patent reduces the specific surface area of ​​white carbon black and improves its dispersibility, but the specific surface area of ​​the white carbon black produced is still large; and the researchers also found that while reducing the specific surface area of ​​white carbon black, the dispersibility of white carbon black will be improved, but the reinforcing performance of white carbon black, especially the wear resistance and low temperature resistance, will be reduced, thereby affecting its application in the tire field.

[0007] Therefore, providing a method for preparing low specific surface area white carbon black for butyl rubber, while reducing the specific surface area, ensuring wear resistance and low temperature resistance is a technical problem that needs to be solved urgently in the prior art. Summary of the invention

[0008] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing low specific surface area white carbon black for reinforcing butyl rubber, which reduces the specific surface area while ensuring the wear resistance and low temperature resistance.

[0009] In view of the above technical problems, the present invention adopts the following technical solutions:

[0010] A method for preparing low specific surface area white carbon black for reinforcing butyl rubber includes the steps of preparing primary white carbon black, preparing acyl chloride lignin, and grafting. The specific operations are as follows:

[0011] 1. Preparation of primary white carbon black

[0012] (1) Preparation of mixed solution

[0013] Add sodium sulfate and water glass solution to the reaction kettle, heat to 56-60°C at a rate of 1.4-1.6°C / min, stir at 56-60°C for 20-25min, add sulfuric acid solution after stirring, control the pH to 8.0-8.3, stir at a speed of 187-206rpm for 46-53min, and obtain a mixed solution 1;

[0014] Add octadecyltrimethylammonium chloride and hydroxyethyl lauryldimethylammonium chloride to the water glass solution, and stir evenly to obtain a mixed solution II;

[0015] In the mixed solution 1, the mass ratio of the sodium sulfate and water glass solution is 1.20-1.22:427-432;

[0016] In the second mixed solution, the mass ratio of the water glass solution, octadecyl trimethyl ammonium chloride, and hydroxyethyl lauryl dimethyl ammonium chloride is 115-122:0.8-1.0:0.5-0.7;

[0017] The mass concentration of the water glass solution is 34-36%;

[0018] The mass concentration of the sulfuric acid solution is 67-70%;

[0019] (2) Reaction

[0020] The reactor was heated to 90-94°C at a rate of 0.4-0.6°C / min, and the mixed solution 2 and the sulfuric acid solution were added to the mixed solution 1 at a rate of 3.4-3.6 g / min. Ultrasonic treatment was performed for 10-16 min, the ultrasonic power was 102-107 W, and the ultrasonic frequency was 64-70 kHz. After the ultrasonic treatment, the mixture was stirred at 228-240 rpm for 27-32 min. The pH value was controlled at 9.7-10.0 during the reaction. After the reaction was completed, the sulfuric acid solution was continued to be added. The pH of the liquid is adjusted to 6.3-6.7 to obtain a white carbon black suspension, the white carbon black suspension is first placed at 87-91°C for 4.5-5.5 minutes, then cooled to 70-74°C at a rate of 0.4-0.6°C / min, and aged for 10-14 minutes. After the end of the thermal aging, sulfuric acid solution is added to control the pH to 4.0-4.2, and naturally reduced to room temperature, washed with water, filtered, and dried at 108-112°C to control the moisture content to 3.8-4.2wt%, to obtain primary white carbon black;

[0021] The mass ratio of the mixed solution 1 to the mixed solution 2 is 11.0-11.4:3.1;

[0022] The mass concentration of the sulfuric acid solution is 67-70%.

[0023] 2. Preparation of chlorinated lignin

[0024] (1) Dispersion

[0025] The lignin is placed in tetrahydrofuran, glyceryl monostearate and polyethylene glycol monolaurate are added, and homogenization is performed at a homogenization pressure of 4.8-5.2 MPa and a homogenization time of 4.3-4.7 min. After the homogenization is completed, the lignin is dried to obtain dispersed lignin;

[0026] The mass ratio of the lignin, tetrahydrofuran, glyceryl monostearate and polyethylene glycol monolaurate is 7.2-7.6:78-82:0.8-1.2:1.4-1.6;

[0027] (2) Acid treatment

[0028] The dispersed lignin is placed in a sealed container, sulfuric acid solution is added, and after being stirred evenly, the temperature is raised to 116-124°C at a rate of 1.0-1.4°C / min, and stirred at a speed of 180-190rpm for 2.8-3.2h. After the stirring is completed, it is filtered, washed, and dried, and then put into tetrahydrofuran, malic acid is added, and stirred at 38-43°C for 18-22min. After the stirring is completed, it is washed and dried to obtain acid-treated lignin;

[0029] The mass ratio of the dispersed lignin, sulfuric acid solution, tetrahydrofuran and malic acid is 6.0-6.4:25-29:27-32:1.6-1.8;

[0030] The mass concentration of the sulfuric acid solution is 30-34%;

[0031] (3) Acid chloride treatment

[0032] Add thionyl chloride and N, N-dimethylformamide to the acid-treated lignin, and then perform ultrasonic treatment, the ultrasonic time is 13-18 minutes, the ultrasonic power is 135-146W, the ultrasonic frequency is 45-50kHz, after the ultrasonic treatment, heat reflux reaction at 73-77°C, the reaction time is 28-32h, after the reaction is completed, filter, and dry at 78-82°C for 2.4-2.6h to obtain acyl chloride lignin;

[0033] The mass volumes of the acid-treated lignin, thionyl chloride and N,N-dimethylformamide are 1.8-2.4 g: 245-254 mL: 16-18 mL.

[0034] 3. Grafting

[0035] Add primary white carbon black and chlorinated lignin to dimethyl sulfoxide, heat to 60-64°C at a rate of 1.7-2.3°C / min, react for 6.3-6.7h, stir while reacting at a rate of 136-145rpm, filter and wash after the reaction, first dry at -25 to -20°C for 5.3-5.7h, then dry at -38 to -34°C for 8.4-8.6h, to obtain white carbon black;

[0036] The mass ratio of the dimethyl sulfoxide, primary white carbon black and acyl chloride lignin is 190-210:18-22:3.5-3.7.

[0037] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0038] 1. The present invention adopts a precipitation method to prepare primary white carbon black. A cationic surfactant is added to the mixed solution 2. The cationic surfactant will carry a positive charge after being dissolved in water. The negative charge on the surface of the primary white carbon black will interact with the positive charge on the surface of the cationic surfactant to form a Coulomb force, thereby improving the stability and dispersibility of the primary white carbon black particles, making the primary white carbon black particles uniform in size, reducing the temperature for preparing the mixed solution 1, and obtaining a relatively dense structure. In combination with the specific water glass mass concentration, the pH value in the reaction step and other parameters, and in the reaction step, two-stage aging is performed, thereby greatly reducing the specific surface area of ​​the primary white carbon black particles and improving the absorption value. , thereby improving the compatibility with components such as butyl rubber; the present invention performs a dispersion treatment on lignin to improve the dispersibility of lignin, and then performs an acid treatment and an acyl chloride treatment so that the surface of lignin contains acyl chloride groups, and after the primary white carbon black is fully activated by a surfactant, the lignin is subjected to an esterification reaction with the groups on the surface of the primary white carbon black, and the prepared white carbon black still has a low specific surface area and high dispersibility, so that the compatibility and affinity of lignin, primary white carbon black and butyl rubber are good, and the uniformity of dispersion in the matrix is ​​promoted, thereby improving the strength performance of the vulcanized rubber and ensuring the wear resistance and low temperature resistance;

[0039] 2. The white carbon black product prepared by the method of the present invention has a BET specific surface area of ​​108-117m 2 / g, DBP absorption value is 2.51-2.64mL / g, and loss on ignition is 3.0-3.6%;

[0040] 3. When the white carbon black product prepared by the method of the present invention is used to reinforce butyl rubber, the tensile strength of the vulcanized rubber is measured to be 27.2-28.1MPa, the elongation at break is 588-596%, the 300% elongation is 9.3-9.8MPa, and the volume abrasion is 95-101mm. 3 , tear strength is 55.6-57.1kN / m;

[0041] 4. When the white carbon black product prepared by the method of the present invention is used to reinforce butyl rubber, the vulcanized rubber is placed at -18°C for 120 hours, taken out and placed at -40°C for 96 hours. After the standing period, it is naturally restored to room temperature. The tensile strength of the vulcanized rubber is measured again to be 25.8-27.0MPa, the elongation at break is 557-571%, and the tear strength is 53.6-55.4kN / m. DETAILED DESCRIPTION

[0042] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.

[0043] Example 1

[0044] 1. Preparation of primary white carbon black

[0045] (1) Preparation of mixed solution

[0046] Add 1.21 g of sodium sulfate and 430 g of water glass solution to the reactor, heat to 58° C. at a rate of 1.5° C. / min, stir at 58° C. for 22 min, add sulfuric acid solution after stirring, control the pH to 8.2, stir and react at a speed of 200 rpm for 50 min, and obtain a mixed solution 1;

[0047] Add 0.9 g of octadecyltrimethylammonium chloride and 0.6 g of hydroxyethyl lauryldimethylammonium chloride to 118 g of water glass solution, and stir evenly to obtain a mixed solution 2;

[0048] The mass concentration of the water glass solution is 35%;

[0049] The mass concentration of the sulfuric acid solution is 68%;

[0050] (2) Reaction

[0051] The reactor was heated to 92°C at a rate of 0.5°C / min, and the mixed solution 2 and the sulfuric acid solution were added to the mixed solution 1 at a rate of 3.5 g / min. The mixed solution 2 and the sulfuric acid solution were added at a rate of 3.5 g / min, and ultrasonic treatment was performed. The ultrasonic time was 13 min, the ultrasonic power was 105 W, and the ultrasonic frequency was 67 kHz. After the ultrasonic treatment, the mixture was stirred at 234 rpm for 30 min. The pH value was controlled to be 10.0 during the reaction. After the reaction, the sulfuric acid solution was continued to be added to adjust the pH value to 6.5 to obtain a white carbon black suspension. The white carbon black suspension was first placed at 89°C for 5.5 min of heat preservation and aging, and then cooled to 72°C at a rate of 0.5°C / min, and the mixture was heat-aged for 12 min. After the heat preservation and aging, the sulfuric acid solution was added to control the pH value to 4.1, and the mixture was naturally cooled to room temperature. After washing and filtering, the mixture was dried at 110°C, and the moisture content was controlled to be 4.0 wt%, to obtain primary white carbon black.

[0052] The mass ratio of the mixed solution 1 to the mixed solution 2 is 11.2:3.1;

[0053] The mass concentration of the sulfuric acid solution is 68%.

[0054] 2. Preparation of chlorinated lignin

[0055] (1) Dispersion

[0056] 7.4 g of lignin was placed in 80 g of tetrahydrofuran, 1.0 g of glyceryl monostearate and 1.5 g of polyethylene glycol monolaurate were added, and homogenization was performed at a homogenization pressure of 5.0 MPa and a homogenization time of 4.5 min. After the homogenization, the mixture was dried to obtain dispersed lignin;

[0057] (2) Acid treatment

[0058] 6.2 g of dispersed lignin was placed in a sealed container, 27 g of sulfuric acid solution was added, and after being stirred evenly, the temperature was raised to 120°C at a rate of 1.2°C / min, and stirred at a speed of 185 rpm for 3.0 h. After the stirring was completed, the mixture was filtered, washed, and dried, and then placed in 30 g of tetrahydrofuran, 1.7 g of malic acid was added, and the mixture was stirred at 40°C for 20 min. After the stirring was completed, the mixture was washed and dried to obtain acid-treated lignin.

[0059] The mass concentration of the sulfuric acid solution is 32%;

[0060] (3) Acid chloride treatment

[0061] To 2.0 g of acid-treated lignin, 250 mL of thionyl chloride and 17 mL of N,N-dimethylformamide were added, followed by ultrasonic treatment. The ultrasonic time was 15 min, the ultrasonic power was 140 W, and the ultrasonic frequency was 47 kHz. After the ultrasonic treatment, the mixture was heated under reflux at 75 ° C for 30 h. After the reaction was completed, the mixture was taken out and dried at 80 ° C for 2.5 h to obtain acyl chloride lignin.

[0062] 3. Grafting

[0063] Add 20 g of primary white carbon black and 3.6 g of chlorinated lignin to 200 g of dimethyl sulfoxide, heat to 62 ° C at a rate of 2.0 ° C / min, react for 6.5 hours, stir while reacting, and stir at a rate of 140 rpm. After the reaction is completed, filter and wash, first dry at -23 ° C for 5.5 hours, and then dry at -36 ° C for 8.5 hours to obtain white carbon black.

[0064] Example 2

[0065] 1. Preparation of primary white carbon black

[0066] (1) Preparation of mixed solution

[0067] Add 1.20 g of sodium sulfate and 427 g of water glass solution to the reactor, heat to 56° C. at a rate of 1.4° C. / min, stir at 56° C. for 20 min, add sulfuric acid solution after stirring, control the pH to 8.0, stir and react at a speed of 187 rpm for 46 min, and obtain a mixed solution 1;

[0068] Add 0.8 g of octadecyltrimethylammonium chloride and 0.5 g of hydroxyethyl lauryldimethylammonium chloride to 115 g of water glass solution, and stir to obtain a mixed solution 2;

[0069] The mass concentration of the water glass solution is 34%;

[0070] The mass concentration of the sulfuric acid solution is 67%;

[0071] (2) Reaction

[0072] The reactor was heated to 90°C at a rate of 0.4°C / min, and the mixed solution 2 and the sulfuric acid solution were added to the mixed solution 1 at a rate of 3.4 g / min. The mixed solution 2 and the sulfuric acid solution were added at a rate of 3.4 g / min, and ultrasonic treatment was performed. The ultrasonic time was 10 min, the ultrasonic power was 102 W, and the ultrasonic frequency was 64 kHz. After the ultrasonic treatment, the mixture was stirred at 228 rpm for 27 min. The pH value was controlled to be 9.7 during the reaction. After the reaction, the sulfuric acid solution was continued to be added to adjust the pH value to 6.3 to obtain a white carbon black suspension. The white carbon black suspension was first placed at 87°C for 5.0 min of heat preservation and aging, and then cooled to 70°C at a rate of 0.4°C / min, and the mixture was aged for 10 min. After the heat preservation and aging, the sulfuric acid solution was added to control the pH value to 4.0, and the mixture was naturally reduced to room temperature. After washing and filtering, the mixture was dried at 108°C, and the moisture content was controlled to be 3.8 wt%, to obtain primary white carbon black.

[0073] The mass ratio of the mixed solution 1 to the mixed solution 2 is 11.0:3.1;

[0074] The mass concentration of the sulfuric acid solution is 67%.

[0075] 2. Preparation of chlorinated lignin

[0076] (1) Dispersion

[0077] 7.2 g of lignin was placed in 78 g of tetrahydrofuran, 0.8 g of glyceryl monostearate and 1.4 g of polyethylene glycol monolaurate were added, and homogenization was performed at a homogenization pressure of 4.8 MPa and a homogenization time of 4.3 min. After the homogenization, the mixture was dried to obtain dispersed lignin;

[0078] (2) Acid treatment

[0079] 6.0 g of dispersed lignin was placed in a sealed container, 25 g of sulfuric acid solution was added, and after being stirred evenly, the temperature was raised to 116°C at a rate of 1.0°C / min, and stirred at a speed of 180 rpm for 2.8 h. After the stirring was completed, the mixture was filtered, washed, and dried, and then placed in 27 g of tetrahydrofuran, 1.6 g of malic acid was added, and the mixture was stirred at 38°C for 18 min. After the stirring was completed, the mixture was washed and dried to obtain acid-treated lignin;

[0080] The mass concentration of the sulfuric acid solution is 30%;

[0081] (3) Acid chloride treatment

[0082] To 1.8 g of acid-treated lignin, 245 mL of thionyl chloride and 16 mL of N,N-dimethylformamide were added, followed by ultrasonic treatment. The ultrasonic time was 13 min, the ultrasonic power was 135 W, and the ultrasonic frequency was 45 kHz. After the ultrasonic treatment, the mixture was heated under reflux at 73 ° C for 28 h. After the reaction was completed, the mixture was taken out and dried at 78 ° C for 2.4 h to obtain acyl chloride lignin.

[0083] 3. Grafting

[0084] Add 18 g of primary white carbon black and 3.5 g of chlorinated lignin to 190 g of dimethyl sulfoxide, heat to 60 ° C at a rate of 1.7 ° C / min, react for 6.3 h, stir while reacting, and stir at a rate of 136 rpm. After the reaction, filter and wash, first dry at -25 ° C for 5.3 h, and then dry at -38 ° C for 8.4 h to obtain white carbon black.

[0085] Example 3

[0086] 1. Preparation of primary white carbon black

[0087] (1) Preparation of mixed solution

[0088] Add 1.22 g of sodium sulfate and 432 g of water glass solution to the reactor, heat to 60° C. at a rate of 1.6° C. / min, stir at 60° C. for 25 min, add sulfuric acid solution after stirring, control the pH to 8.3, stir and react at a speed of 206 rpm for 53 min, and obtain a mixed solution 1;

[0089] Add 1.0 g of octadecyltrimethylammonium chloride and 0.7 g of hydroxyethyl lauryldimethylammonium chloride to 122 g of water glass solution, and stir to obtain a mixed solution 2;

[0090] The mass concentration of the water glass solution is 36%;

[0091] The mass concentration of the sulfuric acid solution is 70%;

[0092] (2) Reaction

[0093] The reactor was heated to 94°C at a rate of 0.6°C / min, and the mixed solution 2 and the sulfuric acid solution were added to the mixed solution 1 at a rate of 3.6 g / min. The mixed solution 2 and the sulfuric acid solution were added at a rate of 3.6 g / min, and ultrasonic treatment was performed. The ultrasonic time was 16 min, the ultrasonic power was 107 W, and the ultrasonic frequency was 70 kHz. After the ultrasonic treatment, the mixture was stirred at 240 rpm for 32 min. The pH value was controlled to be 9.9 during the reaction. After the reaction, the sulfuric acid solution was continued to be added to adjust the pH value to 6.7 to obtain a white carbon black suspension. The white carbon black suspension was first placed at 91°C for 4.5 min of heat preservation and aging, and then cooled to 74°C at a rate of 0.6°C / min, and the mixture was aged for 14 min. After the heat preservation and aging, the sulfuric acid solution was added to control the pH value to 4.2, and the mixture was naturally reduced to room temperature. After washing and filtering, the mixture was dried at 112°C, and the moisture content was controlled to be 4.2 wt%, to obtain primary white carbon black.

[0094] The mass ratio of the mixed solution 1 to the mixed solution 2 is 11.4:3.1;

[0095] The mass concentration of the sulfuric acid solution is 70%.

[0096] 2. Preparation of chlorinated lignin

[0097] (1) Dispersion

[0098] 7.6 g of lignin was placed in 82 g of tetrahydrofuran, 1.2 g of glyceryl monostearate and 1.6 g of polyethylene glycol monolaurate were added, and homogenization was performed at a homogenization pressure of 5.2 MPa and a homogenization time of 4.7 min. After the homogenization, the mixture was dried to obtain dispersed lignin;

[0099] (2) Acid treatment

[0100] 6.4 g of dispersed lignin was placed in a sealed container, 29 g of sulfuric acid solution was added, and after being stirred evenly, the temperature was raised to 124°C at a rate of 1.4°C / min, and stirred at a speed of 190 rpm for 3.2 h. After the stirring was completed, it was filtered, washed, and dried, and then put into 32 g of tetrahydrofuran, 1.8 g of malic acid was added, and stirred at 43°C for 22 min. After the stirring was completed, it was washed and dried to obtain acid-treated lignin;

[0101] The mass concentration of the sulfuric acid solution is 34%;

[0102] (3) Acid chloride treatment

[0103] 254 mL of thionyl chloride and 18 mL of N,N-dimethylformamide were added to 2.4 g of acid-treated lignin, and then ultrasonic treatment was performed. The ultrasonic time was 18 min, the ultrasonic power was 146 W, and the ultrasonic frequency was 50 kHz. After the ultrasonic treatment, heating reflux reaction was carried out at 77 ° C for 32 h. After the reaction was completed, the lignin was taken out and dried at 82 ° C for 2.6 h to obtain acyl chloride lignin.

[0104] 3. Grafting

[0105] Add 22g of primary white carbon black and 3.7g of chlorinated lignin to 210g of dimethyl sulfoxide, heat to 64°C at a rate of 2.3°C / min, react for 6.7h, stir while reacting at a rate of 145rpm. After the reaction, filter and wash, first dry at -20°C for 5.7h, then dry at -34°C for 8.6h to obtain white carbon black.

[0106] Comparative Example 1

[0107] Based on Example 1, the changes are as follows:

[0108] (1) After the white carbon black suspension is obtained in the reaction step, the white carbon black suspension is placed at 80° C. for 17.5 minutes. After the aging, sulfuric acid solution is added to control the pH value to 4.1, and the suspension is naturally cooled to room temperature. After washing and filtering, the suspension is dried at 110° C. to control the moisture content to 4.0 wt%, thereby obtaining primary white carbon black;

[0109] (2) In the step of preparing acyl chloride lignin, the acid treatment and acyl chloride treatment steps are omitted; in the grafting step, an equal amount of acyl chloride lignin is replaced by dispersed lignin;

[0110] The rest of the operations are the same.

[0111] Comparative Example 2

[0112] Based on Example 1, the changes are as follows:

[0113] (1) In the step of preparing the mixed solution, the stirring temperature of the mixed solution 1 is controlled to 78° C., and the octadecyltrimethylammonium chloride and hydroxyethyllauryldimethylammonium chloride components in the mixed solution 2 are replaced by water glass solution in equal amounts, and the molar concentration of the water glass solution is 2.05 mol / L;

[0114] (2) In the step of preparing the chlorinated lignin, the dispersion treatment step is omitted; in the acid treatment step, the dispersed lignin is replaced with an equal amount of lignin that has not been treated in any way;

[0115] The rest of the operations are the same.

[0116] Performance Testing

[0117] (1) Basic properties of white carbon black

[0118] The performance of the white carbon black obtained in Examples 1-3 and Comparative Examples 1-2 was tested, and the results were as follows:

[0119]

[0120] (2) Reinforcement properties of silica for butyl rubber

[0121] The white carbon black obtained in Examples 1-3 and Comparative Examples 1-2 were respectively prepared into vulcanized rubbers, and the reinforcing properties for butyl rubber were measured, wherein the formula of the vulcanized rubber is as follows:

[0122]

[0123] The above formulas were mixed separately, and then vulcanized at 160° C. for 20 minutes to obtain vulcanized rubber. The performance of Examples 1-3 and the separately obtained vulcanized rubbers was tested, and the test results are as follows:

[0124]

[0125] The vulcanized rubbers prepared by the above formulas in Examples 1-3 and Comparative Examples 1-2 were placed at -18°C for 120 hours, taken out and placed at -40°C for 96 hours. After the standing period, the rubbers were naturally restored to room temperature and the strength performance was tested again. The test results are as follows:

[0126]

[0127] The present invention adopts a precipitation method to prepare primary white carbon black. A cationic surfactant is added to a mixed solution II. The cationic surfactant carries a positive charge after being dissolved in water. The negative charge on the surface of the primary white carbon black interacts with the positive charge on the surface of the cationic surfactant to form a Coulomb force, thereby improving the stability and dispersibility of the primary white carbon black particles, making the primary white carbon black particles uniform in size, reducing the temperature for preparing the mixed solution I, obtaining a relatively dense structure, combining specific water glass mass concentration, pH value in the reaction step and other parameters, and performing two-stage aging in the reaction step, thereby greatly reducing the primary white carbon black particles. The specific surface area is increased, and the absorption value is improved, thereby improving the compatibility with components such as butyl rubber; the present invention performs dispersion treatment on lignin to improve the dispersibility of lignin, and then performs acid treatment and acyl chloride treatment to make the surface of lignin contain acyl chloride groups, and after the primary white carbon black is fully activated by a surfactant, the lignin and the groups on the surface of the primary white carbon black are subjected to esterification reaction, so that the compatibility and affinity of lignin, primary white carbon black and butyl rubber are better, and the dispersion uniformity in the matrix is ​​promoted, thereby improving the strength performance of the vulcanized rubber and ensuring the wear resistance and low temperature resistance.

[0128] In Comparative Example 1, in the reaction step, the white carbon black suspension was kept at 80° C. for aging, which significantly increased the specific surface area of ​​the white carbon black and reduced the dispersion performance. In addition, the acid treatment and chlorination steps of the lignin were omitted. The dispersed lignin obtained was directly mixed with the primary white carbon black. The bonding force between the two was weak and the connection was unstable, which would reduce the wear resistance and stability of the vulcanized rubber and the strength performance was poor.

[0129] Comparative Example 2 increases the stirring temperature for preparing the mixed solution, and omits the octadecyltrimethylammonium chloride and hydroxyethyl lauryldimethylammonium chloride components in the mixed solution 2, which will result in uneven particle size, poor morphology, uneven structure, poor density, and high specific surface area of ​​the primary silica particles. In addition, Comparative Example 2 also omits the lignin dispersion step, which will result in incomplete acidification and chlorination treatment of the lignin, and insufficient grafting of lignin with the primary silica when grafted with the primary silica. The final silica product has poor stability. When used to reinforce butyl rubber, it has poor affinity with butyl rubber, reduces the strength and stability of the vulcanized rubber, and has poor wear resistance.

[0130] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.

[0131] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing low specific surface area white carbon black for reinforcing butyl rubber, characterized in that: The preparation method comprises the steps of preparing primary white carbon black, preparing acyl chloride lignin, and grafting; The method for preparing primary white carbon black comprises the steps of preparing a mixed solution and reacting; The step of preparing the mixed solution is to add sodium sulfate and water glass solution into a reaction kettle, heat it to 56-60°C at a rate of 1.4-1.6°C / min, stir it at 56-60°C for 20-25min, add sulfuric acid solution after stirring, control the pH value to 8.0-8.3, stir and react at a speed of 187-206rpm for 46-53min, and obtain a mixed solution 1; Add octadecyltrimethylammonium chloride and hydroxyethyl lauryldimethylammonium chloride to the water glass solution, and stir evenly to obtain a mixed solution II; The reaction step comprises: heating the reactor to 90-94° C. at a rate of 0.4-0.6° C. / min, adding the mixed solution 2 and the sulfuric acid solution to the mixed solution 1, controlling the adding rate to be 3.4-3.6 g / min, performing ultrasonic treatment, the ultrasonic time being 10-16 min, the ultrasonic power being 102-107 W, the ultrasonic frequency being 64-70 kHz, stirring and reacting at 228-240 rpm for 27-32 min after the ultrasonic treatment, controlling the pH value to be 9.7-10.0 during the reaction, and continuing to add A sulfuric acid solution is added to adjust the pH to 6.3-6.7 to obtain a white carbon black suspension; the white carbon black suspension is first placed at 87-91°C for 4.5-5.5 minutes of heat preservation and aging, then cooled to 70-74°C at a rate of 0.4-0.6°C / min, and heat-aged for 10-14 minutes. After the heat preservation and aging, a sulfuric acid solution is added to control the pH to 4.0-4.2, and the suspension is naturally cooled to room temperature. After washing and filtering, the suspension is dried at 108-112°C to control the moisture content to 3.8-4.2wt%, thereby obtaining primary white carbon black; The chlorination step of lignin includes dispersion, acid treatment and chlorination treatment steps; The dispersion step comprises placing lignin in tetrahydrofuran, adding glyceryl monostearate and polyethylene glycol monolaurate, and performing homogenization treatment at a homogenization pressure of 4.8-5.2 MPa and a homogenization time of 4.3-4.7 min. After the homogenization treatment is completed, drying is performed to obtain dispersed lignin; The acid treatment step comprises placing the dispersed lignin in a sealed container, adding a sulfuric acid solution, stirring evenly, heating to 116-124° C. at a rate of 1.0-1.4° C. / min, stirring at a speed of 180-190 rpm for 2.8-3.2 hours, filtering, washing, and drying after the stirring is completed, then putting into tetrahydrofuran, adding malic acid, stirring at 38-43° C. for 18-22 minutes, washing, and drying after the stirring is completed, to obtain the acid-treated lignin; The acyl chloride treatment step comprises adding thionyl chloride and N,N-dimethylformamide to the acid-treated lignin, and then performing ultrasonic treatment, wherein the ultrasonic time is 13-18 minutes, the ultrasonic power is 135-146W, and the ultrasonic frequency is 45-50kHz. After the ultrasonic treatment, heating reflux reaction is performed at 73-77°C for 28-32 hours. After the reaction is completed, filtering is performed, and drying is performed at 78-82°C for 2.4-2.6 hours to obtain acyl chloride lignin. The grafting step is to add primary white carbon black and chlorinated lignin into dimethyl sulfoxide, heat the mixture to 60-64°C at a rate of 1.7-2.3°C / min, react for 6.3-6.7 hours, stir the mixture while reacting, and stir at a rate of 136-145 rpm. After the reaction is completed, the mixture is filtered and washed, and then dried at -25 to -20°C for 5.3-5.7 hours, and then dried at -38 to -34°C for 8.4-8.6 hours to obtain white carbon black.

2. The method for preparing low specific surface area white carbon black for reinforcing butyl rubber according to claim 1, characterized in that: In the step of preparing the mixed solution, in the mixed solution 1, the mass ratio of the sodium sulfate and the water glass solution is 1.20-1.22:427-432; In the second mixed solution, the mass ratio of the water glass solution, octadecyl trimethyl ammonium chloride, and hydroxyethyl lauryl dimethyl ammonium chloride is 115-122:0.8-1.0:0.5-0.7; The mass concentration of the water glass solution is 34-36%; The mass concentration of the sulfuric acid solution is 67-70%.

3. The method for preparing low specific surface area white carbon black for reinforcing butyl rubber according to claim 1, characterized in that: In the reaction step, the mass ratio of the mixed solution 1 to the mixed solution 2 is 11.0-11.4:3.1; The mass concentration of the sulfuric acid solution is 67-70%.

4. The method for preparing low specific surface area white carbon black for reinforcing butyl rubber according to claim 1, characterized in that: In the dispersing step, the mass ratio of the lignin, tetrahydrofuran, glyceryl monostearate and polyethylene glycol monolaurate is 7.2-7.6:78-82:0.8-1.2:1.4-1.

6.

5. The method for preparing low specific surface area white carbon black for reinforcing butyl rubber according to claim 1, characterized in that: In the acid treatment step, the mass ratio of the dispersed lignin, the sulfuric acid solution, tetrahydrofuran and malic acid is 6.0-6.4:25-29:27-32:1.6-1.8; The mass concentration of the sulfuric acid solution is 30-34%.

6. The method for preparing low specific surface area white carbon black for reinforcing butyl rubber according to claim 1, characterized in that: In the acid chloride treatment step, the mass volumes of the acid-treated lignin, thionyl chloride, and N,N-dimethylformamide are 1.8-2.4 g: 245-254 mL: 16-18 mL.

7. The method for preparing low specific surface area white carbon black for reinforcing butyl rubber according to claim 1, characterized in that: In the grafting step, the mass ratio of the dimethyl sulfoxide, primary white carbon black and acyl chloride lignin is 190-210:18-22:3.5-3.7.

Citation Information

Patent Citations

  • Method for reducing specific surface area BET (Brunauer Emmet Teller) of white carbon black prepared by using sulfuric acid precipitation method

    CN103466640A

  • Modified white carbon black preparation method and modified white carbon black prepared therethrough

    CN108164754A

  • Secondary modified white carbon black for tires

    CN109096799A

  • Precipitation method white carbon black surface modification method

    CN111808441A

  • Preparation method of lignin-silicon dioxide composite material

    CN117430964A