Heat-insulating polyurethane material and preparation method thereof

By optimizing the raw material ratio for the preparation of polyurethane materials and adding diatomite-loaded hollow spherical silica and other ingredients, the problem of poor thermal insulation performance of polyurethane materials has been solved, the thermal insulation and mechanical properties have been significantly improved, and better thermal insulation has been achieved. Effect.

CN118755255AInactive Publication Date: 2024-10-11PENGDE RUBBER PLASTIC CO LTD

Patent Information

Application Number
CN202411245866.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polyurethane materials have poor thermal insulation properties, which limits their application. Traditional porous thermal insulation materials are difficult to maintain high porosity while maintaining pore size, which affects the thermal insulation effect.

Method used

By optimizing the raw material ratio for the preparation of polyurethane materials, diatomite-loaded hollow spherical silica, tin-doped titanium dioxide, fullerene, graphene and other ingredients are added to form composite fillers, improve the physical structure and chemical properties of the material, and enhance its Thermal insulation effect.

Benefits of technology

It significantly improves the thermal insulation and mechanical properties of polyurethane materials, ensuring its stable thermal insulation effect at high temperatures, reducing heat dissipation, and enhancing the application value of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a heat-insulating polyurethane material and a preparation method thereof, and belongs to the field of high polymer material preparation. According to the invention, the added treated diatomite-loaded hollow spherical silicon dioxide can be uniformly dispersed in the polyurethane prepolymer and has more excellent compatibility, and the physical structure of the diatomite-loaded hollow spherical silicon dioxide can effectively delay the effect of heat flow and is beneficial to improving the heat insulation performance; and meanwhile, a remarkable heat insulation effect can be further achieved through the synergistic effect with the composite filler. In addition, the added composite filler can form effective grafting with a molecular chain of polyurethane, a certain interface effect is achieved, and the heat insulation stability and the mechanical property of the polyurethane material can be improved. On the whole, through optimization of the raw materials and the raw material ratio, the physical structure and the chemical performance are matched with each other, and the remarkable heat insulation effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a heat-insulating polyurethane material and a preparation method thereof. Background Art

[0002] Thermal insulation materials refer to materials that can effectively block the transmission of heat flow. There are three ways of heat transmission in nature: heat convection, heat conduction and heat radiation. According to these three ways, thermal insulation materials can be divided into: heat reflective insulation materials, vacuum insulation materials and porous insulation materials. Heat reflective insulation materials have high infrared reflection ability and can reflect most of the heat into the atmosphere to achieve the purpose of heat insulation. However, heat reflective insulation materials use silver, aluminum foil or metal-plated polyimide, polyester film, etc., which have the problem of high preparation cost. Vacuum insulation materials mainly refer to vacuum insulation panels, which are composed of core insulation materials, gas adsorption materials and closed air-insulating films. However, vacuum insulation materials also have the problems of complex preparation process and high production cost. Porous insulation materials achieve the purpose of heat insulation by means of tiny pores inside the material. Traditional porous insulation materials include foam glass, foam polystyrene and foam polyurethane, but porous insulation materials are difficult to ensure the pore size while maintaining high porosity, which will also affect the insulation effect.

[0003] Polyurethane is the full name of polyurethane, which is a general term for macromolecular compounds containing repeated carbamate groups on the main chain. Polyurethane is made by processing raw materials into specific materials, and then blending the raw materials with various additives to form them. Polyurethane is often used as a thermal insulation material, especially for pipe insulation, but the polyurethane prepared in the prior art has poor thermal insulation performance as a whole, which limits its application. Therefore, it is of positive significance to further improve the thermal insulation performance of polyurethane materials. Summary of the invention

[0004] Based on this, in order to solve the problem of poor thermal insulation performance of polyurethane materials in the prior art, the present invention provides a thermal insulation polyurethane material and a preparation method thereof, and the specific technical scheme is as follows: A heat-insulating polyurethane material, comprising the following raw materials in parts by weight: 50 to 100 parts of a polyurethane prepolymer, 15 to 25 parts of a composite filler, 1 to 7 parts of a catalyst, 1 to 15 parts of an antioxidant, 1 to 3 parts of a stabilizer, and 1 to 10 parts of a leveling agent; The polyurethane prepolymer comprises the following raw materials in parts by weight: 25 to 40 parts of tetrahydrofuran, 15 to 50 parts of 4,4-dimethyl diisocyanate, 50 to 55 parts of polyethylene glycol, 25 to 40 parts of neopentyl glycol, and 9 to 15 parts of diatomaceous earth-loaded hollow spherical silica; The composite filler comprises the following raw materials in parts by weight: 5 to 10 parts of tin-doped titanium dioxide, 1 to 3 parts of fullerene, 1 to 5 parts of graphene and 25 to 30 parts of a treating agent.

[0005] Furthermore, the preparation method of the polyurethane prepolymer is as follows: under a nitrogen atmosphere, tetrahydrofuran is added to a reaction kettle, stirred at 80°C to 90°C for 1h to 3h, cooled to room temperature, and then polyethylene glycol and 4,4-dimethyl diisocyanate are added, stirred at 55°C to 65°C for 3h to 5h, and then neopentyl glycol is added, and the stirring reaction is continued at 70°C to 85°C for 15min to 30min to obtain a mixture; diatomaceous earth-loaded hollow spherical silica is added to the mixture, and stirred at 45°C to 55°C for 30min to 45min to obtain a polyurethane prepolymer.

[0006] Furthermore, the preparation method of the diatomite-loaded hollow spherical silica is as follows: adding a surfactant to the heat-treated diatomite, stirring at 65°C to 80°C for 20min to 30min, then adding the hollow spherical silica, ultrasonically dispersing for 30min to 45min, centrifuging and washing, calcining at 110°C to 120°C for 1h to 2h, and ball milling to obtain the diatomite-loaded hollow spherical silica.

[0007] Furthermore, the surfactant is one or a mixture of sodium stearate and hexamethylenetetramine.

[0008] Furthermore, the average particle size of the diatomaceous earth-loaded hollow spherical silica is 60nm~120nm.

[0009] Furthermore, the treatment agent is 3-aminopropyltriethoxysilane and isocyanate.

[0010] Furthermore, the preparation method of the composite filler is: adding tin-doped titanium dioxide to 3-aminopropyltriethoxysilane, stirring and treating at 45°C to 70°C for 45min to 60min to obtain pretreated tin-doped titanium dioxide; adding fullerene and graphene to isocyanate, stirring and treating at 65°C to 90°C for 30min to 45min to obtain a pretreated mixture of fullerene and graphene, and then stirring the pretreated mixture and the pretreated tin-doped titanium dioxide evenly, heating and drying, and ball milling to obtain the composite filler.

[0011] Furthermore, the antioxidant is at least one of antioxidant 1010 and antioxidant 1076.

[0012] Furthermore, the stabilizer is at least one of light stabilizer 292 and UV123.

[0013] In addition, the present application also provides a method for preparing a heat-insulating polyurethane material, the preparation method comprising the following steps: Add the polyurethane prepolymer, composite filler and catalyst into the reactor, stir and treat at 65°C~75°C for 1h~2h, then add the antioxidant, stabilizer and leveling agent, continue stirring for 2h~3h to obtain the heat-insulating polyurethane material.

[0014] Compared with the prior art, this application has the following beneficial effects: The present application optimizes the raw materials and raw material ratios for preparing polyurethane materials, so that the physical structure and chemical properties cooperate with each other to achieve a significant thermal insulation effect. Among them, the addition of diatomite-loaded hollow spherical silica can be evenly dispersed in the polyurethane prepolymer, the surface area of ​​the treated diatomite increases and the adsorption capacity in the pores is enhanced, the hollow spherical silica is effectively loaded, and the hollow spherical silica wrapped by diatomite has better compatibility in the polyurethane prepolymer, and the physical structure of the diatomite-loaded hollow spherical silica can effectively delay the effect of heat flow, which is beneficial to improving the thermal insulation performance, and the chemical properties also have a better thermal insulation effect, and the synergistic effect of it with the composite filler can also further improve the thermal insulation effect.

[0015] Tin-doped titanium dioxide in the composite filler has a certain absorption and reflection effect on ultraviolet light. Fullerene has a six-ring structure and graphene has a sheet structure and is interspersed in the polyurethane material. Adding components with different physical structures can delay the heat flow and effectively reduce heat dissipation. 3-aminopropyltriethoxysilane is used to treat tin-doped titanium dioxide to improve its compatibility in the system. Isocyanate is used to treat fullerene and graphene, which can form a steric hindrance with the -NCO group on the isocyanate on the outside, reducing the probability of agglomeration. At the same time, when added to the polyurethane material formula system, it can also effectively form an effective graft with the molecular chain of polyurethane, play a certain interface role, and also help to improve the thermal stability and mechanical properties of polyurethane materials. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0018] A heat-insulating polyurethane material in one embodiment of the present invention comprises the following raw materials in parts by weight: 50 to 100 parts of a polyurethane prepolymer, 15 to 25 parts of a composite filler, 1 to 7 parts of a catalyst, 1 to 15 parts of an antioxidant, 1 to 3 parts of a stabilizer, and 1 to 10 parts of a leveling agent; The polyurethane prepolymer comprises the following raw materials in parts by weight: 25 to 40 parts of tetrahydrofuran, 15 to 50 parts of 4,4-dimethyl diisocyanate, 50 to 55 parts of polyethylene glycol, 25 to 40 parts of neopentyl glycol, and 9 to 15 parts of diatomaceous earth-loaded hollow spherical silica; The composite filler comprises the following raw materials in parts by weight: 5 to 10 parts of tin-doped titanium dioxide, 1 to 3 parts of fullerene, 1 to 5 parts of graphene and 25 to 30 parts of a treating agent.

[0019] In one embodiment, the preparation method of the polyurethane prepolymer is as follows: under a nitrogen atmosphere, tetrahydrofuran is added to a reactor, stirred at 80°C to 90°C for 1h to 3h, cooled to room temperature, and then polyethylene glycol and 4,4-dimethyl diisocyanate are added, stirred at 55°C to 65°C for 3h to 5h, and then neopentyl glycol is added, and the stirring reaction is continued at 70°C to 85°C for 15min to 30min to obtain a mixture; diatomaceous earth-loaded hollow spherical silica is added to the mixture, and stirred at 45°C to 55°C for 30min to 45min to obtain a polyurethane prepolymer.

[0020] In one embodiment, the preparation method of the diatomite-loaded hollow spherical silica is as follows: adding a surfactant to the heat-treated diatomite, stirring at 65°C to 80°C for 20min to 30min, then adding the hollow spherical silica, ultrasonically dispersing for 30min to 45min, centrifuging and washing, calcining at 110°C to 120°C for 1h to 2h, and ball milling to obtain the diatomite-loaded hollow spherical silica.

[0021] In one embodiment, the heat treatment temperature is 500° C. to 600° C., and the time is 1 h to 3 h. After the heat treatment, the pore structure of the diatomite becomes larger and has fewer impurities.

[0022] In one embodiment, the surfactant is one or a mixture of sodium stearate and hexamethylenetetramine.

[0023] In one embodiment, the liquid-to-drink ratio of the diatomaceous earth volume to the surfactant is (1 g-5 g) / 10 mL.

[0024] In one embodiment, the mass ratio of the diatomaceous earth to the hollow spherical silica is (1-7): (1-5).

[0025] In one embodiment, the average particle size of the diatomaceous earth-loaded hollow spherical silica is 60 nm to 120 nm.

[0026] In one embodiment, the treating agent is 3-aminopropyltriethoxysilane and isocyanate.

[0027] In one embodiment, the preparation method of the composite filler is: adding tin-doped titanium dioxide to 3-aminopropyltriethoxysilane, stirring and treating at 45°C~70°C for 45min~60min to obtain pretreated tin-doped titanium dioxide; adding fullerene and graphene to isocyanate, stirring and treating at 65°C~90°C for 30min~45min to obtain a pretreated mixture of fullerene and graphene, and then stirring the pretreated mixture and the pretreated tin-doped titanium dioxide evenly, heating and drying, and obtaining a composite filler.

[0028] In one embodiment, the catalyst is dibutyltin dilaurate.

[0029] In one embodiment, the antioxidant is at least one of antioxidant 1010 and antioxidant 1076.

[0030] In one embodiment, the stabilizer is at least one of light stabilizer 292 and UV123.

[0031] In one embodiment, the leveling agent is at least one of polydimethylsiloxane and acrylate copolymer.

[0032] In addition, the present application also provides a method for preparing a heat-insulating polyurethane material, the preparation method comprising the following steps: Add the polyurethane prepolymer, composite filler and catalyst into the reactor, stir and treat at 65°C~75°C for 1h~2h, then add the antioxidant, stabilizer and leveling agent, continue stirring for 2h~3h to obtain the heat-insulating polyurethane material.

[0033] In the above scheme, by optimizing the raw materials for preparing the polyurethane material, the physical structure and chemical components of the material are coordinated with each other, thus achieving a significant heat insulation effect.

[0034] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0035] Example 1 A method for preparing a heat-insulating polyurethane material comprises the following steps: The diatomite was heat treated at 500°C for 2h, and then sodium stearate was added to the heat-treated diatomite at a material-liquid ratio of 3g / 10mL, and stirred at 65°C for 30min, and then hollow spherical silica was added at a mass ratio of 1:3 between diatomite and hollow spherical silica, and ultrasonically dispersed for 45min. After centrifugal treatment and washing treatment, the mixture was calcined at 120°C for 1h, and ball milled to obtain diatomite-loaded hollow spherical silica with an average particle size of 80nm; Under a nitrogen atmosphere, 30 parts of tetrahydrofuran were added to a reaction kettle, stirred at 80°C for 1 hour, cooled to room temperature, and then 50 parts of polyethylene glycol and 45 parts of 4,4-dimethyl diisocyanate were added, stirred at 60°C for 3 hours, and then 25 parts of neopentyl glycol were added, and the stirring reaction was continued at 70°C for 15 minutes to obtain a mixture; 10 parts of diatomaceous earth-loaded hollow spherical silica were added to the mixture, and stirred at 55°C for 45 minutes to obtain a polyurethane prepolymer; 5 parts of tin-doped titanium dioxide are added to 10 parts of 3-aminopropyltriethoxysilane, and the mixture is stirred at 65° C. for 45 minutes to obtain pretreated tin-doped titanium dioxide; 1 part of fullerene and 5 parts of graphene are added to 15 parts of isocyanate, and the mixture is stirred at 65° C. for 30 minutes to obtain a pretreated mixture of fullerene and graphene, and then the pretreated mixture and the pretreated tin-doped titanium dioxide are uniformly stirred, heated and dried to obtain a composite filler; 90 parts of polyurethane prepolymer, 20 parts of composite filler and 5 parts of dibutyltin dilaurate were added to a reactor, stirred at 65°C for 1 hour, and then 3 parts of antioxidant 1010, 3 parts of light stabilizer 292 and 5 parts of polydimethylsiloxane were added, and the stirring was continued for 2 hours to obtain a heat-insulating polyurethane material.

[0036] Example 2 A method for preparing a heat-insulating polyurethane material comprises the following steps: The diatomite was heat treated at 500°C for 2h, and then sodium stearate was added to the heat-treated diatomite at a material-liquid ratio of 3g / 10mL, and stirred at 70°C for 30min, and then hollow spherical silica was added at a mass ratio of 1:3 between diatomite and hollow spherical silica, and ultrasonically dispersed for 45min. After centrifugal treatment and washing treatment, the mixture was calcined at 115°C for 1h, and ball milled to obtain diatomite-loaded hollow spherical silica with an average particle size of 80nm; Under a nitrogen atmosphere, 32 parts of tetrahydrofuran were added to a reaction kettle, stirred at 85° C. for 2 hours, cooled to room temperature, and then 55 parts of polyethylene glycol and 43 parts of 4,4-dimethyl diisocyanate were added, stirred at 60° C. for 3 hours, and then 25 parts of neopentyl glycol were added, and the stirring reaction was continued at 80° C. for 15 minutes to obtain a mixture; 12 parts of diatomaceous earth-loaded hollow spherical silica were added to the mixture, and stirred at 55° C. for 45 minutes to obtain a polyurethane prepolymer; 6 parts of tin-doped titanium dioxide are added to 10 parts of 3-aminopropyltriethoxysilane, and the mixture is stirred at 65° C. for 50 minutes to obtain pretreated tin-doped titanium dioxide; 2 parts of fullerene and 4 parts of graphene are added to 15 parts of isocyanate, and the mixture is stirred at 65° C. for 35 minutes to obtain a pretreated mixture of fullerene and graphene, and then the pretreated mixture and the pretreated tin-doped titanium dioxide are uniformly stirred, heated and dried to obtain a composite filler; 95 parts of polyurethane prepolymer, 22 parts of composite filler and 7 parts of dibutyltin dilaurate were added to a reactor, stirred at 70°C for 1 hour, and then 3 parts of antioxidant 1010, 3 parts of light stabilizer 292 and 5 parts of polydimethylsiloxane were added, and the stirring was continued for 2 hours to obtain a heat-insulating polyurethane material.

[0037] Example 3 A method for preparing a heat-insulating polyurethane material comprises the following steps: The diatomite was heat treated at 500°C for 2h, and then sodium stearate was added to the heat-treated diatomite at a material-liquid ratio of 3g / 10mL, and stirred at 70°C for 30min, and then hollow spherical silica was added at a mass ratio of 1:3 between diatomite and hollow spherical silica, and ultrasonically dispersed for 45min. After centrifugal treatment and washing treatment, the mixture was calcined at 120°C for 1h, and ball milled to obtain diatomite-loaded hollow spherical silica with an average particle size of 80nm; Under a nitrogen atmosphere, 35 parts of tetrahydrofuran were added to a reaction kettle, stirred at 85° C. for 2 hours, cooled to room temperature, and then 52 parts of polyethylene glycol and 45 parts of 4,4-dimethyl diisocyanate were added, stirred at 65° C. for 4 hours, and then 30 parts of neopentyl glycol were added, and the stirring reaction was continued at 85° C. for 20 minutes to obtain a mixture; 15 parts of diatomaceous earth-loaded hollow spherical silica were added to the mixture, and stirred at 55° C. for 40 minutes to obtain a polyurethane prepolymer; 8 parts of tin-doped titanium dioxide are added to 10 parts of 3-aminopropyltriethoxysilane, and the mixture is stirred at 70° C. for 60 minutes to obtain pretreated tin-doped titanium dioxide; 3 parts of fullerene and 3 parts of graphene are added to 15 parts of isocyanate, and the mixture is stirred at 70° C. for 45 minutes to obtain a pretreated mixture of fullerene and graphene, and then the pretreated mixture and the pretreated tin-doped titanium dioxide are uniformly stirred, heated and dried to obtain a composite filler; 100 parts of polyurethane prepolymer, 25 parts of composite filler and 7 parts of dibutyltin dilaurate were added to a reactor, stirred at 75°C for 2 hours, and then 4 parts of antioxidant 1010, 3 parts of light stabilizer 292 and 5 parts of polydimethylsiloxane were added, and the stirring was continued for 2 hours to obtain a heat-insulating polyurethane material.

[0038] Comparative Example 1: The difference between Comparative Example 1 and Example 3 is that conventional silica is used in Comparative Example 1 to replace the diatomaceous earth-loaded hollow spherical silica in the present application, and the rest is the same as Example 3.

[0039] Comparative Example 2: The difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, hollow spherical silica is used to replace the diatomaceous earth-loaded hollow spherical silica of the present application, and the rest is the same as Example 3.

[0040] Comparative Example 3: The difference between Comparative Example 3 and Example 3 is that diatomaceous earth-loaded hollow spherical silica is not added in Comparative Example 3, and the rest is the same as Example 3.

[0041] Comparative Example 4: The difference between Comparative Example 4 and Example 3 is that no tin-doped titanium dioxide is added in Comparative Example 4, and the rest is the same as Example 3.

[0042] Comparative Example 5: The difference between Comparative Example 5 and Example 3 is that fullerene is not added in Comparative Example 5, and the rest is the same as Example 3.

[0043] Comparative Example 6: The difference between Comparative Example 6 and Example 3 is that graphene is not added in Comparative Example 6, and the rest is the same as Example 3.

[0044] Comparative Example 7: The difference between Comparative Example 7 and Example 3 is that no composite filler is added to the raw materials for preparing the polyurethane material in Comparative Example 7, and the rest is the same as Example 3.

[0045] Comparative Example 8: The difference between Comparative Example 8 and Example 3 is that the tin-doped titanium dioxide in Comparative Example 8 is not treated with 3-aminopropyltriethoxysilane, and the rest is the same as Example 3.

[0046] Comparative Example 9: The difference between Comparative Example 9 and Example 3 is that the fullerene and graphene in Comparative Example 9 are not treated with isocyanate, and the rest are the same as Example 3.

[0047] Comparative Example 10: The difference between Comparative Example 10 and Example 3 is that the composition ratio of the polyurethane material in Comparative Example 10 is different, and the rest is the same as Example 3.

[0048] The heat-insulating polyurethane material in Comparative Example 10 includes the following raw materials in parts by weight: 100 parts of polyurethane prepolymer, 2 parts of composite filler, 7 parts of dibutyltin dilaurate, 4 parts of antioxidant 1010, 3 parts of light stabilizer 292, and 5 parts of polydimethylsiloxane.

[0049] Comparative Example 11: The difference between Comparative Example 11 and Example 3 is that the composition ratio of the polyurethane material in Comparative Example 11 is different, and the rest is the same as Example 3.

[0050] The heat-insulating polyurethane material in Comparative Example 11 includes the following raw materials in parts by weight: 100 parts of polyurethane prepolymer, 30 parts of composite filler, 7 parts of dibutyltin dilaurate, 4 parts of antioxidant 1010, 3 parts of light stabilizer 292, and 5 parts of polydimethylsiloxane.

[0051] The polyurethane material samples prepared in Examples 1 to 3 and the polyurethane material comparative samples prepared in Comparative Examples 1 to 11 were subjected to performance tests, and the results are shown in Table 1. The thermal conductivity refers to GB / 3399-1982, the freeze-thaw cycle refers to ASTMC666, the compressive strength refers to GB / T8813-1988, and the tensile strength refers to GB / T9641-1988.

[0052] Table 1: Performance test results

[0053] From the data analysis of Table 1, it can be seen that the polyurethane material samples prepared in the present application have low thermal conductivity, excellent thermal insulation effect, and stable thermal insulation performance after 300 freeze-thaw cycles. This shows that after the optimization of the components and the ratio of the components, the interaction between the components can not only play a significant thermal insulation effect, but also help improve the mechanical properties and increase its application value.

[0054] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0055] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A heat-insulating polyurethane material, characterized in that: The heat-insulating polyurethane material comprises the following raw materials in parts by weight: 50 to 100 parts of polyurethane prepolymer, 15 to 25 parts of composite filler, 1 to 7 parts of catalyst, 1 to 15 parts of antioxidant, 1 to 3 parts of stabilizer and 1 to 10 parts of leveling agent; The polyurethane prepolymer comprises the following raw materials in parts by weight: 25 to 40 parts of tetrahydrofuran, 15 to 50 parts of 4,4-dimethyl diisocyanate, 50 to 55 parts of polyethylene glycol, 25 to 40 parts of neopentyl glycol, and 9 to 15 parts of diatomaceous earth-loaded hollow spherical silica; The composite filler comprises the following raw materials in parts by weight: 5 to 10 parts of tin-doped titanium dioxide, 1 to 3 parts of fullerene, 1 to 5 parts of graphene and 25 to 30 parts of a treating agent.

2. The heat insulating polyurethane material according to claim 1, characterized in that: The preparation method of the polyurethane prepolymer comprises the following steps: adding tetrahydrofuran to a reaction kettle under a nitrogen atmosphere, stirring for 1h to 3h at 80°C to 90°C, cooling to room temperature, adding polyethylene glycol and 4,4-dimethyl diisocyanate, stirring for reaction for 3h to 5h at 55°C to 65°C, adding neopentyl glycol, continuing to stir for reaction for 15min to 30min at 70°C to 85°C, and obtaining a mixture; and adding diatomaceous earth-loaded hollow spherical silica to the mixture, stirring for 30min to 45min at 45°C to 55°C, and obtaining a polyurethane prepolymer.

3. The heat insulating polyurethane material according to claim 2, characterized in that: The preparation method of the diatomite-loaded hollow spherical silica comprises the following steps: adding a surfactant to the heat-treated diatomite, stirring at 65° C. to 80° C. for 20 min to 30 min, then adding the hollow spherical silica, ultrasonically dispersing for 30 min to 45 min, centrifuging and washing, calcining at 110° C. to 120° C. for 1 h to 2 h, and ball milling to obtain the diatomite-loaded hollow spherical silica.

4. The heat insulating polyurethane material according to claim 3, characterized in that: The surfactant is one of sodium stearate and hexamethylenetetramine or a mixture of the two.

5. The heat insulating polyurethane material according to claim 4, characterized in that: The average particle size of the diatomaceous earth-loaded hollow spherical silica is 60nm-120nm.

6. The heat insulating polyurethane material according to claim 1, characterized in that: The treating agent is 3-aminopropyltriethoxysilane and isocyanate.

7. The heat insulating polyurethane material according to claim 6, characterized in that: The preparation method of the composite filler comprises the following steps: adding tin-doped titanium dioxide to 3-aminopropyltriethoxysilane, stirring the mixture at 45°C to 70°C for 45min to 60min to obtain pretreated tin-doped titanium dioxide; adding fullerene and graphene to isocyanate, stirring the mixture at 65°C to 90°C for 30min to 45min to obtain a pretreated mixture of fullerene and graphene, and then uniformly stirring the pretreated mixture and the pretreated tin-doped titanium dioxide, heating and drying the mixture, and ball milling the mixture to obtain the composite filler.

8. The heat insulating polyurethane material according to claim 1, characterized in that: The antioxidant is at least one of the antioxidant 1010 and the antioxidant 1076 .

9. The heat insulating polyurethane material according to claim 1, characterized in that: The stabilizer is at least one of light stabilizer 292 and UV123.

10. A method for preparing a heat-insulating polyurethane material, characterized in that: The preparation method is used to prepare the heat-insulating polyurethane material according to any one of claims 1 to 9, and the preparation method comprises the following steps: Add the polyurethane prepolymer, composite filler and catalyst into the reactor, stir and treat at 65°C~75°C for 1h~2h, then add the antioxidant, stabilizer and leveling agent, continue stirring for 2h~3h to obtain the heat-insulating polyurethane material.

Citation Information

Patent Citations

  • Preparation method of thermal insulation material for marine oil gas transportation pipeline

    CN103772635A

  • Polyurethane hard foam thermal-insulation material

    CN105542104A

  • Diatomite loaded nitrogen doped titanium dioxide / silicon dioxide photocatalytic coating

    CN108250808A

  • Polyurethane thermal insulation material and preparation method thereof

    CN115322323A

Cited By

  • Preparation method of hydrolysis-resistant polyimide film and hydrolysis-resistant polyimide film