A low-temperature acidification corrosion inhibitor for petroleum and preparation method thereof
The existing technology is solved by using the corrosion inhibitor reaction of linolenic acid, hydroxyethylenediamine and dichlorhexane in the low-temperature acidification corrosion inhibitor, and combining potassium chromate, sodium silicate and potassium iodide to form an oxide film. The problems of poor compatibility and poor corrosion inhibitors in medium and low temperature acidification corrosion inhibitors have significantly improved the corrosion inhibition effect and stability.
Patent Information
- Application Number
- CN202411253899.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-09
AI Technical Summary
When used in oil fields, there are problems such as poor compatibility, poor corrosion inhibition effect and poor stability. In particular, the use of alcohol as a solvent leads to high cost and poor compatibility with acid liquid, and the resistance of the membrane layer. Inadequate flushing ability.
The corrosion inhibiting main agent prepared by reaction of linolenic acid, hydroxyethylenediamine and dichlorohexane is formed by forming a chemical adsorption film and combining it with the metal surface, and combining the auxiliary agents potassium chromate, sodium silicate and potassium iodide to form an insoluble oxide film, and Add thiol acetic acid to the low-temperature acidification corrosion inhibitor to reduce Fe3+ content and improve the corrosion inhibition effect.
It realizes effective protection of metal surfaces under low-temperature acidification environment, improves the compatibility and stability of corrosion inhibitors, enhances the erosion resistance of the film layer, and significantly improves the corrosion inhibition effect and storage stability.
Smart Images

Figure CN118755462B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oil and gas field exploitation and corrosion prevention, and in particular relates to a low-temperature acidification corrosion inhibitor for petroleum and a preparation method thereof. Background Art
[0002] Acidizing is an important means to improve the productivity of oil and gas wells, and will continue to be used on a large scale in the development of deep and ultra-deep oil and gas reservoirs. However, acid has a corrosive effect on surface equipment, downhole pipe strings, etc., so it is necessary to use corrosion inhibitors in acid to reduce or eliminate corrosion.
[0003] The commonly used corrosion inhibitors on the market, whether they are high-temperature series corrosion inhibitors or medium-temperature series corrosion inhibitors, mostly use alcohol as a solvent to prepare the corrosion inhibitor. However, the corrosion inhibitor configured with alcohol as a solvent has poor compatibility with the acid system, and the cost of the corrosion inhibitor increases accordingly, so it is necessary to develop a water-soluble corrosion inhibitor. For example, the Chinese patent application document with publication number CN113278409A discloses a high-temperature acidification corrosion inhibitor, which includes components of a corrosion inhibitor main agent, an auxiliary agent A and an auxiliary agent B; the mass ratio of the corrosion inhibitor main agent, auxiliary agent A and auxiliary agent B is 10:3:1; the corrosion inhibitor main agent, auxiliary agent A and auxiliary agent B are mixed to form a corrosion inhibitor, and ethanol is used to dissolve it into a corrosion inhibitor solution. This kind of corrosion inhibitor has the advantages of good solubility, more adsorption sites, high corrosion inhibition efficiency, and low toxicity in a high-temperature acidification environment, but it uses ethanol as the solvent of the corrosion inhibitor, has poor compatibility with acidic liquids, and has a high cost.
[0004] The presence of heteroatoms such as N, O, S, and P in organic compounds causes the corrosion inhibitor molecules to form a film and adsorb on the metal surface, separating the metal surface from the corrosive medium, thereby effectively reducing the erosion of the metal surface by corrosive substances. Currently used low-temperature (greater than 60°C and less than 90°C) acidification corrosion inhibitors are usually nitrogen-containing compounds, sulfur-containing compounds, acetylenic compounds, aldehydes, ketones, lipophilic compounds, surfactants, etc., but some corrosion inhibitors will form flocculent precipitation in acid solution, and the film layer formed by some corrosion inhibitors on the pipe string has weak erosion resistance and poor corrosion inhibition effect on the pipe string. These shortcomings limit the large-scale use and promotion of these low-temperature corrosion inhibitors in oil fields. A Chinese patent application document with publication number CN102031526A discloses a low-temperature acidification corrosion inhibitor, which is composed of 10-50 parts by weight of acetylenic alcohol, 10-50 parts by weight of quaternary ammonium salt and 5-10 parts by weight of heterocyclic compound. This low-temperature acidification corrosion inhibitor has good compatibility with the acid solution system and will not generate flocculent precipitation, but the film layer formed on the pipe string has weak erosion resistance and the corrosion inhibition effect needs to be improved. Summary of the invention
[0005] In order to solve the technical problems of poor compatibility, poor corrosion inhibition effect, poor stability and the like existing in the related art, the object of the present invention is to provide a low-temperature acidizing corrosion inhibitor for petroleum and a preparation method thereof.
[0006] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:
[0007] A low-temperature acidification corrosion inhibitor for petroleum, comprising the following components and their weight proportions:
[0008] 35-40 parts of main corrosion inhibitor, 10-15 parts of auxiliary agent, 5-10 parts of acetylene alcohol, 15-19 parts of emulsifier, 4-8 parts of thioglycolic acid and 50-60 parts of water; the main corrosion inhibitor is prepared by reacting linolenic acid, hydroxyethylenediamine and dichlorohexane.
[0009] The corrosion inhibitor used in the present invention is prepared by the reaction of linolenic acid, hydroxyethylenediamine and dichlorohexane. Nitrogen and oxygen in the molecular structure can combine with the empty d orbitals of iron atoms on the metal surface to form coordination bonds, thereby being adsorbed on the metal surface to form a protective film to prevent corrosion of the metal. The molecular structure has multiple adsorption centers, which strengthens the binding ability of the formed protective film and improves the erosion resistance. The alkyl hydrophobic long chain at the other end of the molecular structure can form a hydrophobic layer to prevent water molecules from entering the adsorption film layer, thereby inhibiting corrosion.
[0010] Fe in the acid 3+ The performance of the corrosion inhibitor will be reduced. In the present invention, thioglycolic acid is added as a reducing agent in the formula of the low-temperature acidification corrosion inhibitor, which effectively reduces the Fe 3+ content to ensure the corrosion inhibition effect of low-temperature acidizing corrosion inhibitor.
[0011] Furthermore, the preparation method of the main corrosion inhibitor is as follows: linolenic acid and hydroxyethylenediamine are added to a reactor, xylene is added, the temperature is raised for reaction, after the reaction is completed, the temperature is lowered and the unreacted raw materials and xylene are removed by vacuum distillation, and the reaction is cooled; dichlorohexane and anhydrous ethanol are continuously added, the reaction is refluxed, after the reaction is completed, the ethanol is removed by vacuum distillation, and acetone is added for recrystallization to obtain the main corrosion inhibitor.
[0012] Furthermore, in the preparation method of the main corrosion inhibitor, the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane is 1-3:2-3.4:1-1.8.
[0013] Furthermore, in the preparation method of the main corrosion inhibitor, the amount of xylene used is 3-5 times the mass of linolenic acid; the amount of anhydrous ethanol used is 4-7 times the mass of dichlorohexane.
[0014] Furthermore, the temperature increase reaction in the preparation method of the corrosion inhibitor is divided into two stages. The first stage is heated to 150-155°C, and the reaction time is 4-4.2h. The second stage is heated to 220-230°C, and the reaction time is 4-4.5h. The temperature of the cooling and reduced pressure distillation is 110-120°C, and the cooling temperature is 80-90°C; the reflux reaction time is 4-4.5h.
[0015] Furthermore, the auxiliary agent is composed of potassium chromate, sodium silicate and potassium iodide in a mass ratio of 7-10:5-7:1-2.
[0016] In the present invention, potassium chromate, sodium silicate and potassium iodide are used to form auxiliary agents, wherein potassium chromate and sodium silicate can form complexes with metal ions in acid solution to form insoluble oxide films on the metal surface, and the addition of potassium iodide can effectively improve the corrosion inhibition efficiency of the low-temperature acidification corrosion inhibitor. The inventor found in the research process that the mass ratio of each component in the auxiliary agent has a great influence on the corrosion inhibition efficiency of the low-temperature acidification corrosion inhibitor, especially the amount of potassium iodide. When it exceeds the ratio range specified in the present invention, the corrosion inhibition effect of the low-temperature acidification corrosion inhibitor will deteriorate. This is because too much potassium iodide will reduce the adsorption tendency of the low-temperature acidification corrosion inhibitor on the metal surface, thereby causing the corrosion inhibition effect to deteriorate.
[0017] Furthermore, the alkynol is at least one of acetylene alcohol, octynol, methylbutynol, 3,6-dimethyl-4-octyne-3,6-diol or 2,5-dimethyl-3-hexyne-2,5-diol.
[0018] Furthermore, the emulsifier is one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate and sodium sarcosinate.
[0019] The present invention also provides a method for preparing the low-temperature acidification corrosion inhibitor for petroleum, comprising the following steps:
[0020] S1: Mix the emulsifier and water evenly, add the main corrosion inhibitor after heating, stir until dissolved, and cool to room temperature to obtain a mixture I;
[0021] S2: adding the auxiliary agent, acetylenic alcohol and thioglycolic acid to the mixture I obtained in step S1, heating and stirring, cooling to room temperature, and obtaining a low-temperature acidification corrosion inhibitor for petroleum.
[0022] Furthermore, the heating temperature in step S1 is 50-60° C.; the heating temperature in step S2 is 80-90° C., and the stirring time is 0.5-1 h.
[0023] Compared with the prior art, the low-temperature acidification corrosion inhibitor for petroleum and the preparation method thereof provided by the present invention have the following technical advantages:
[0024] (1) In the present invention, linolenic acid, hydroxyethylenediamine and dichlorohexane are reacted to form a corrosion inhibitor main agent, which forms a corrosion inhibition film on the metal surface through chemical adsorption to prevent the metal from being corroded;
[0025] (2) The present invention uses potassium chromate, sodium silicate and potassium iodide as auxiliary agents to form an insoluble oxide film on the metal surface through physical adsorption, thereby further protecting the metal;
[0026] (3) The low-temperature acidification corrosion inhibitor for petroleum provided in the present invention has good storage stability in acid solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a reaction flow chart of the main corrosion inhibitor of the present invention.
[0028] In the figure, R is -(CH2)7(CHCHCH2)3CH3, and RCOOH is linolenic acid. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. Those skilled in the art can make various modifications based on the basic idea of the present invention, but as long as they do not deviate from the basic idea of the present invention, they are all within the scope of the present invention.
[0030] The reaction flow chart of the low temperature acidizing corrosion inhibitor for petroleum in this specific embodiment is as follows: Figure 1 shown.
[0031] Example 1
[0032] A low-temperature acidification corrosion inhibitor for petroleum, comprising the following components and their weight proportions:
[0033] 35 parts of a main corrosion inhibitor, 10 parts of an auxiliary agent, 5 parts of 3,6-dimethyl-4-octyne-3,6-diol, 15 parts of sodium dodecyl sulfonate, 4 parts of thioglycolic acid, and 60 parts of water; the preparation method of the main corrosion inhibitor is: adding linolenic acid and hydroxyethylenediamine into a reactor, adding xylene, heating to 150°C, reacting for 4.2 hours, continuing to heat to 220°C, reacting for 4.5 hours, cooling to 110°C after the reaction, removing unreacted raw materials and xylene by vacuum distillation, and cooling to 80°C; continuing to add dichlorohexane and anhydrous ethanol, reflux reaction at 80°C for 4.5 hours, removing ethanol by vacuum distillation after the reaction, adding acetone for recrystallization, and obtaining the main corrosion inhibitor; the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane is 1:2:1, the amount of xylene is 3 times the mass of linolenic acid; the amount of anhydrous ethanol is 4 times the mass of dichlorohexane.
[0034] The auxiliary agent is composed of potassium chromate, sodium silicate and potassium iodide in a mass ratio of 7:5:1.
[0035] The preparation method of the low-temperature acidification corrosion inhibitor for petroleum comprises the following steps:
[0036] S1: Mix the emulsifier and water evenly, heat to 50°C, add the main corrosion inhibitor, stir until dissolved, and cool to room temperature to obtain mixture I;
[0037] S2: Add the auxiliary agent, acetylenic alcohol and thioglycolic acid to the mixture I prepared in step S1, heat to 80° C. and stir for 0.5 h, cool to room temperature, and obtain a low-temperature acidification corrosion inhibitor for petroleum.
[0038] Example 2
[0039] A low-temperature acidification corrosion inhibitor for petroleum, comprising the following components and their weight proportions:
[0040] 40 parts of a main corrosion inhibitor, 15 parts of an auxiliary agent, 10 parts of octynol, 19 parts of sodium sarcosinate, 8 parts of thioglycolic acid and 50 parts of water; the preparation method of the main corrosion inhibitor is as follows: linolenic acid and hydroxyethylenediamine are added into a reactor, xylene is added, the temperature is raised to 155°C, the reaction time is 4 hours, the temperature is further raised to 230°C, the reaction time is 4 hours, the temperature is lowered to 120°C after the reaction is completed, unreacted raw materials and xylene are removed by vacuum distillation, and the reaction is cooled to 90°C; dichlorohexane and anhydrous ethanol are continuously added, the reaction is refluxed at 90°C for 4 hours, the ethanol is removed by vacuum distillation after the reaction is completed, acetone is added for recrystallization to obtain the main corrosion inhibitor; the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane is 3:3.4:1.8; the amount of xylene is 5 times the mass of linolenic acid; the amount of anhydrous ethanol is 7 times the mass of dichlorohexane.
[0041] The auxiliary agent is composed of potassium chromate, sodium silicate and potassium iodide in a mass ratio of 10:7:2.
[0042] The preparation method of the low-temperature acidification corrosion inhibitor for petroleum comprises the following steps:
[0043] S1: Mix the emulsifier and water evenly, heat to 60°C, add the main corrosion inhibitor, stir until dissolved, and cool to room temperature to obtain mixture I;
[0044] S2: Add the auxiliary agent, acetylenic alcohol and thioglycolic acid to the mixture I prepared in step S1, heat to 90° C. and stir for 1 hour, cool to room temperature, and obtain a low-temperature acidification corrosion inhibitor for petroleum.
[0045] Example 3
[0046] A low-temperature acidification corrosion inhibitor for petroleum, comprising the following components and their weight proportions:
[0047] 38 parts of a main corrosion inhibitor, 13 parts of an auxiliary agent, 7 parts of 2,5-dimethyl-3-hexyne-2,5-diol, 17 parts of sodium dodecylbenzenesulfonate, 6 parts of thioglycolic acid, and 57 parts of water; the preparation method of the main corrosion inhibitor is: adding linolenic acid and hydroxyethylenediamine into a reactor, adding xylene, heating to 153°C, reacting for 4.1 hours, continuing to heat to 225°C, reacting for 4.3 hours, cooling to 117°C after the reaction, removing unreacted raw materials and xylene by vacuum distillation, and cooling to 85°C; continuing to add dichlorohexane and anhydrous ethanol, reflux reaction at 85°C for 4.2 hours, removing ethanol by vacuum distillation after the reaction, adding acetone for recrystallization, and obtaining a main corrosion inhibitor; the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane is 2:3:1.5; the amount of xylene is 4 times the mass of linolenic acid; the amount of anhydrous ethanol is 5 times the mass of dichlorohexane.
[0048] The auxiliary agent is composed of potassium chromate, sodium silicate and potassium iodide in a mass ratio of 8:6:1.
[0049] The preparation method of the low-temperature acidification corrosion inhibitor for petroleum comprises the following steps:
[0050] S1: Mix the emulsifier and water evenly, heat to 55°C, add the main corrosion inhibitor, stir until dissolved, and cool to room temperature to obtain mixture I;
[0051] S2: Add the auxiliary agent, acetylenic alcohol and thioglycolic acid to the mixture I prepared in step S1, heat to 85° C. and stir for 0.7 h, cool to room temperature, and obtain a low-temperature acidification corrosion inhibitor for petroleum.
[0052] Comparative Example 1
[0053] The corrosion inhibitor described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that an equal amount of oleic acid is used instead of linolenic acid in the preparation method of the main corrosion inhibitor in this comparative example.
[0054] Comparative Example 2
[0055] The corrosion inhibitor described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that an equal amount of hydroxyethylethylenediamine is used instead of hydroxyethylenediamine in the preparation method of the main corrosion inhibitor in this comparative example.
[0056] Comparative Example 3
[0057] The corrosion inhibitor described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that in the preparation method of the main corrosion inhibitor in this comparative example, the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane is 1:1:5.
[0058] Comparative Example 4
[0059] The corrosion inhibitor described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that an equal amount of potassium chromate is used in the auxiliary agent of this comparative example instead of potassium iodide.
[0060] Comparative Example 5
[0061] The corrosion inhibitor described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that the auxiliary agent in this comparative example is composed of potassium chromate, sodium silicate and potassium iodide in a mass ratio of 3:2:5.
[0062] Comparative Example 6
[0063] The corrosion inhibitor described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that an equal amount of sodium sulfite is used instead of thioglycolic acid in this comparative example.
[0064] Test example
[0065] Corrosion inhibition performance test: According to the static corrosion rate determination conditions and corrosion inhibitor evaluation indicators at normal pressure in SY / T 5405-2019 "Test Method and Evaluation Standard for Performance of Corrosion Inhibitors for Acidification", the corrosion inhibition performance of the corrosion inhibitors prepared in Examples 1-3 and Comparative Examples 1-6 was tested by the static hanging weight loss method, and the corrosion inhibition rate of each group of steel sheets was recorded. The test results are shown in Tables 1-1 and 1-2. The specific method is as follows: select a standard X65 steel sheet as the test object, with a specification of 50mm×10mm×3mm, first soak the steel sheet in petroleum ether for 8 minutes to remove low-polarity grease, take out the steel sheet and soak it in anhydrous ethanol and acetone for 5 minutes respectively, dry it with cold air, wrap it with filter paper, and place it in a vacuum drying oven to dry for 20 minutes, weigh it (the mass is accurate to 0.0001g), dissolve the acidified corrosion inhibitor in a 20% mass fraction hydrochloric acid solution, and measure the mass fraction of the acidified corrosion inhibitor to be 0 (blank group), 0. The corrosion inhibition rate of X65 steel sheet in acid solution with a certain concentration of 0.04wt% (40ppm), 0.06wt% (60ppm), and 0.08wt% (80ppm) was calculated. The test temperature was 60°C and the measurement time was 4h. After the test, the steel sheet was taken out, and the impurities such as HCl on the surface of the steel sheet were dissolved with water, and then immersed in anhydrous ethanol and acetone for 5min respectively, and finally dried in a vacuum drying oven for 20min, and then taken out and weighed (the mass was accurate to 0.0001g), and then the corrosion inhibition rate of X65 steel sheet in acid solution with a certain concentration was calculated. Corrosion inhibition rate = (△m0-△m1) / △m0×100%, where △m0 is the mass loss of the blank group steel sheet (g), and △m1 is the mass loss of the steel sheet after adding the acidified corrosion inhibitor (g).
[0066] Stability test: The low-temperature acidification corrosion inhibitor for petroleum prepared in Example 1 to Example 3 was stored in a hydrochloric acid solution with a mass percentage of 25% for 24 hours, and the storage stability test was performed at 60°C, 90°C, 100°C, and 120°C, respectively. The amount of the low-temperature acidification corrosion inhibitor for petroleum was 1%, 2%, and 3% by mass percentage, respectively, and whether stratification, flocculation, and precipitation occurred in the system was observed. The test results are shown in Table 2.
[0067] Table 1-1 Corrosion inhibition performance test results of Example 1 to Example 3
[0068]
[0069] Table 1-2 Corrosion inhibition performance test results of Example 3, Comparative Examples 1 to 6
[0070]
[0071] It can be seen from Table 1-1 that the corrosion inhibition rate of the low-temperature acidizing corrosion inhibitor for petroleum provided by the present invention is 85.56-93.41% when the mass percentage is 0.04%, the corrosion inhibition rate is 90.28-97.46% when the mass percentage is 0.06%, and the corrosion inhibition rate is 94.15-99.12% when the mass percentage is 0.08%, which fully demonstrates that the low-temperature acidizing corrosion inhibitor for petroleum provided by the present invention has a good corrosion inhibition effect.
[0072] As shown in Table 1-2, compared with Example 3, in Comparative Example 1, an equal amount of oleic acid is used instead of linolenic acid, and in Comparative Example 2, an equal amount of hydroxyethylethylenediamine is used instead of hydroxyethylenediamine, but the corrosion inhibition rate is significantly reduced, which shows that the reaction of linolenic acid and hydroxyethylenediamine in the present invention is irreplaceable; in Comparative Example 3, the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane is changed, but the corrosion inhibition rate is reduced, which shows that the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane in the present invention has been optimized; in Comparative Example 4, the auxiliary agent In Example 1, an equal amount of potassium chromate is used instead of potassium iodide, but the corrosion inhibition rate is reduced, which shows that the addition of potassium iodide can improve the corrosion inhibition efficiency of the corrosion inhibitor; in Comparative Example 5, the dosage ratio of each component of the auxiliary agent is changed, but the corrosion inhibition rate is significantly reduced, which shows that too much potassium iodide will affect the adsorption trend of the corrosion inhibitor on the metal surface, resulting in a worse slow-release effect of the corrosion inhibitor; in Comparative Example 6, an equal amount of sodium sulfite is used instead of thioglycolic acid, but the corrosion inhibition rate is reduced, which shows that not all reducing agents can achieve the effect of thioglycolic acid.
[0073] Table 2 Stability performance test results
[0074]
[0075] As can be seen from Table 2, the low-temperature acidizing corrosion inhibitor for petroleum prepared in Examples 1 to 3 of the present invention is stored in acid solution at 60°C, 90°C, 100°C, and 120°C for 24 hours, and has good stability when the addition amount is 1-3%, and no stratification, flocculation, or precipitation occurs, which indicates that the low-temperature acidizing corrosion inhibitor for petroleum provided by the present invention has good storage stability and compatibility.
[0076] The above embodiments are only preferred embodiments of the present invention, and are not intended to limit the present invention. Any person skilled in the art shall not modify the above embodiments without violating the spirit and scope of the present invention. Therefore, any modification, equivalent substitution and improvement made by those skilled in the art under the technical concept of the present invention shall still be covered by the claims of the present invention.
Claims
1. A low-temperature acidification corrosion inhibitor for petroleum, characterized in that: It includes the following components and their weight parts: 35-40 parts of main corrosion inhibitor, 10-15 parts of auxiliary agent, 5-10 parts of acetylene alcohol, 15-19 parts of emulsifier, 4-8 parts of thioglycolic acid, 50-60 parts of water; the main corrosion inhibitor is prepared by the reaction of linolenic acid, hydroxyethylenediamine and dichlorohexane; the auxiliary agent is composed of potassium chromate, sodium silicate and potassium iodide in a mass ratio of 7-10:5-7:1-2; The preparation method of the main corrosion inhibitor is as follows: adding linolenic acid and hydroxyethylenediamine into a reactor, adding xylene, heating for reaction, cooling and distilling to remove unreacted raw materials and xylene after the reaction, and cooling; continuing to add dichlorohexane and anhydrous ethanol, reflux reaction, distilling to remove ethanol after the reaction, adding acetone for recrystallization, and obtaining the main corrosion inhibitor; the molar ratio of linolenic acid, hydroxyethylenediamine and dichlorohexane is 1-3:2-3.4:1-1.8; the heating reaction is divided into two stages, the first stage is heated to 150-155°C, the reaction time is 4-4.2h, and the second stage is heated to 220-230°C, the reaction time is 4-4.5h; the temperature of the cooling and distilling is 110-120°C, and the cooling temperature is 80-90°C; the reflux reaction time is 4-4.5h.
2. The low-temperature acidification corrosion inhibitor for petroleum according to claim 1, characterized in that: The amount of xylene used is 3-5 times the mass of linolenic acid, and the amount of anhydrous ethanol used is 4-7 times the mass of dichlorohexane.
3. The low-temperature acidification corrosion inhibitor for petroleum according to claim 1, characterized in that: The alkynol is at least one of acetylene alcohol, octynol, methylbutynol, 3,6-dimethyl-4-octyne-3,6-diol or 2,5-dimethyl-3-hexyne-2,5-diol.
4. The low-temperature acidification corrosion inhibitor for petroleum according to claim 1, characterized in that: The emulsifier is one of sodium dodecyl sulfonate and sodium dodecylbenzene sulfonate.
5. The method for preparing a low-temperature acidizing corrosion inhibitor for petroleum according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: Mix the emulsifier and water evenly, add the main corrosion inhibitor after heating, stir until dissolved, and cool to room temperature to obtain a mixture I; S2: adding the auxiliary agent, acetylenic alcohol and thioglycolic acid to the mixture I obtained in step S1, heating and stirring, cooling to room temperature, and obtaining a low-temperature acidification corrosion inhibitor for petroleum.
6. The method for preparing a low-temperature acidification corrosion inhibitor for petroleum according to claim 5, characterized in that: The heating temperature in step S1 is 50-60° C.; the heating temperature in step S2 is 80-90° C., and the stirring time is 0.5-1 h.
Citation Information
Cited By
A high-temperature resistant aniline-based organosilicon Mannich base quaternary ammonium salt corrosion inhibitor and its preparation method