Internal high-pressure forming reducer pipe springback control method based on axial compression deformation
By using axial compression deformation technology during the internal high-pressure forming process, the stress difference in the thickness direction of the reducer is uniformized, solving the springback and accuracy problems in traditional reducer manufacturing, and achieving efficient dimensional control and improved material stability. .
Patent Information
- Application Number
- CN202411256101.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-10-15
AI Technical Summary
The traditional reducing pipe manufacturing method has problems such as welding thermal deformation, large diameter, poor shape accuracy, long process and poor mechanical properties of the weld. In addition, during the internal high pressure forming process, pipe fittings are prone to excessive wall thickness thinning or instability and rupture, resulting in springback. The dimensional accuracy is poor, and the traditional mold compensation method is costly and has a long cycle.
An internal high-pressure forming method based on axial compression deformation is adopted. By arranging axially movable inserts in the transition area of the final forming mold, axial pressure is applied to the reducer tube to cause axial compression deformation in the beneficial wrinkle flattening area. , to homogenize the stress difference through thickness to control springback.
It significantly reduces the springback of the reducer, improves the dimensional accuracy, avoids the high cost and long cycle of the traditional compensation method, and enhances the applicability of the material and the service performance of the parts.
Smart Images

Figure CN118768451A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a forming and manufacturing method of a high-precision metal pipe fitting, and more specifically, to a springback control method of an internal high-pressure forming reducer pipe based on axial compression deformation, belonging to the technical field of pipe forming. Background Art
[0002] As a typical representative of hollow components, reducers are widely needed in the aerospace and automotive fields. They are mainly used in the exhaust systems, hydraulic systems, environmental control pipeline systems and load-bearing structural parts of automobiles, rockets or aircraft. For such parts, the traditional manufacturing method is generally to stamp out several sheets and then weld them into a whole. There are shortcomings such as large welding thermal deformation, poor shape accuracy, long process and poor mechanical properties of the weld.
[0003] In recent years, in order to eliminate the shortcomings of punching and welding of reducer tubes, internal high pressure forming technology has been used to form such parts. However, for light alloys such as aluminum alloys and magnesium alloys, due to their poor room temperature forming performance, the reducer tube is very likely to have excessive wall thickness thinning or even instability and rupture during the internal high pressure forming process dominated by "expansion deformation". For this reason, domestic and foreign scholars have proposed a variety of improvement methods based on internal high pressure forming, among which the beneficial wrinkle fully exerts the "material aggregation" effect of wrinkles, effectively reduces the thinning rate, improves the forming limit of the tube, and broadens the forming range of internal high pressure forming. However, the flattening of the beneficial wrinkle in the shaping stage is a reverse bending deformation process. When the liquid pressure in the pipe is unloaded, a certain amount of rebound will inevitably occur, which will affect the final dimensional accuracy of the reducer tube, resulting in poor dimensional accuracy, large dispersion, and even exceeding the design requirements and producing scrap. The traditional mold compensation method requires repeated mold repair, which is costly and has a long cycle. Therefore, how to effectively control the rebound of the reducer tube during the beneficial wrinkle internal high pressure forming process has been a problem that has been troubling those skilled in the art. Summary of the invention
[0004] To solve the above problems, the purpose of the present invention is to provide a convenient and effective method for controlling the springback of a high pressure forming reducer. The present invention uses axial compression deformation to homogenize or reduce the stress difference in the thickness direction of the reducer, thereby eliminating or reducing the springback.
[0005] In order to achieve the above-mentioned invention object, it is specifically completed according to the following technical scheme: A springback control method for an internal high-pressure forming reducer tube based on axial compression deformation comprises placing a tube blank into a forming die to preform a preformed tube, and placing the preformed tube into a final forming die to form a formed tube. The method is characterized in that an insert with axial movement that meets the design requirements is arranged in a transition area of the final forming die, and an axial pressure is applied to the reducer tube to cause axial compression deformation in a beneficial wrinkle flattening area, thereby changing the stress state and distribution of the tube blank in the thickness direction in the area, so as to eliminate or reduce the stress difference in the thickness direction, thereby achieving the effect of controlling springback.
[0006] In the above-mentioned method for controlling the springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation, the forming tube is completed according to the following steps: Step 1: Select a round-section tube blank, form a preformed reducer part through beneficial wrinkles, and unload the inner pressure. After unloading, the flattened area of the beneficial wrinkles will rebound, and the size will be smaller than the design value; Step 2: Place the preformed reducer part into the final forming die, seal the two ends of the preformed reducer part with the left sealing punch and the right sealing punch respectively, and then fill the interior of the preformed reducer part with a fluid medium; Step 3: Adjust the internal pressure of the preformed reducer part to the set value P, and under the support of the internal fluid medium, the wrinkles will rebound and re-fit the mold cavity (rebound again after pressure relief). The internal pressure value is 5 p s ≤P≤20 p s , p s It is the initial yield pressure of the tube blank, which is used to ensure that the preformed reducer parts can be smoothly axially compressed in the next step without compression instability and wrinkling.
[0007] Furthermore, after step three, step four is added; the left sealing punch and the right sealing punch are axially fed at the same time, pushing the left movable insert and the right movable insert to axially compress the beneficial wrinkle flattening area of the reducer and cause it to undergo plastic deformation. When the axial compression reaches a set value, the left sealing punch and the right sealing punch stop feeding. During the compression process, the preformed reducer part is pressed against the final forming cavity under the support of the internal pressure; the axial compression is 0.1%-10% of the length of the beneficial wrinkle flattening area; the compression deformation changes the stress state and distribution of the beneficial wrinkle flattening area, realizes the uniformization of the compressive stress, eliminates or reduces the thickness stress difference, and significantly reduces the rebound caused by the reverse bending deformation of the beneficial wrinkles. After unloading the internal pressure, a reducer that meets the dimensional accuracy requirements can be obtained.
[0008] In the above scheme, in step 1, the tube blank includes but is not limited to low carbon steel, high strength steel, aluminum alloy, magnesium alloy tube; The mold comprises an upper mold, a lower mold, a left movable insert, a right movable insert, a left sealing punch and a right sealing punch.
[0009] Further, in step three, 5 p s ≤P≤20 p s , p s is the initial yield pressure of the tube blank; in step 4, the amount of compression is 0.1%-10% of the length of the beneficial wrinkle flattening area.
[0010] Furthermore, the fluid medium is liquid or gas.
[0011] Compared with the prior art, the present invention has achieved the following beneficial technical effects: The springback control method for internal high-pressure forming reducer tube based on axial compression deformation provided by the present invention first realizes compressive stress homogenization through axial compression deformation, which can eliminate the difference in internal pressure and external tensile stress of beneficial wrinkle reverse bending deformation and significantly reduce springback; secondly, compressive stress homogenization can effectively avoid the influence brought by material property changes, and the dimensional stability of parts is good, which solves the problems of repeated mold repair, long cycle, high cost and the like of traditional springback compensation method, and the material has wide applicability. Finally, compression deformation can not only improve the wall thickness uniformity of the flattening area of beneficial wrinkles in reducer tube, but also eliminate microcracks that may be introduced in the flattening process to avoid cracking, and make residual compressive stress in the structure, which is beneficial to improving the service performance of parts. The present invention has reasonable design, reliable operation, remarkable effect and strong promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The following will describe a method for controlling the springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to the present invention with reference to the accompanying drawings. Figure 1 Schematic diagram of a preformed reducer part obtained by flattening beneficial wrinkles; Figure 2 for Figure 1 Part A is a schematic diagram of the thickness stress of the tube after pressurization and depressurization; Figure 3 for Figure 1 Part A shows the springback of the tube after pressurization and depressurization; Figure 4 Schematic diagram of placing the preformed reducer part into the final forming die; Figure 5 It is a schematic diagram of the reducing tube forming and die status; Figure 6 for Figure 4 Schematic diagram of stress variation in thickness direction of part B; Figure 7 for Figure 6Part B is a schematic diagram of the thickness stress of the tube after pressurization and depressurization; Figure 8 for Figure 6 Schematic diagram of the springback of the tube after pressurization and depressurization in Part B.
[0013] Description of Reference Numerals 1-preformed reducer part; 2-upper die; 3-lower die; 4-left sealing punch; 5-right sealing punch; 6-left movable insert; 7-right movable insert; 8-fluid medium channel; 9-final formed reducer; a-rebound amount after flattening and unloading of beneficial wrinkles; b-rebound amount after unloading of axial compression. DETAILED DESCRIPTION
[0014] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0015] The purpose of the present invention is to provide a method for controlling the springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation, so as to solve the problem that the beneficial wrinkles are flattened and the springback after pressure relief reduces the dimensional accuracy of the formed part during the process of internal high pressure forming of the tube. Figures 1 to 8 The present invention is further described in detail with reference to the accompanying drawings and specific embodiments.
[0016] The internal high-pressure forming reducer springback control method described in the present application uses a mold including an upper mold 2, a lower mold 3, a left sealing punch 4, a right sealing punch 5, a left movable insert 6 and a right movable insert 7; the upper mold 2, the lower mold 3, the left movable insert 6 and the right movable insert 7 together constitute the final forming mold cavity; the seal between the preformed reducer part 1 and the left sealing punch 4 and the right sealing punch 5 adopts an O-ring (conventional technical means, not shown); the left sealing punch 4 and the right sealing punch 5 can move axially respectively to apply axial pressure to the preformed reducer part 1 and the left movable insert 6 and the right movable insert 7, and the right sealing punch 5 is provided with a fluid channel 8 for filling the fluid medium into the interior of the preformed reducer part 1.
[0017] During the high pressure forming process of the reducer, the beneficial wrinkles are reversely bent and deformed under the action of the internal pressure, and then completely flattened against the mold cavity. The reverse bending deformation causes the flattened area to bear tensile stress on one side in the thickness direction of the tube blank and compressive stress on the other side, that is, there is a stress difference in the thickness direction. When the internal pressure is unloaded, the internal stress in the flattened area needs to be released. The above stress difference causes the tube blank to produce a bending moment, resulting in the separation of the flattened area from the mold cavity and rebound. Based on this, the present invention uses axial compression deformation to homogenize or reduce the stress difference in the thickness direction of the reducer, thereby eliminating or reducing the rebound.
[0018] The present invention provides a springback control method for an internal high-pressure forming reducer tube based on axial compression deformation. The method arranges an axially movable insert that meets the design requirements in the transition area of the final forming die, applies axial pressure to the reducer tube, causes axial compression deformation in the beneficial wrinkle flattening area, changes the stress state and distribution of the tube blank in the thickness direction in the area, eliminates or reduces the stress difference in the thickness direction, and achieves the effect of controlling springback.
[0019] Specifically, taking 6063 aluminum alloy reducer as an example, the present invention is completed according to the following steps: Step 1: The diameter of the tube is d0 = 50 mm, the wall thickness is t0 = 1.5 mm, and the expansion rate of the reducer is λ = (d-d0) / d0*100%=30%. A round-section tube blank is selected, and a preformed reducer tube part 1 is formed by forming the beneficial wrinkles. After unloading the internal pressure, there is a difference in internal pressure and external tension stress in the thickness direction of the flattened area of the beneficial wrinkles, resulting in a rebound a, such as Figure 2 In this case, the size of the reducer obtained is smaller than the design value. In this embodiment, the rebound amount generated after the beneficial wrinkles are flattened and unloaded is a = 0.5 mm; the tube blank includes but is not limited to low carbon steel, high strength steel, aluminum alloy or magnesium alloy tubes; Step 2: Place the preformed reducer part 1 into the final forming die, seal the two ends of the tube blank with the left sealing punch 4 and the right sealing punch 5 respectively, and then fill the preformed reducer part 1 with a fluid medium; the fluid medium is liquid or gas; Step 3: Adjust the internal pressure value of the preformed reducer part 1 to reach the set value P, and under the support of the internal fluid medium, the wrinkles will rebound and re-fit the mold cavity (rebound again after pressure relief). The internal pressure value P is 5 p s ≤P≤20 p s , p s The initial yield pressure of the tube blank is used to ensure that the preformed reducer parts can be smoothly axially compressed in the next step without compression instability and wrinkling; Step 4, the left sealing punch 4 and the right sealing punch 5 are axially fed at the same time, pushing the left movable insert 6 and the right movable insert 7 to axially compress the beneficial wrinkle flattening area of the preformed reducer part 1 and cause it to undergo plastic deformation. When the axial compression reaches the set value, the left sealing punch 4 and the right sealing punch 5 stop feeding. During the compression process, the preformed reducer part 1 is pressed against the final forming cavity under the support of the internal pressure; the axial compression is 0.1%-10% of the length of the beneficial wrinkle flattening area; the compression deformation changes the stress state and distribution of the beneficial wrinkle flattening area, realizes the uniformization of the compressive stress, eliminates or reduces the thickness stress difference, and significantly reduces the rebound caused by the reverse bending deformation of the beneficial wrinkles, such as Figure 5 As shown, after unloading the internal pressure, the reducer 9 that meets the dimensional accuracy requirements can be obtained; in this embodiment, the rebound amount of the reducer after axial compression deformation is b = 0.1 mm, which is significantly smaller than the rebound amount a.
[0020] The dimensional accuracy of the 6063 aluminum alloy reducer formed in this embodiment is improved by more than 80% compared with the reducer formed by conventional high pressure forming.
[0021] It should be understood that the above-mentioned embodiments are merely exemplary and are only used to help understand the method of the present invention and its core concept. Without departing from the basic principles of the present invention, various obvious or equivalent modifications or substitutions that can be made by technicians in this field to the above details will be included in the scope of the claims of the present invention.
Claims
1. A method for controlling the springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation, comprising placing a tube blank into a forming die, performing preforming processing to form a preformed tube, placing the preformed tube into a final forming die to form a formed tube, wherein the method is characterized in that: The springback control method applies axial pressure to the reducer by using an insert arranged in the transition area of the final forming die, so that the beneficial wrinkle flattening area undergoes axial compression deformation, and the stress state and distribution of the tube blank in the thickness direction in this area are changed to eliminate or reduce the stress difference in the thickness direction, thereby achieving the effect of controlling springback.
2. The method for controlling springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to claim 1, characterized in that: The forming tube is completed according to the following steps: Step 1: Select a round-section tube blank, and form a preformed reducer tube part through beneficial wrinkles. After unloading the internal pressure, the flattened area of the beneficial wrinkles will rebound, and the size will be smaller than the design value; Step 2: Place the preformed reducer part into the final forming die, seal the two ends of the preformed reducer part with the left sealing punch and the right sealing punch respectively, and then fill the interior of the preformed reducer part with a fluid medium; Step 3: Adjust the internal pressure value of the preformed reducer part to reach the set value P, and under the support of the internal fluid medium, the wrinkles will rebound and re-fit the mold cavity. The internal pressure value is 5 p s ≤P≤20 p s , p s It is the initial yield pressure of the tube blank, which is used to ensure that the preformed reducer parts can be smoothly axially compressed in the next step without compression instability and wrinkling.
3. The method for controlling springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to claim 2, characterized in that: After step 3, add step 4; Step 4: The left sealing punch and the right sealing punch are axially fed at the same time to push the left movable insert and the right movable insert to axially compress the beneficial wrinkle flattening area of the reducer and cause it to undergo plastic deformation. When the axial compression reaches a set value, the left sealing punch and the right sealing punch stop feeding. During the compression process, the preformed reducer part is pressed against the final forming die cavity under the support of the internal pressure; the axial compression is 0.1%-10% of the length of the beneficial wrinkle flattening area.
4. The method for controlling springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to claim 2, characterized in that: In step 1, the tube blank comprises a tube made of low carbon steel, high strength steel, aluminum alloy or magnesium alloy.
5. The method for controlling springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to claim 2, characterized in that: In step one, the mold comprises an upper mold (2), a lower mold (3), a left movable insert (6), a right movable insert (7), a left sealing punch (4) and a right sealing punch (5).
6. The method for controlling springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to claim 2, characterized in that: In the step 3, 5 p s ≤P≤20 p s , p s is the initial yield pressure of the tube.
7. The method for controlling springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to claim 3, characterized in that: In the step 4, the amount of compression is 0.1%-10% of the length of the beneficial wrinkle flattening area.
8. The method for controlling springback of a variable diameter tube formed by internal high pressure forming based on axial compression deformation according to claim 2, characterized in that: The fluid medium is liquid or gas.
Citation Information
Cited By
Corrugated pipe forming springback control method and mold based on stress regulation and control
CN119794148A