Cold and hot tearing type transfer printing film and preparation method thereof

Through the surface treatment of modified nano-silica and titanium dioxide, a release layer suitable for hot and cold peel-off transfer films is prepared, which solves the problem that traditional transfer films cannot meet the requirements of hot and cold peeling at the same time, and improves the physical properties and resistance UV capability.

CN118769745APending Publication Date: 2024-10-15JIANGSU SUNDERRAY LASER PACKAGING MATERIALS CO LTD

Patent Information

Application Number
CN202410726977.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional hot-tear and cold-tear transfer films each have limitations. They cannot meet the requirements of cold tear and hot tear at the same time, and the physical properties of their release layers are insufficient.

Method used

The release agent is prepared using polymethyl methacrylate, modified nano-silica, modified titanium dioxide and other materials, and its surface tension is reduced through surface treatment to form a release layer suitable for hot and cold tear-off transfer films, and combined with solvents Type glue to prepare hot and cold tear-off transfer film.

Benefits of technology

A transfer film that can effectively peel off images under both cold and hot conditions is achieved, which enhances the physical properties and UV resistance while improving the wear resistance and smoothness of the transfer film.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of transfer printing films, in particular to a cold and hot tearing type transfer printing film and a preparation method thereof. Comprising the following steps: 1, pouring a release agent on a PET film, carrying out one-time blade coating to form a film by using a silk-screen scraper with a scraper angle of 45-50 degrees, and drying to obtain a release layer; 2, the PET film coated with the release layer penetrates through the position between an impression cylinder and a plate cylinder, the plate cylinder rotates in an ink groove and is dried, and a printing layer is obtained; and 3, coating the solvent type glue on the printing layer, and drying at normal temperature to obtain the cold and hot tearing type transfer printing film. The transfer printing film has the beneficial effects that the surface tension is reduced by performing surface treatment on nano silicon dioxide and titanium dioxide in the release substance, so that the binding force of the release layer and the substrate layer is smaller than that of the adhesive layer and the base material, the requirements of cold tearing and hot tearing are met, and meanwhile, the physical property of the transfer printing film is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of transfer films, in particular to a hot / cold tearing transfer film and a preparation method thereof. Background Art

[0002] Transfer film is a special material used in thermal transfer technology, which transfers images or patterns to various substrates such as textiles, plastics, ceramics, etc. through heat and pressure. Thermal transfer technology is widely used in clothing, footwear, bags, sports equipment and other fields due to its easy operation, exquisite and delicate patterns, bright and long-lasting colors. During the thermal transfer process, the image on the transfer film is transferred to the substrate through the heat and pressure applied by the heat press. This process requires the transfer film to have good thermal stability, adhesion and release properties. The release layer is a key part of the transfer film, which determines the efficiency and quality of the image transfer.

[0003] At present, the traditional hot-tear release layer needs to be peeled off at high temperature, while the cold-tear type allows peeling at room temperature, but both have limitations. Therefore, in order to solve the above problems, the present invention prepares a hot-cold-tear transfer film. Summary of the invention

[0004] The object of the present invention is to provide a hot / cold tear type transfer film and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] More optimally: the transfer film is composed of a base layer, a release layer, a printing layer, and an adhesive layer from bottom to top; the base layer is a PET film; the release layer is composed of a release agent, including polymethyl methacrylate and a release substance; the adhesive layer is composed of a solvent-based glue, including epoxy resin, a curing agent, an accelerator, and toluene.

[0007] More optimally: the preparation method of the release agent is: dissolving polymethyl methacrylate in toluene, adding a release material and mixing and stirring for 20-30 minutes, adding polyurethane, stirring at 110-120°C for 1-2 hours, cooling to 60-65°C, adding ethyl acetate, stirring for 0.5-1 hour, cooling and discharging to obtain a release agent.

[0008] More optimally, the release agent comprises the following components: by weight, 10 parts of polymethyl methacrylate, 15-20 parts of toluene, 0.8-1 parts of release material, 0.1-0.2 parts of polyurethane, and 15-20 parts of ethyl acetate; the release material comprises modified nano-silicon dioxide and modified titanium dioxide in a mass ratio of 1:(1.2-1.5).

[0009] More optimally: the preparation method of the modified nano-silicon dioxide is: mixing nano-silicon dioxide with concentrated nitric acid, stirring at room temperature for 10-15 minutes; separating, adding the treated nano-silicon dioxide to anhydrous ethanol, reflux at 80-82°C for 20-30 minutes, and evaporating the ethanol to obtain modified nano-silicon dioxide.

[0010] More optimally: the preparation method of the modified titanium dioxide is as follows: (1) 3,7-dimethyloctylmagnesium bromide, 1,3-bis(diphenylphosphinopropane)nickel dichloride and o-dichlorobenzene are mixed and reacted for 6-8 hours to separate and obtain intermediate A; (2) intermediate A, maleic anhydride and carbon disulfide are mixed and stirred, anhydrous AlCl3 is added in batches, reacted for 30-50 minutes, and the modifier is separated and obtained; (3) titanium dioxide is dissolved in toluene, γ-aminopropyltriethoxysilane is added under a protective atmosphere, reacted at 70-90°C for 4-5 hours, and dried to obtain amino titanium dioxide; (5) amino titanium dioxide is dissolved in ethyl acetate, the modifier and benzenesulfonic acid are added, reacted at 50-60°C for 3-4 hours, filtered, washed and dried to obtain modified titanium dioxide.

[0011] More optimally: the intermediate A comprises the following components: by weight, 1-3 parts of 3,7-dimethyloctylmagnesium bromide, 0.5-0.8 parts of 1,3-bis(diphenylphosphinopropane)nickel dichloride, and 2-3 parts of o-dichlorobenzene; the modifier comprises the following components: by weight, 5-6 parts of intermediate A, 6-7 parts of maleic anhydride, 0.5-1 parts of carbon disulfide, and 1-2 parts of anhydrous AlCl3; the amination titanium dioxide comprises the following components: by weight, 10-12 parts of titanium dioxide, and 15-18 parts of γ-aminopropyltriethoxysilane; the modified titanium dioxide comprises the following components: by weight, 10-12 parts of amination titanium dioxide, 5-8 parts of modifier, and 1-2 parts of benzenesulfonic acid.

[0012] More optimally: the preparation method of the solvent-based glue is: dissolving the dimer acid-modified epoxy resin in tetrahydrofuran, stirring for 1-2 hours, adding a fatty amine curing agent and an accelerator, and continuing to stir for 4-5 hours to obtain the solvent-based glue.

[0013] More optimally, the solvent-based glue comprises the following components: by weight, 30-50 parts of dimer acid-modified epoxy resin, 1-8 parts of fatty amine curing agent, 1-2 parts of accelerator, and 150-200 parts of tetrahydrofuran; the model of the dimer acid-modified epoxy resin is SQE-172; the fatty amine curing agent is diethylenetriamine; and the model of the accelerator is ADP155.

[0014] More optimally: the method for preparing a hot and cold tear transfer film comprises the following steps:

[0015] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 45-50°, and then dry it to obtain a release layer.

[0016] Step 2: Coat the surface of the PET film coated with the release layer with ink, and dry it to obtain a printing layer;

[0017] Step 3: Apply solvent-based glue to the printed layer, dry at 60-70° C. for 30-60 minutes, and obtain a hot-cold tear transfer film.

[0018] The present invention reduces the surface tension of the nano-silicon dioxide and titanium dioxide in the release material by surface treatment, so that the bonding force between the release layer and the base layer is smaller than the bonding force between the adhesive layer and the base material, meets the requirements of cold tearing and hot tearing, and enhances the physical properties of the transfer film. The details are as follows:

[0019] First, titanium dioxide is aminated by γ-aminopropyltriethoxysilane, and the resulting amino group reacts with the carboxyl group in the modifier, so that a longer carbon molecular chain is grafted onto the surface of titanium dioxide, which improves the dispersibility of titanium dioxide in the release agent and reduces the surface tension of titanium dioxide, thereby reducing the surface tension of the release agent, so that it can better infiltrate and spread on the surface of the PET film, and maintain a certain degree of adhesion, which can meet the effects of cold tearing and hot tearing. At the same time, the surface of the modified nano-silicon dioxide contains a large number of hydroxyl groups, which will aggregate with the modified titanium dioxide through molecular forces, reducing the surface area of ​​the two, thereby reducing the surface tension of the two. At the same time, nano-silicon dioxide and titanium dioxide are used as reinforcing materials to effectively enhance the physical properties of the transfer film.

[0020] Second, the molecular chain grafted on the surface of titanium dioxide contains benzene rings and double bonds, which can absorb ultraviolet rays through the conjugation effect and enhance the transfer film's ability to resist ultraviolet radiation. At the same time, when the coating is drying, nano-silicon dioxide can form a three-dimensional network structure, which improves the strength and smoothness of the coating and enhances the ink-fixing ability. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] It should be noted that the following parts are by weight, and the purchase manufacturers of all raw materials involved in the present invention are exemplary without any special restrictions: In the following embodiments, the PET film item number is PETLXM, and the brand is Yuxuan; polymethyl methacrylate CAS is 9011-14-7, and the manufacturer is Merck; 3,7-dimethyloctylmagnesium bromide CAS is 114499-45-5, and the purchase manufacturer is Jinjinle; 1,3-bis(diphenylphosphinopropane) nickel dichloride CAS is 15629-92-2, and the purchase manufacturer is Yongkuo Technology; nano-silicon dioxide model is TSP-H10, and the purchase manufacturer is Tianxing; titanium dioxide model is PT05-0. The purchase manufacturer is Baoket New Materials; the ink brand used for inkjet is xfy, and the item number is 202117.

[0023] Embodiment 1: A method for preparing a hot-cold tear transfer film, comprising the following steps:

[0024] Pre-preparation:

[0025] (1) Preparation of modified nano-silica: Nano-silica was mixed with concentrated nitric acid and stirred at room temperature for 10 min. After separation, the treated nano-silica was added to anhydrous ethanol and refluxed at 80° C. for 20 min. The ethanol was evaporated to obtain modified nano-silica.

[0026] (2) Preparation of modified titanium dioxide: (1) Mix 1 part of 3,7-dimethyloctylmagnesium bromide, 0.5 parts of 1,3-bis(diphenylphosphinopropane)nickel dichloride and 2 parts of o-dichlorobenzene and react for 6 hours to separate and obtain intermediate A; (2) Mix 5 parts of intermediate A6, 1 part of maleic anhydride and 0.5 part of carbon disulfide, add 1 part of anhydrous AlCl3 in batches, react for 30 minutes, and separate and obtain the modifier; (3) Dissolve 10 parts of titanium dioxide in toluene, add 15 parts of γ-aminopropyltriethoxysilane under nitrogen atmosphere, react at 70°C for 4 hours, and dry to obtain amino titanium dioxide; (5) Dissolve 10 parts of amino titanium dioxide in ethyl acetate, add 5 parts of modifier and 1 part of benzenesulfonic acid, react at 50°C for 3 hours, filter, wash and dry to obtain modified titanium dioxide.

[0027] (3) Preparation of release agent: 10 parts of polymethyl methacrylate was dissolved in toluene, 2.2 parts of release material (1 part of modified nano-silicon dioxide, 1.2 parts of modified titanium dioxide) were added and mixed and stirred for 20 minutes, 0.1 parts of polyurethane were added, and the mixture was stirred at 110°C for 1 hour, cooled to 60°C, 15 parts of ethyl acetate were added, and the mixture was stirred for 0.5 hours, cooled and discharged to obtain a release agent.

[0028] Pre-preparation: Preparation of solvent-based glue: Dissolve 30 parts of dimer acid-modified epoxy resin SQE-172 in tetrahydrofuran, stir for 1 hour, add 1 part of fatty amine curing agent diethylenetriamine and 1 part of accelerator ADP155, continue stirring for 4 hours to obtain solvent-based glue.

[0029] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 45°, and then dry it to obtain a release layer.

[0030] Step 2: The PET film coated with the release layer is passed through the middle of the impression cylinder and the plate cylinder. The plate cylinder rotates in the ink tank and dries to obtain the printing layer.

[0031] Step 3: Apply solvent-based glue to the printed layer and dry it to obtain a hot and cold tear transfer film.

[0032] Embodiment 2: A method for preparing a hot-cold tear transfer film, comprising the following steps:

[0033] Pre-preparation:

[0034] (1) Preparation of modified nano-silica: Nano-silica was mixed with concentrated nitric acid and stirred at room temperature for 15 minutes; separated, the treated nano-silica was added to anhydrous ethanol, refluxed at 82° C. for 30 minutes, and the ethanol was evaporated to obtain modified nano-silica.

[0035] (2) Preparation of modified titanium dioxide: (1) Mix 3 parts of 3,7-dimethyloctylmagnesium bromide, 0.8 parts of 1,3-bis(diphenylphosphinopropane)nickel dichloride and 3 parts of o-dichlorobenzene and react for 8 hours to separate and obtain intermediate A; (2) Mix 6 parts of intermediate A, 7 parts of maleic anhydride and 1 part of carbon disulfide, add 2 parts of anhydrous AlCl3 in batches, react for 50 minutes, and separate and obtain the modifier; (3) Dissolve 12 parts of titanium dioxide in toluene, add 18 parts of γ-aminopropyltriethoxysilane under nitrogen atmosphere, react at 90°C for 5 hours, and dry to obtain amino titanium dioxide; (5) Dissolve 12 parts of amino titanium dioxide in ethyl acetate, add 8 parts of modifier and 2 parts of benzenesulfonic acid, react at 60°C for 4 hours, filter, wash and dry to obtain modified titanium dioxide.

[0036] (3) Preparation of release agent: 10 parts of polymethyl methacrylate was dissolved in toluene, 2.5 parts of release material (1 part of modified nano-silicon dioxide, 1.5 parts of modified titanium dioxide) were added and mixed and stirred for 30 minutes, 0.2 parts of polyurethane were added, and the mixture was stirred at 120°C for 2 hours. The mixture was cooled to 65°C, 20 parts of ethyl acetate were added, and the mixture was stirred for 1 hour. The mixture was cooled and discharged to obtain a release agent.

[0037] Pre-preparation: Preparation of solvent-based glue: Dissolve 50 parts of dimer acid-modified epoxy resin SQE-172 in tetrahydrofuran, stir for 2 hours, add 8 parts of fatty amine curing agent diethylenetriamine and 2 parts of accelerator ADP155, continue stirring for 5 hours to obtain solvent-based glue.

[0038] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 50°, and then dry it to obtain a release layer.

[0039] Step 2: The PET film coated with the release layer is passed through the middle of the impression cylinder and the plate cylinder. The plate cylinder rotates in the ink tank and dries to obtain the printing layer.

[0040] Step 3: Apply solvent-based glue to the printed layer and dry it to obtain a hot and cold tear transfer film.

[0041] Embodiment 3: A method for preparing a hot-cold tear transfer film, comprising the following steps:

[0042] Pre-preparation:

[0043] (1) Preparation of modified nano-silica: Nano-silica was mixed with concentrated nitric acid and stirred at room temperature for 12 minutes; separated, the treated nano-silica was added to anhydrous ethanol, refluxed at 81° C. for 25 minutes, and the ethanol was evaporated to obtain modified nano-silica.

[0044] (2) Preparation of modified titanium dioxide: (1) 2 parts of 3,7-dimethyloctylmagnesium bromide, 0.6 parts of 1,3-bis(diphenylphosphinopropane)nickel dichloride and 2.5 parts of o-dichlorobenzene were mixed and reacted for 7 hours to separate and obtain intermediate A; (2) 5.5 parts of intermediate A, 6.5 parts of maleic anhydride and 0.6 parts of carbon disulfide were mixed and stirred, 1.5 parts of anhydrous AlCl3 were added in batches, reacted for 40 minutes, and the modifier was separated and obtained; (3) 11 parts of titanium dioxide were dissolved in toluene, 16 parts of γ-aminopropyltriethoxysilane were added under nitrogen atmosphere, reacted at 80°C for 4.5 hours, and dried to obtain amino titanium dioxide; (5) 11 parts of amino titanium dioxide were dissolved in ethyl acetate, 6 parts of modifier and 1.5 parts of benzenesulfonic acid were added, reacted at 55°C for 3.5 hours, filtered, washed and dried to obtain modified titanium dioxide.

[0045] (3) Preparation of release agent: 10 parts of polymethyl methacrylate was dissolved in toluene, 2.3 parts of release material (1 part of modified nano-silica, 1.3 parts of modified titanium dioxide) were added and the mixture was stirred for 25 minutes, 0.15 parts of polyurethane was added, the mixture was stirred at 115°C for 1.5 hours, the temperature was lowered to 65°C, 18 parts of ethyl acetate was added, the mixture was stirred for 0.8 hours, the temperature was lowered and the mixture was discharged to obtain a release agent.

[0046] Pre-preparation: Preparation of solvent-based glue: Dissolve 40 parts of dimer acid-modified epoxy resin SQE-172 in tetrahydrofuran, stir for 1.5 hours, add 5 parts of fatty amine curing agent diethylenetriamine and 1.5 parts of accelerator ADP155, continue stirring for 4.5 hours to obtain solvent-based glue.

[0047] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 50°, and then dry it to obtain a release layer.

[0048] Step 2: The PET film coated with the release layer is passed through the middle of the impression cylinder and the plate cylinder. The plate cylinder rotates in the ink tank and dries to obtain the printing layer.

[0049] Step 3: Apply solvent-based glue to the printed layer and dry it to obtain a hot and cold tear transfer film.

[0050] Embodiment 4: A method for preparing a hot-tear transfer film, comprising the following steps:

[0051] Pre-preparation:

[0052] (1) Preparation of modified nano-silica: Nano-silica was mixed with concentrated nitric acid and stirred at room temperature for 12 minutes; separated, the treated nano-silica was added to anhydrous ethanol, refluxed at 81° C. for 25 minutes, and the ethanol was evaporated to obtain modified nano-silica.

[0053] (2) Preparation of modified titanium dioxide: (1) 2 parts of 3,7-dimethyloctylmagnesium bromide, 0.6 parts of 1,3-bis(diphenylphosphinopropane)nickel dichloride and 2.5 parts of o-dichlorobenzene were mixed and reacted for 7 hours to separate and obtain intermediate A; (2) 5.5 parts of intermediate A, 6.5 parts of maleic anhydride and 0.6 parts of carbon disulfide were mixed and stirred, 1.5 parts of anhydrous AlCl3 were added in batches, reacted for 40 minutes, and the modifier was separated and obtained; (3) 11 parts of titanium dioxide were dissolved in toluene, 16 parts of γ-aminopropyltriethoxysilane were added under nitrogen atmosphere, reacted at 80°C for 4.5 hours, and dried to obtain amino titanium dioxide; (5) 11 parts of amino titanium dioxide were dissolved in ethyl acetate, 6 parts of modifier and 1.5 parts of benzenesulfonic acid were added, reacted at 55°C for 3.5 hours, filtered, washed and dried to obtain modified titanium dioxide.

[0054] (3) Preparation of release agent: 10 parts of polymethyl methacrylate was dissolved in toluene, 2.2 parts of release material (1 part of modified nano-silicon dioxide, 1.2 parts of modified titanium dioxide) were added and mixed and stirred for 20 minutes, 0.1 parts of polyurethane were added, and the mixture was stirred at 110°C for 1 hour, cooled to 60°C, 15 parts of ethyl acetate were added, and the mixture was stirred for 0.5 hours, cooled and discharged to obtain a release agent.

[0055] Pre-preparation: Preparation of solvent-based glue: Dissolve 30 parts of dimer acid-modified epoxy resin SQE-172 in tetrahydrofuran, stir for 1.5 hours, add 5 parts of fatty amine curing agent diethylenetriamine and 1.5 parts of accelerator ADP155, continue stirring for 4.5 hours to obtain solvent-based glue.

[0056] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 50°, and then dry it to obtain a release layer.

[0057] Step 2: The PET film coated with the release layer is passed through the middle of the impression cylinder and the plate cylinder. The plate cylinder rotates in the ink tank and dries to obtain the printing layer.

[0058] Step 3: Apply solvent-based glue to the printed layer and dry it to obtain a hot and cold tear transfer film.

[0059] Comparative Example 1: No modified nano-silicon dioxide was added, and the rest was the same as Example 4, as follows:

[0060] Pre-preparation:

[0061] (1) Preparation of modified titanium dioxide: (1) 2 parts of 3,7-dimethyloctylmagnesium bromide, 0.6 parts of 1,3-bis(diphenylphosphinopropane)nickel dichloride and 2.5 parts of o-dichlorobenzene were mixed and reacted for 7 hours to separate and obtain intermediate A; (2) 5.5 parts of intermediate A, 6.5 parts of maleic anhydride and 0.6 parts of carbon disulfide were mixed and stirred, 1.5 parts of anhydrous AlCl3 were added in batches, reacted for 40 minutes, and the modifier was separated and obtained; (3) 11 parts of titanium dioxide were dissolved in toluene, 16 parts of γ-aminopropyltriethoxysilane were added under nitrogen atmosphere, reacted at 80°C for 4.5 hours, and dried to obtain amino titanium dioxide; (5) 11 parts of amino titanium dioxide were dissolved in ethyl acetate, 6 parts of modifier and 1.5 parts of benzenesulfonic acid were added, reacted at 55°C for 3.5 hours, filtered, washed and dried to obtain modified titanium dioxide.

[0062] (2) Preparation of release agent: 10 parts of polymethyl methacrylate was dissolved in toluene, 2.2 parts of modified titanium dioxide was added, and the mixture was stirred for 20 min. 0.1 parts of polyurethane was added, and the mixture was stirred at 110° C. for 1 h. The mixture was cooled to 60° C., 15 parts of ethyl acetate was added, and the mixture was stirred for 0.5 h. The mixture was cooled and discharged to obtain a release agent.

[0063] Pre-preparation: Preparation of solvent-based glue: Dissolve 30 parts of dimer acid-modified epoxy resin SQE-172 in tetrahydrofuran, stir for 1.5 hours, add 5 parts of fatty amine curing agent diethylenetriamine and 1.5 parts of accelerator ADP155, continue stirring for 4.5 hours to obtain solvent-based glue.

[0064] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 50°, and then dry it to obtain a release layer.

[0065] Step 2: The PET film coated with the release layer is passed through the middle of the impression cylinder and the plate cylinder. The plate cylinder rotates in the ink tank and dries to obtain the printing layer.

[0066] Step 3: Apply solvent-based glue to the printed layer and dry it to obtain a hot and cold tear transfer film.

[0067] Comparative Example 2: No modified titanium dioxide was added, and the rest was the same as Example 4, specifically as follows:

[0068] Pre-preparation:

[0069] (1) Preparation of modified nano-silica: Nano-silica was mixed with concentrated nitric acid and stirred at room temperature for 12 minutes; separated, the treated nano-silica was added to anhydrous ethanol, refluxed at 81° C. for 25 minutes, and the ethanol was evaporated to obtain modified nano-silica.

[0070] (2) Preparation of release agent: 10 parts of polymethyl methacrylate was dissolved in toluene, 2.2 parts of modified nano-silica was added, and the mixture was stirred for 20 min. 0.1 parts of polyurethane was added, and the mixture was stirred at 110° C. for 1 h. The mixture was cooled to 60° C., 15 parts of ethyl acetate was added, and the mixture was stirred for 0.5 h. The mixture was cooled and discharged to obtain a release agent.

[0071] Pre-preparation: Preparation of solvent-based glue: Dissolve 30 parts of dimer acid-modified epoxy resin SQE-172 in tetrahydrofuran, stir for 1.5 hours, add 5 parts of fatty amine curing agent diethylenetriamine and 1.5 parts of accelerator ADP155, continue stirring for 4.5 hours to obtain solvent-based glue.

[0072] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 50°, and then dry it to obtain a release layer.

[0073] Step 2: The PET film coated with the release layer is passed through the middle of the impression cylinder and the plate cylinder. The plate cylinder rotates in the ink tank and dries to obtain the printing layer.

[0074] Step 3: Apply solvent-based glue to the printed layer and dry it to obtain a hot and cold tear transfer film.

[0075] Comparative Example 3: Nano-silicon dioxide and titanium dioxide were not treated, and the rest was the same as Example 4, as follows:

[0076] Pre-preparation: Preparation of release agent: dissolve 10 parts of polymethyl methacrylate in toluene, add 2.2 parts of modified titanium dioxide, stir for 20 minutes, add 0.1 parts of polyurethane, stir at 110°C for 1 hour, cool to 60°C, add 15 parts of ethyl acetate, stir for 0.5 hour, cool and discharge to obtain the release agent.

[0077] Pre-preparation: Preparation of solvent-based glue: Dissolve 30 parts of dimer acid-modified epoxy resin SQE-172 in tetrahydrofuran, stir for 1.5 hours, add 5 parts of fatty amine curing agent diethylenetriamine and 1.5 parts of accelerator ADP155, continue stirring for 4.5 hours to obtain solvent-based glue.

[0078] Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 50°, and then dry it to obtain a release layer.

[0079] Step 2: The PET film coated with the release layer is passed through the middle of the impression cylinder and the plate cylinder. The plate cylinder rotates in the ink tank and dries to obtain the printing layer.

[0080] Step 3: Apply solvent-based glue to the printed layer and dry it to obtain a hot and cold tear transfer film.

[0081] Testing experiment: Print a standard CMYK image on the transfer film obtained in the embodiment and the comparative example, sprinkle powder and shake powder on the surface, and peel it off after hot stamping. Measure whether there is a residual image on the surface of the intermediate medium after transfer. If there is a residual image, it cannot be peeled off, and if there is no residual image, it can be peeled off. If the peeling can be achieved within the temperature of 100-120℃, it can meet the requirements of hot peeling; if the peeling can be achieved at a peeling temperature of <80℃, it can meet the requirements of cold peeling;

[0082] The transfer films obtained in the examples and comparative examples were cut into corresponding sizes and fixed on the working turntable of the wear tester. A weight of 250g was added to the pressure arm, and the pressure arm was gently lowered. The dust nozzle was lowered and adjusted to 1-1.5mm away from the sample plate. The switches were turned on in sequence, and the samples were abraded for 20 turns. The difference before and after abrasion was measured by an analytical balance. The smaller the difference, the better the abrasion resistance.

[0083] The obtained data are shown in the following table:

[0084] project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Can it be thermally stripped? able able able able able no no Can cold stripping be performed able able able able no no yes Wear amount / g 0.004 0.005 0.007 0.003 0.015 0.017 0.019

[0085] Table 1

[0086] Conclusion: Examples 1-4 reduce the surface tension of nano-silicon dioxide and titanium dioxide in the release material by surface treatment, so that the bonding force between the release agent and the base layer is less than the bonding force between the adhesive layer and the base material, meeting the requirements of cold tearing and hot tearing, and enhancing the wear resistance and physical properties of the transfer film. Comparative Example 1 does not add modified nano-silicon dioxide, and the performance is reduced; Comparative Example 2 does not add modified silicon dioxide, and the performance is reduced; Comparative Example 3 does not treat nano-silicon dioxide and titanium dioxide, which reduces the dispersibility of the two in the release agent and the performance is reduced.

[0087] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A hot and cold tear transfer film, characterized in that: The transfer film comprises a base layer, a release layer, a printing layer and an adhesive layer from bottom to top; the base layer is a PET film; the release layer is composed of a release agent, including polymethyl methacrylate and a release substance; the adhesive layer is composed of a solvent-based glue, including epoxy resin, a curing agent, an accelerator and toluene.

2. The hot / cold tear transfer film according to claim 1, characterized in that: The preparation method of the release agent is as follows: polymethyl methacrylate is dissolved in toluene, a release material is added and mixed and stirred for 20-30 minutes, polyurethane is added, and the mixture is stirred at 110-120° C. for 1-2 hours, the mixture is cooled to 60-65° C., ethyl acetate is added, the mixture is stirred for 0.5-1 hour, the mixture is cooled and discharged, and the release agent is obtained.

3. The hot / cold tear transfer film according to claim 2, characterized in that: The release agent comprises the following components: by weight, 10 parts of polymethyl methacrylate, 15-20 parts of toluene, 0.8-1 parts of release material, 0.1-0.2 parts of polyurethane, and 15-20 parts of ethyl acetate; the release material comprises modified nano silicon dioxide and modified titanium dioxide in a mass ratio of 1:(1.2-1.5).

4. The hot / cold tear transfer film according to claim 3, characterized in that: The preparation method of the modified nano-silicon dioxide is as follows: mixing the nano-silicon dioxide with concentrated nitric acid and stirring at room temperature for 10-15 minutes; Separate, add the treated nano-silica into anhydrous ethanol, reflux at 80-82° C. for 20-30 min, evaporate the ethanol, and obtain modified nano-silica.

5. The hot / cold tear transfer film according to claim 3, characterized in that: The preparation method of the modified titanium dioxide is as follows: (1) 3,7-dimethyloctylmagnesium bromide, 1,3-bis(diphenylphosphinopropane)nickel dichloride and o-dichlorobenzene are mixed and reacted for 6-8 hours to separate and obtain an intermediate A; (2) the intermediate A, maleic anhydride and carbon disulfide are mixed and stirred, anhydrous AlCl3 is added in batches, reacted for 30-50 minutes, and a modifier is separated and obtained; (3) titanium dioxide is dissolved in toluene, γ-aminopropyltriethoxysilane is added under a protective atmosphere, the reaction is carried out at 70-90° C. for 4-5 hours, and dried to obtain amino titanium dioxide; (5) the amino titanium dioxide is dissolved in ethyl acetate, the modifier and benzenesulfonic acid are added, the reaction is carried out at 50-60° C. for 3-4 hours, suction filtered, washed and dried to obtain the modified titanium dioxide.

6. The hot / cold tear transfer film according to claim 5, characterized in that: The intermediate A comprises the following components: by weight, 1-3 parts of 3,7-dimethyloctylmagnesium bromide, 0.5-0.8 parts of 1,3-bis(diphenylphosphinopropane)nickel dichloride, and 2-3 parts of o-dichlorobenzene; the modifier comprises the following components: by weight, 5-6 parts of intermediate A, 6-7 parts of maleic anhydride, 0.5-1 parts of carbon disulfide, and 1-2 parts of anhydrous AlCl3; the amination titanium dioxide comprises the following components: by weight, 10-12 parts of titanium dioxide and 15-18 parts of γ-aminopropyltriethoxysilane; The modified titanium dioxide comprises the following components: by weight, 10-12 parts of amino titanium dioxide, 5-8 parts of modifier, and 1-2 parts of benzenesulfonic acid.

7. The hot / cold tear transfer film according to claim 1, characterized in that: The preparation method of the solvent-based glue is as follows: dissolving dimer acid-modified epoxy resin in tetrahydrofuran, stirring for 1-2 hours, adding a fatty amine curing agent and an accelerator, and continuing to stir for 4-5 hours to obtain the solvent-based glue.

8. The hot / cold tear transfer film according to claim 1, characterized in that: The solvent-based glue comprises the following components: by weight, 30-50 parts of dimer acid-modified epoxy resin, 1-8 parts of fatty amine curing agent, 1-2 parts of accelerator, and 150-200 parts of tetrahydrofuran.

9. A method for preparing a hot / cold tear transfer film according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Pour the release agent onto the PET film and use a silk screen scraper to scrape it once to form a film. The scraper angle is 45-50°, and then dry it to obtain a release layer. Step 2: Coat the surface of the PET film coated with the release layer with ink, dry it, and obtain a printing layer; Step 3: Apply solvent-based glue to the printed layer, dry at 60-70° C. for 30-60 minutes, and obtain a hot-cold tear transfer film.

Citation Information

Patent Citations

  • Heat transfer printing adhesive for glass matrix, heat transfer printing film, preparation method and application

    CN102936477A

  • Heat transfer printing membrane and manufacturing method thereof

    CN103465669A

  • PET protective film having good wear resistance and strong impact resistance and preparation technology thereof

    CN103602044A

  • Water-based hot-cold tearing type transfer print release agent and preparation method thereof

    CN106883660A

  • Release agent, release film, composite film and ink-jet printing medium, preparation methods of release agent, release film, composite film and ink-jet printing medium, and application of ink-jet printing medium

    CN107699067A

Cited By

  • Positioning environment-friendly laser transfer film

    CN119858400A