Continuous polyolefin-based carbon fiber and preparation method thereof
Through multi-stage sulfonation and carbonization treatment of modified polyolefin fiber, combined with multi-stage drafting technology, the structure and mechanical properties of carbon fiber are optimized, which solves the problems of high cost and insufficient mechanical properties of carbon fiber in the existing technology, and achieves high strength. and high modulus carbon fiber preparation.
Patent Information
- Application Number
- CN202410984699.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-15
AI Technical Summary
Existing carbon fibers have high costs and problems in improving mechanical properties during the preparation process. Especially in the stabilization and carbonization process of polyolefin-based carbon fibers, existing research fails to effectively match fiber properties and tension, resulting in insufficient structural and mechanical properties.
Modified polyolefin fiber is used for multi-stage sulfonation and carbonization treatment, combined with multi-stage drafting treatment, and the fiber structure and mechanical properties are optimized through acid treatment, water washing, oiling treatment and drying hot roller steps.
It improves the microstructure and mechanical properties of carbon fiber, reduces production costs, and meets the automotive industry's needs for high strength and high modulus.
Smart Images

Figure BDA0004957042820000161 
Figure BDA0004957042820000171 
Figure BDA0004957042820000281
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials and relates to a continuous polyolefin-based carbon fiber and a preparation method thereof. Background Art
[0002] Carbon fiber has been used in more and more industries such as wind turbine blades, sports, and automobiles due to its excellent properties such as high strength, high modulus, high temperature resistance, and corrosion resistance. However, the high manufacturing cost of carbon fiber limits the large-scale application of carbon fiber in civilian fields such as automobiles. Polyacrylonitrile-based carbon fiber is the carbon fiber that has been put into large-scale use, with a market share of more than 95%. In the preparation cost of polyacrylonitrile-based carbon fiber, the cost of raw silk accounts for more than 51% of the total preparation cost, so reducing the cost of raw silk is the main direction of low-cost carbon fiber.
[0003] Polyolefin fibers are strong candidates for low-cost carbon fiber precursors due to their high carbon content and low raw material costs. At present, the highest tensile strength and tensile modulus of polyethylene-based carbon fibers have reached 2.4 GPa and 400 GPa respectively (small, 2017, 1701926), exceeding the automotive industry's demand for carbon fiber mechanical strength (tensile strength: 1.72 GPa, tensile modulus: 172 GPa). However, the current research on polyolefin-based carbon fibers is still in the laboratory stage, and the existing research has adopted a simple constant temperature and constant drawing tension in the stabilization and carbonization process of carbon fibers, without considering the matching of fiber performance and tension, which is not conducive to the further improvement of fiber structure and mechanical properties.
[0004] More importantly, the infusibility (also known as thermal stabilization) of polyolefin precursors of high-performance polypropylene-based carbon fibers usually needs to be carried out in a liquid medium. The changes in the chemical and physical structure of the fibers in this process are significantly different from those of commercial carbon fiber precursors such as polyacrylonitrile, asphalt-based, and viscose that do not melt in the air medium. For example, the liquid medium has a swelling effect on the precursor and the infusible fiber, causing the fiber to swell to varying degrees in the axial and radial directions. The radial swelling not only inhibits the formation of a dense infusible cortical structure, but also helps the material exchange in the infusible process. The axial expansion causes the fiber to reversibly extend in the length direction. However, for fibers that do not melt in the air medium, it is difficult to completely eliminate the skin-core structure of the fiber, which hinders the material exchange in the infusible process, and the fiber shrinks in the length direction during the heating process. Therefore, combined with the genetic relationship between the fiber structure in the infusibility and carbonization processes, the existing infusibility process of commercial carbon fiber precursors and the temperature and tension setting principles and parameter systems in the subsequent carbonization process cannot be directly applied.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The object of the present invention is to provide a continuous polyolefin-based carbon fiber and a preparation method thereof, so as to solve the above-mentioned problems existing in the prior art.
[0007] In order to achieve the above purpose, the following technical solutions are adopted:
[0008] The first object of the present invention is to provide a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0009] (a) providing fibers made from modified polyolefins;
[0010] (b) performing a multi-stage sulfonation treatment on the fiber using an acid, and performing a multi-stage drafting treatment during the multi-stage sulfonation treatment to obtain an infusible fiber;
[0011] The infusible fiber is washed with water to obtain washed fiber;
[0012] (c) the washed fiber is subjected to oiling treatment to obtain oiled fiber;
[0013] (d) the oiled fiber is passed through a drying hot roller to obtain a dry fiber;
[0014] (e) performing carbonization treatment on the dried fibers, and adopting a multi-stage drawing process during the carbonization process to obtain continuous polyolefin-based carbon fibers.
[0015] Further, based on the above technical solution of the present invention, in step (a), the modified polyolefin is obtained by modifying the polyolefin using a polyolefin compatibilizer;
[0016] Preferably, the polyolefin to be modified includes polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, poly-4-methyl-1-pentene, poly-1-hexene, poly-3-methylbutene-1, polybutadiene, polyisoprene, polydicyclopentadiene, polyethylene norbornene, polyethylene norbornene homopolymer and carbon nanofiller modified products thereof, binary, ternary, multi-component copolymers containing the above homopolymer structural units and carbon nanofiller modified products thereof or one or more thereof; further preferably, the mass fraction of the carbon nanofiller in the carbon nanofiller modified product of the polyolefin homopolymer or the carbon nanofiller modified product of the polyolefin copolymer is 0-5%;
[0017] Preferably, the polyolefin compatibilizer is a modified product obtained by grafting a polar monomer onto a polyolefin, wherein the polar monomer comprises at least one of maleic anhydride, acrylic acid, α-methacrylic acid, acrylamide, glycidyl methacrylate or styrene, and the polyolefin comprises polyethylene or polypropylene;
[0018] Preferably, the mass fraction of the polyolefin compatibilizer in the modified polyolefin is 0.5-20%.
[0019] Further, on the basis of the above technical solution of the present invention, in step (b), the multi-stage sulfonation treatment comprises sequentially using 1 to 3 levels of concentrated acid baths for concentrated acid treatment and using 2 to 5 levels of dilute acid baths for dilute acid treatment;
[0020] Preferably, in step (b), when the concentrated acid treatment is performed in two or three concentrated acid baths in the multi-stage sulfonation treatment, the draft ratio used in the third concentrated acid bath is smaller than the draft ratio used in the second concentrated acid bath, and the draft ratio used in the second concentrated acid bath is smaller than the draft ratio used in the first concentrated acid bath;
[0021] Preferably, in step (b), the acid used in the multi-stage sulfonation treatment includes sulfuric acid.
[0022] Further, on the basis of the above technical solution of the present invention, in step (b), when a concentrated acid bath is used for concentrated acid treatment, the concentration of the concentrated acid used in the concentrated acid bath is 95-99%, the temperature is 110-160°C, the draft ratio is 50-320%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 90-100%; preferably, the concentration of the concentrated acid used in the concentrated acid bath is 97.5-98.5%, the temperature is 120-140°C, and the draft ratio is 90-300%; the degree of sulfonation of the fiber in the first concentrated acid bath is 95-100%;
[0023] Or, in step (b), when two-stage concentrated acid baths are used for concentrated acid treatment, the concentration of concentrated acid used in the first stage concentrated acid bath is 95-99%, the temperature is 50-120°C, the draft ratio is 60-200%, and the degree of sulfonation of the fiber in the first stage concentrated acid bath is 20-70%; the concentration of concentrated acid used in the second stage concentrated acid bath is 95-99%, the temperature is 100-160°C, the draft ratio is 50-180%, the degree of sulfonation of the fiber in the second stage concentrated acid bath is 90-100%, and the draft ratio used in the second stage concentrated acid bath is less than that used in the first stage concentrated acid bath. The draft ratio used; preferably, the concentration of the concentrated acid used in the first concentrated acid bath is 97.5-98.5%, the temperature is 60-110°C, the draft ratio is 70-150%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 30%-50%; the concentration of the concentrated acid used in the second concentrated acid bath is 97.5-98.5%, the temperature is 100-145°C, the draft ratio is 50-130%, the degree of sulfonation of the fiber in the second concentrated acid bath is 95-100%, and the draft ratio used in the second concentrated acid bath is less than the draft ratio used in the first concentrated acid bath;
[0024] Or, in step (b), when three-stage concentrated acid baths are used for concentrated acid treatment, the concentration of concentrated acid used in the first-stage concentrated acid bath is 95-99%, the temperature is 50-120°C, the draft ratio is 60-200%, and the degree of sulfonation of the fiber in the first-stage concentrated acid bath is 10-50%; the concentration of concentrated acid used in the second-stage concentrated acid bath is 95-99%, the temperature is 100-160°C, the draft ratio is 40-180%, and the degree of sulfonation of the fiber in the second-stage concentrated acid bath is 40-70%; the concentration of concentrated acid used in the third-stage concentrated acid bath is 95-99%, the temperature is 100-160°C, the draft ratio is 30-120%, the degree of sulfonation of the fiber in the third-stage concentrated acid bath is 90-100%, and the draft ratio used in the third-stage concentrated acid bath is less than the draft ratio used in the second-stage concentrated acid bath, and the draft ratio used in the second-stage concentrated acid bath is less than the draft ratio used in the first-stage concentrated acid bath. Draft ratio; preferably, the concentration of concentrated acid used in the first concentrated acid bath is 97.5-98.5%, the temperature is 60-110 ° C, the draft ratio is 70-150%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 20-40%; the concentration of concentrated acid used in the second concentrated acid bath is 97.5-98.5%, the temperature is 100-145 ° C, the draft ratio is 40-130%, and the fiber in the second concentrated acid bath is The degree of sulfonation is 50-70%; the concentration of concentrated acid used in the third concentrated acid bath is 97.5-98.5%, the temperature is 100-145°C, the draft ratio is 30-80%, and the degree of sulfonation of the fiber in the third concentrated acid bath is 95-100%; and the draft ratio used in the third concentrated acid bath is less than the draft ratio used in the second concentrated acid bath, and the draft ratio used in the second concentrated acid bath is less than the draft ratio used in the first concentrated acid bath.
[0025] Further, on the basis of the above technical solution of the present invention, in step (b), when two-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first-stage dilute acid bath is 60-90%, the temperature is 15-120°C, and the draft ratio is 70-150%; the concentration of the dilute acid used in the second-stage dilute acid bath is 30-60%, the temperature is 15-90°C, and the draft ratio is 70-120%; the residence time of the fiber in the first-stage dilute acid bath and the second-stage dilute acid bath is independently 10-60min;
[0026] Or, in step (b), when three-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first stage dilute acid bath is 70-90%, the temperature is 15-120°C, and the draft ratio is 80-140%; the concentration of the dilute acid used in the second stage dilute acid bath is 50-70%, the temperature is 15-100°C, and the draft ratio is 80-120%; the concentration of the dilute acid used in the third stage dilute acid bath is 30-50%, the temperature is 15-80°C, and the draft ratio is 80-110%; the residence time of the fiber in the first stage dilute acid bath, the second stage dilute acid bath and the third stage dilute acid bath is independently 10-60 min;
[0027] Or, in step (b), when four-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first-stage dilute acid bath is 75-90%, the temperature is 15-120°C, and the draft ratio is 90-130%; the concentration of the dilute acid used in the second-stage dilute acid bath is 60-75%, the temperature is 15-100°C, and the draft ratio is 90-110%; the concentration of the dilute acid used in the third-stage dilute acid bath is 45-60%, the temperature is 15-80°C, and the draft ratio is 90-110%; the concentration of the dilute acid used in the fourth-stage dilute acid bath is 30-45%, the temperature is 15-60°C, and the draft ratio is 90-110%; the residence time of the fiber in the first-stage dilute acid bath, the second-stage dilute acid bath, the third-stage dilute acid bath and the fourth-stage dilute acid bath is independently 10-60 min;
[0028] Or, in step (b), when 5 levels of dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first level dilute acid bath is 80-90%, the temperature is 15-120° C., and the draft ratio is 95-120%; the concentration of the dilute acid used in the second level dilute acid bath is 70-80%, the temperature is 15-100° C., and the draft ratio is 95-120%; the concentration of the dilute acid used in the third level dilute acid bath is 60-70%, the temperature is 15-80° C., and the draft ratio is 95-110%; the concentration of the dilute acid used in the fourth level dilute acid bath is 40-60%, the temperature is 15-60° C., and the draft ratio is 95-110%; the concentration of the dilute acid used in the fifth level dilute acid bath is 20-40%, the temperature is 15-40° C., and the draft ratio is 95-110%. The residence time of the fiber in the first dilute acid bath, the second dilute acid bath, the third dilute acid bath, the fourth dilute acid bath and the fifth dilute acid bath is independently 10-60 minutes.
[0029] Furthermore, based on the above technical solution of the present invention, in step (b), the infusible fiber is subjected to multi-stage water washing, the water flow rate is opposite to the transmission direction of the infusible fiber, the water washing temperature is 15-90°C, and the drawing ratio of each stage of water washing is independently 90-130%.
[0030] Further, on the basis of the above technical solution of the present invention, in step (c), the oil agent used for oiling treatment includes a main agent and a solvent, and the main agent in the oil agent includes at least one of modified silicone oil, nonionic material, polycationic material or polyanionic material;
[0031] Preferably, the modified silicone oil includes at least one of amino-modified silicone oil, polyether-modified silicone oil or epoxy-modified silicone oil;
[0032] Preferably, the nonionic material comprises at least one of polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene glycol or polyacrylamide;
[0033] Preferably, the polycationic material comprises at least one of polyamine, polyquaternium-5, polyquaternium-6, polyquaternium-7, polyquaternium-39, polyquaternium-1, polyquaternium-51, polyquaternium-47, polyquaternium-44, polyquaternium-22, polyquaternium-11, polyquaternium-28, polyquaternium-6, polyquaternium-32, polyquaternium-63, polyquaternium-33, polyvinylamine, cationic polyacrylamide, polyethyleneimine, cationic waterborne polyurethane or polydiallyldimethylammonium chloride;
[0034] Preferably, the polyanionic material comprises at least one of sodium carboxymethylcellulose, polyacrylic acid, poly(methyl methacrylate), polyacrylamide or poly(styrene sulfonic acid) or anionic polyacrylamide);
[0035] Preferably, the concentration of the main agent in the oil agent is 0.1-2.5wt%.
[0036] Further, on the basis of the above technical solution of the present invention, in step (d), the oiled fiber passes through a multi-stage drying hot roller, the temperature of the drying hot roller is 30-150° C., and the draft ratio is 50-98%;
[0037] Preferably, the temperature of the drying hot roller is 30-60° C., and the draft ratio is 50-98%.
[0038] Furthermore, on the basis of the above technical solution of the present invention, in step (e), the dry fiber is carbonized at 200-3000°C in an inert atmosphere; the stretching ratio at 200-700°C is 70-130%, the stretching ratio at >700-900°C is 80-120%, the stretching ratio at >900-1500°C is 90-115%, and the stretching ratio at >1500-3000°C is 100-115%.
[0039] The second object of the present invention is to provide a continuous polyolefin-based carbon fiber, which is prepared by the preparation method of the continuous polyolefin-based carbon fiber provided by the first object of the present invention.
[0040] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:
[0041] (1) The present invention provides a method for preparing continuous polyolefin-based carbon fibers, wherein the continuous polyolefin-based carbon fibers are prepared by first subjecting fibers made of modified polyolefins to multi-stage sulfonation treatment, water washing, oiling, hot roller drying, and then carbonization treatment. Since the structure and mechanical properties of polyolefin fibers are in a dynamic change process during the multi-stage sulfonation and carbonization treatments, the present invention mainly uses multi-stage stretching treatments in the multi-stage sulfonation and carbonization treatments to make the applied stretching tension change with the evolution of the fiber structure and properties during the preparation process, thereby facilitating the improvement of the carbon fiber microstructure and the improvement of the mechanical properties.
[0042] (2) The present invention provides a continuous polyolefin-based carbon fiber, which is prepared by the above-mentioned preparation method of the continuous polyolefin-based carbon fiber provided by the present invention. In view of the advantages of the above-mentioned preparation method of the present invention, the prepared continuous polyolefin-based carbon fiber has good microstructure and mechanical properties. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0044] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0045] According to a first aspect of the present invention, there is provided a method for preparing a continuous polyolefin-based carbon fiber, comprising the following steps:
[0046] (a) providing fibers made from modified polyolefins;
[0047] (b) performing a multi-stage sulfonation treatment on the fiber using an acid, and performing a multi-stage drafting treatment during the multi-stage sulfonation treatment to obtain an infusible fiber;
[0048] The infusible fiber is washed with water to obtain washed fiber;
[0049] (c) the washed fiber is subjected to oiling treatment to obtain oiled fiber;
[0050] (d) the oiled fiber is passed through a drying hot roller to obtain a dry fiber;
[0051] (e) performing carbonization treatment on the dried fibers, and adopting a multi-stage drawing process during the carbonization process to obtain continuous polyolefin-based carbon fibers.
[0052] Specifically, in step (a), the modified polyolefin is obtained by modifying the polyolefin with a modifier. The type of polyolefin is not specifically limited, and common polyolefin types in the art can be used, such as polyethylene, polypropylene, polybutylene, polyisobutylene, polypentene, etc. Modification of the polyolefin can increase the compatibility of the sulfonation agent and the polyolefin in the subsequent sulfonation process, and reduce stress cracking or defects caused by the compatibility difference between the sulfonated polyolefin and the polyolefin in the sulfonation process (infusible process) of the polyolefin fiber.
[0053] The specific steps of preparing the fiber from the modified polyolefin are not limited, and the fiber can be prepared by a common spinning method in the art.
[0054] In step (b), the sulfonation treatment (infusibility treatment) refers to the use of an acid as a sulfonation agent to crosslink the modified polyolefin to form a conjugated polyolefin structure that is infusible at high temperatures. The purpose of the multi-stage drafting in the sulfonation stage (infusibility stage) is to dynamically match the drafting force according to the evolution mechanism of the fiber structure and mechanical properties during the sulfonation process, improve the orientation of the fiber, and optimize the structure and performance of the fiber.
[0055] The oiling treatment in step (c) is to attach a protective layer to the surface of the washed fiber to prevent adhesion between the monofilaments during drying and subsequent carbonization.
[0056] In step (d), the oiled fibers are treated with a drying hot roller, mainly to remove the solvent in the oil.
[0057] The purpose of the multi-stage drawing in the carbonization stage of step (e) is to dynamically match the drawing force according to the evolution mechanism of the fiber structure and mechanical properties during the carbonization process, improve the orientation of the graphite crystallites of the fiber, and optimize the structure and properties of the carbon fiber.
[0058] After a lot of experimental research, the inventors of the present invention found that the structure and properties of carbon fiber are closely related to the temperature, sulfonation degree (or time), tension, etc. during the sulfonation and carbonization process. Coordinated regulation of the balance between the several factors is the key to improving the mechanical properties of carbon fiber.
[0059] The present invention provides a method for preparing continuous polyolefin-based carbon fibers, wherein the continuous polyolefin-based carbon fibers are prepared by first subjecting fibers made of modified polyolefins to multi-stage sulfonation treatment, water washing, oiling treatment, hot roller drying, and then carbonization treatment. Since the structure and mechanical properties of polyolefin fibers are in a dynamic change process during the multi-stage sulfonation treatment and carbonization treatment, the present invention supplements the multi-stage sulfonation treatment and carbonization treatment with multi-stage drafting treatment, so that the applied drafting tension changes with the evolution of the fiber structure and properties during the preparation process, thereby facilitating the improvement of the microstructure of the carbon fibers and the improvement of the mechanical properties.
[0060] As an optional embodiment of the present invention, in step (a), the modified polyolefin is obtained by modifying the polyolefin using a polyolefin compatibilizer.
[0061] As an optional embodiment of the present invention, the polyolefin includes one or more of polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, poly-4-methyl-1-pentene, poly-1-hexene, poly-3-methylbutene-1, polybutadiene, polyisoprene, polydicyclopentadiene, polyethylene norbornene, polyethylene norbornene homopolymers and carbon nanofiller modified products thereof, binary, ternary, and multi-polymers containing the above homopolymer structural units (for example, ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-pentene copolymers, ethylene-butene-pentene copolymers, ethylene-propylene-butene copolymers, ethylene-propylene-ene-pentene copolymers, etc.) and carbon nanofiller modified products thereof. The carbon nanofiller-modified product of the above-mentioned polyolefin homopolymer or the carbon nanofiller-modified product of the above-mentioned polyolefin copolymer mainly refers to the modified product obtained by modifying the polyolefin homopolymer or polyolefin copolymer with carbon nanofillers (carbon nanotubes, alkyl-modified carbon nanotubes, siloxane-modified carbon nanotubes, graphene nanosheets, alkyl-modified graphene nanosheets, siloxane-modified graphene nanosheets, graphene oxide, graphite, etc.).
[0062] As an optional embodiment of the present invention, the mass fraction of the carbon nanofiller in the carbon nanofiller-modified product of the homopolymer or the carbon nanofiller-modified product of the copolymer is 0-5%.
[0063] As an optional embodiment of the present invention, the polyolefin compatibilizer is a modified product obtained by grafting and modifying polyolefin with a polar monomer (maleic anhydride, acrylic acid, α-methacrylic acid, acrylamide, glycidyl methacrylate or styrene, etc.), and the polyolefin in the grafted modified polyolefin includes polyethylene or polypropylene. For example, the polyolefin compatibilizer includes at least one of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, acrylic acid grafted polyethylene, acrylic acid grafted polypropylene, α-methacrylic acid grafted polyethylene, α-methacrylic acid grafted polypropylene, acrylamide grafted polyethylene, acrylamide grafted polypropylene, glycidyl methacrylate grafted polyethylene, glycidyl methacrylate grafted polypropylene, styrene grafted polyethylene or styrene grafted polypropylene, etc.
[0064] As an optional embodiment of the present invention, the mass fraction of the polyolefin compatibilizer in the modified polyolefin is 0.5-20%. Typical but non-limiting mass fractions are 0.5%, 1%, 2%, 4%, 5%, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%.
[0065] By further limiting the specific type and amount of the polyolefin compatibilizer, the compatibility of the polyolefin and the sulfonated reagent is improved while the spinnability of the polyolefin and the strength of the polyolefin fiber are not damaged.
[0066] As an optional embodiment of the present invention, in step (b), the multi-stage sulfonation treatment includes sequentially using 1 to 3 levels (e.g., 1, 2 or 3 levels, etc.) of concentrated acid baths for concentrated acid treatment and using 2 to 5 levels (e.g., 2, 3, 4 or 5 levels, etc.) of dilute acid baths for dilute acid treatment.
[0067] As an optional embodiment of the present invention, in step (b), when a multi-stage (e.g., 2-stage or 3-stage, etc.) concentrated acid bath is used for concentrated acid treatment in the multi-stage sulfonation treatment, the draft ratio gradually decreases with the increase in the number of concentrated acid bath treatment stages, that is, the draft ratio used in the third-stage concentrated acid bath is smaller than the draft ratio used in the second-stage concentrated acid bath, and the draft ratio used in the second-stage concentrated acid bath is smaller than the draft ratio used in the first-stage concentrated acid bath.
[0068] As an optional embodiment of the present invention, in step (b), the acid used in the multi-stage sulfonation treatment includes sulfuric acid.
[0069] As an optional embodiment of the present invention, in step (b), when a first-level concentrated acid bath is used for concentrated acid treatment, the concentration of the concentrated acid used in the concentrated acid bath is 95-99%, the temperature is 110-160° C., and the draft ratio is 50-320% (for example, 50%, 60%, 80%, 90%, 100%, 120%, 150%, 160%, 180%, 200%, 220%, 250%, 260%, 280%, 290%, 300%, 310%, 320%, 330%, 340%, 360%, 370%, 380%, 390%, 400%, 410%, 420%, 430%, 440%, 450%, 460%, 470%, 480%, 490%, 500%, 510%, 520%, 530%, 540%, 550%, 560%, 570%, 580%, 590%, 600%, 610%, 610%, 620%, 630%, 640%, 650%, 660%, 670%, 680%, 690%, 700%, 710%, 720%, 730%, 740%, 750%, 760%, 770%, 780%, 790%, 80 ... 0%, 300% or 320%, etc.), the degree of sulfonation of the fiber in the primary concentrated acid bath is 90-100% (for example, 90%, 92%, 94%, 95%, 96%, 98% or 100%, etc.); preferably, the concentration of the concentrated acid used in the concentrated acid bath is 97.5-98.5%, the temperature is 120-140°C, and the draft ratio is 90-300%; the degree of sulfonation of the fiber in the primary concentrated acid bath is 95-100%;
[0070] Or, in step (b), when two-stage concentrated acid baths are used for concentrated acid treatment, the concentration of concentrated acid used in the first stage concentrated acid bath is 95-99%, the temperature is 50-120° C., the draft ratio is 60-200% (for example, 60%, 70%, 80%, 90%, 100%, 120%, 130%, 150%, 160%, 180% or 200%, etc.), and the fiber in the first stage concentrated acid bath is The degree of sulfonation is 20-70% (for example, 20%, 30%, 40%, 50%, 60% or 70%, etc.); the concentration of concentrated acid used in the second concentrated acid bath is 95-99%, the temperature is 100-160°C, and the draft ratio is 50-180% (for example, 50%, 60%, 70%, 80%, 90%, 100%, 120%, 130%, 150%, 160% or 180%). 0%, etc.), the degree of sulfonation of the fiber in the second concentrated acid bath is 90-100% (for example, 90%, 92%, 94%, 95%, 96%, 98% or 100%, etc.), and the draft ratio adopted by the second concentrated acid bath is less than the draft ratio adopted by the first concentrated acid bath; preferably, the concentration of the concentrated acid adopted by the first concentrated acid bath is 97.5-98.5%, the temperature is 60-110°C, the draft ratio is 70-150%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 30%-50%; the concentration of the concentrated acid adopted by the second concentrated acid bath is 97.5-98.5%, the temperature is 100-145°C, the draft ratio is 50-130%, the degree of sulfonation of the fiber in the second concentrated acid bath is 95-100%, and the draft ratio adopted by the second concentrated acid bath is less than the draft ratio adopted by the first concentrated acid bath;
[0071] Or, in step (b), when three-stage concentrated acid baths are used for concentrated acid treatment, the concentration of concentrated acid used in the first stage concentrated acid bath is 95-99%, the temperature is 50-120° C., the draft ratio is 60-200% (for example, 60%, 70%, 80%, 90%, 100%, 120%, 130%, 150%, 160%, 180% or 200%, etc.), and the degree of sulfonation of the fiber in the first stage concentrated acid bath is 10-50% (for example, 10%, 20%, 30%, 40% or 50%, etc.); the concentration of concentrated acid used in the second stage concentrated acid bath is 95-99%, the temperature is 100 -160 ℃, the draft ratio is 40-180% (for example, 40%, 50%, 60%, 70%, 80%, 90%, 100%, 120%, 130%, 150%, 160% or 180%, etc.), the degree of sulfonation of the fiber in the second concentrated acid bath is 40-70% (for example, 40%, 50%, 60% or 70%, etc.); the concentration of concentrated acid used in the third concentrated acid bath is 95-99%, the temperature is 100-160 ℃, the draft ratio is 30-120% (for example, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100% or 120%, etc.), the degree of sulfonation of the fiber in the third concentrated acid bath is 90-100% (for example, 90%, 92%, 94%, 95%, 96%, 98% or 100%, etc.), and the draft ratio used in the third concentrated acid bath is less than the draft ratio used in the second concentrated acid bath, and the draft ratio used in the second concentrated acid bath is less than the draft ratio used in the first concentrated acid bath; preferably, the concentration of the concentrated acid used in the first concentrated acid bath is 97.5-98.5%, the temperature is 60-110°C, the draft ratio is 70-150%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 20-40%; the second concentrated acid bath is The concentrated acid used in the concentrated acid bath has a concentration of 97.5-98.5%, a temperature of 100-145°C, a draft ratio of 40-130%, and a sulfonation degree of the fiber in the second concentrated acid bath of 50-70%; the concentrated acid used in the third concentrated acid bath has a concentration of 97.5-98.5%, a temperature of 100-145°C, a draft ratio of 30-80%, and a sulfonation degree of the fiber in the third concentrated acid bath of 95-100%; and the draft ratio used in the third concentrated acid bath is smaller than the draft ratio used in the second concentrated acid bath, and the draft ratio used in the second concentrated acid bath is smaller than the draft ratio used in the first concentrated acid bath.
[0072] It should be noted that the draft ratio in the present invention refers to the ratio of the linear speeds of two adjacent winding rollers in the process of preparing continuous fibers.
[0073] The sulfonation process is a process in which the sulfonation reaction gradually advances from the fiber surface to the fiber interior. The sulfonation degree of the fiber in the concentrated acid bath refers to the ratio of the thickness (or depth) of the sulfonation reaction on the polyolefin fiber surface to the diameter of the polyolefin fiber.
[0074] As an optional embodiment of the present invention, in step (b), when two-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first-stage dilute acid bath is 60-90%, the temperature is 15-120°C, and the draft ratio is 70-150% (for example, 70%, 80%, 90%, 100%, 120%, 130% or 150%, etc.); the concentration of the dilute acid used in the second-stage dilute acid bath is 30-60%, the temperature is 15-90°C, and the draft ratio is 70-120% (for example, 70%, 80%, 90%, 100% or 120%, etc.); the residence time of the fiber in the first-stage dilute acid bath and the second-stage dilute acid bath is independently 10-60 min (for example, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min, etc.);
[0075] Or, in step (b), when three-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first stage dilute acid bath is 70-90%, the temperature is 15-120° C., and the draft ratio is 80-140% (for example, 80%, 90%, 100%, 120%, 130% or 140%, etc.); the concentration of the dilute acid used in the second stage dilute acid bath is 50-70%, the temperature is 15-100° C., and the draft ratio is 80-120% (for example, 80%, 90%, 100%, 120%, 130% or 140%, etc.). 110% or 120%, etc.); the concentration of the dilute acid used in the third dilute acid bath is 30-50%, the temperature is 15-80°C, and the draft ratio is 80-110% (for example, 80%, 90%, 100% or 110%, etc.); the residence time of the fiber in the first dilute acid bath, the second dilute acid bath and the third dilute acid bath is independently 10-60min (for example, 10min, 20min, 30min, 40min, 50min or 60min, etc.);
[0076] Or, in step (b), when four-stage dilute acid bath is used for dilute acid treatment, the concentration of the dilute acid used in the first stage dilute acid bath is 75-90%, the temperature is 15-120°C, and the draft ratio is 90-130% (for example, 90%, 100%, 110%, 120% or 130%, etc.); the concentration of the dilute acid used in the second stage dilute acid bath is 60-75%, the temperature is 15-100°C, and the draft ratio is 90-110% (for example, 90%, 100% or 110%, etc.); the concentration of the dilute acid used in the third stage dilute acid bath is 45-60%, the temperature is 15 -80℃, the draft ratio is 90-110% (for example, 90%, 100% or 110%); the concentration of the dilute acid used in the fourth dilute acid bath is 30-45%, the temperature is 15-60℃, and the draft ratio is 90-110% (for example, 90%, 100% or 110%); the residence time of the fiber in the first dilute acid bath, the second dilute acid bath, the third dilute acid bath and the fourth dilute acid bath is independently 10-60min (for example, 10min, 20min, 30min, 40min, 50min or 60min);
[0077] Or, in step (b), when five levels of dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first level of dilute acid bath is 80-90%, the temperature is 15-120° C., and the draft ratio is 95-120% (for example, 95%, 100%, 110% or 120%, etc.); the concentration of the dilute acid used in the second level of dilute acid bath is 70-80%, the temperature is 15-100° C., and the draft ratio is 95-120% (for example, 95%, 100%, 110% or 120%, etc.); the concentration of the dilute acid used in the third level of dilute acid bath is 60-70%. , the temperature is 15-80℃, and the draft ratio is 95-110% (for example, 95%, 100%, 105% or 110%); the concentration of the diluted acid used in the fourth dilute acid bath is 40-60%, the temperature is 15-60℃, and the draft ratio is 95-110% (for example, 95%, 100%, 105% or 110%); the concentration of the diluted acid used in the fifth dilute acid bath is 20-40%, the temperature is 15-40℃, and the draft ratio is 95-110% (for example, 95%, 100%, 105% or 110%). The residence time of the fiber in the first dilute acid bath, the second dilute acid bath, the third dilute acid bath, the fourth dilute acid bath and the fifth dilute acid bath is 10-60min respectively.
[0078] By specifically limiting the multi-stage stretching treatment steps in the sulfonation stage, the coordinated regulation of fiber mechanical properties, temperature, stretching tension, etc. can be achieved, which can improve the graphite crystallite orientation of polyolefin-based carbon fibers and enhance the mechanical properties of polyolefin-based carbon fibers.
[0079] As an optional embodiment of the present invention, in step (b), the infusible fiber undergoes multi-stage water washing, the water flow rate is opposite to the direction of transmission of the infusible fiber, the water washing temperature is 15-90°C, and the drawing ratio of each stage of water washing is independently 90-130% (for example, 90%, 100%, 110%, 120% or 130%, etc.).
[0080] As an optional embodiment of the present invention, in step (c), the oil agent used for oiling treatment is usually prepared in the form of a main agent + solvent, and the main agent in the oil agent includes modified silicone oil (for example, amino-modified silicone oil, polyether-modified silicone oil, epoxy-modified silicone oil), non-ionic materials (for example, polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, polyacrylamide, etc.), polycationic materials (for example, polyacrylamine, polyamine, polyquaternary ammonium salt-5, polyquaternary ammonium salt-6, polyquaternary ammonium salt-7, polyquaternary ammonium salt-39, polyquaternary ammonium salt-1, polyquaternary ammonium salt -51, polyquaternium-47, polyquaternium-44, polyquaternium-22, polyquaternium-11, polyquaternium-28, polyquaternium-6, polyquaternium-32, polyquaternium-63, polyquaternium-33, polyethylene amine, polyethylene imine, cationic polyacrylamide, cationic water-based polyurethane or polydiallyldimethylammonium chloride, etc.), polyanionic materials (for example, sodium carboxymethyl cellulose, polyacrylic acid, poly (methyl methacrylate), poly (styrene sulfonic acid), anionic polyacrylamide, etc.) at least one.
[0081] Among them, polyacrylamide (PAM) itself is a non-ionic polymer. However, it can form different types of ionic polymers through copolymerization or modification: (1) Cationic polyacrylamide (CPAM): prepared by introducing cationic monomers (such as methacryloyloxyethyl trimethyl ammonium chloride, DMC), which is used in water treatment for sludge dewatering and flocculation of suspended particles in water; (2) Anionic polyacrylamide (APAM): prepared by introducing anionic monomers (such as sodium acrylate or acrylic acid), which is used in water treatment for flocculation of suspended particles and sewage treatment.
[0082] As an optional embodiment of the present invention, in step (c), the type of solvent in the oil solution is not limited, and for example, water can be selected.
[0083] By further limiting the specific types of the main agent in the oil agent, the antistatic properties and softness of the sulfonated fiber can be better regulated.
[0084] As an optional embodiment of the present invention, in step (c), the mass concentration of the main agent in the oil agent is 0.1-2.5wt%, and a typical but non-limiting concentration is 0.1wt%, 0.2wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.8wt%, 1.0wt%, 1.2wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.4wt% or 2.5wt%, etc.
[0085] By limiting the type and concentration of the oil used in the oiling process, the sulfonated polyolefin fiber has good fiber opening performance after drying, ensuring that the sulfonated polypropylene fiber does not stick and twist during the subsequent carbonization process.
[0086] As an optional embodiment of the present invention, in step (d), the oiled fiber passes through a multi-stage drying hot roller, the temperature of the drying hot roller is 30-150°C, the stretch ratio is 50-98%, and the residence time on the drying hot roller is independently 5min-60min; the typical but restrictive temperature of the drying hot roller is 30°C, 40°C, 50°C, 60°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, etc., and the typical but restrictive stretch ratio is 50%, 60%, 70%, 80%, 90%, 95% or 98%, etc.
[0087] As a preferred embodiment of the present invention, in step (d), the temperature of the drying hot roller is 30-60° C., and the draft ratio is 50-98%.
[0088] As an optional embodiment of the present invention, in step (e), the dried fiber is carbonized at 200-3000° C. in an inert atmosphere; the draft ratio at 200-700° C. is 70-130% (for example, 70%, 80%, 90%, 100%, 110%, 120% or 130%, etc.), the draft ratio at >700-900° C. is 80-120% (for example, 80%, 90%, 100%, 110% or 120%, etc.), and the draft ratio at >900-900° C. is 100-120% (for example, 100%, 110%, 120%, etc.). The drawing ratio at 1500°C is 90-115% (for example, 90%, 100%, 110% or 115%, etc.), and the drawing ratio at >1500-3000°C is 100-115% (for example, 100%, 105%, 110% or 115%, etc.); the carbonization treatment of the dry fiber at 200-700°C, >700-900°C, >900-1500°C, >1500-3000°C is to directly enter the carbonization furnace at a specific temperature for carbonization.
[0089] >700~900℃ refers to temperatures between 700℃ and 900℃ but not including 700℃. Similarly, >900~1500℃ refers to temperatures between 900℃ and 1500℃ but not including 900℃. >1500~3000℃ refers to temperatures between 1500℃ and 3000℃ but not including 1500℃.
[0090] According to a second aspect of the present invention, there is also provided a continuous polyolefin-based carbon fiber, which is prepared by the method for preparing the continuous polyolefin-based carbon fiber provided by the first aspect of the present invention.
[0091] In view of the advantages of the above-mentioned preparation method of the present invention, the prepared continuous polyolefin-based carbon fiber has good microstructure and mechanical properties.
[0092] The present invention is further described in detail below in conjunction with specific examples and comparative examples. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Unless otherwise specified, the raw materials used in the present invention can all be obtained from commercially available products. Specific raw material information is shown in Table 1.
[0093] Table 1
[0094]
[0095]
[0096] Example 1
[0097] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0098] (a) providing fibers made from modified polyolefins;
[0099] 50 wt% of polyethylene, 40 wt% of polybutene, 9.5 wt% of polyisobutylene, and 0.5 wt% of maleic anhydride grafted polypropylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, pelletized, and dried to obtain a modified polyolefin;
[0100] The modified polyolefin was placed in a melt spinning machine to prepare 15 μm fully drawn yarns, the spinning temperature was 200° C., the speed of the yarn collection roller was 2500 r / min, and fibers were obtained.
[0101] (b) subjecting the fiber to a sulfonation treatment in two-stage concentrated acid bath and two-stage dilute acid bath, respectively, wherein the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drafting treatment is used during the sulfonation treatment to obtain an infusible fiber;
[0102] The first concentrated acid bath has a concentration of 98%, a temperature of 50°C, a draft ratio of 180%, and a sulfonation degree of the fiber in the first concentrated acid bath of 40%. The second concentrated acid bath has a concentration of 95%, a temperature of 120°C, a draft ratio of 150%, and a sulfonation degree of the fiber in the second concentrated acid bath of 95%. The first diluted acid bath has a concentration of 60%, a temperature of 120°C, and a draft ratio of 150%. The second diluted acid bath has a concentration of 30%, a temperature of 90°C, and a draft ratio of 70%. The residence time of the fiber in the first diluted acid bath and the second diluted acid bath is 10 minutes and 30 minutes, respectively.
[0103] The infusible fiber is washed in a two-stage washing tank and stretched to obtain washed fiber; wherein the first stage washing temperature is 90°C and the stretching ratio is 90%; the second stage washing temperature is 50°C and the stretching ratio is 100%; the residence time of the fiber in the first stage washing and the second stage washing is 20 minutes and 60 minutes respectively.
[0104] (c) treating the washed fiber with oil in an oil tank to obtain oiled fiber; wherein the oil is an aqueous solution of amino-modified silicone oil, and the concentration of the amino-modified silicone oil in the oil is 0.1 wt %.
[0105] (d) The oiled fiber is successively passed through two stages of drying hot rollers to obtain dry fiber; the temperature of the first stage drying hot roller is 30°C, and the draft ratio is 50%; the temperature of the second stage drying hot roller is 50°C, and the draft ratio is 98%; the drying hot roller time of the fiber on the first stage drying hot roller and the second stage drying hot roller is 10 min and 20 min, respectively.
[0106] (e) The dried fibers are carbonized in a nitrogen atmosphere at a temperature ranging from 200 to 1500° C. to obtain continuous polyolefin-based carbon fibers; wherein the drawing ratio at 200 to 700° C. is 100%, the drawing ratio at temperatures >700 to 900° C. is 120%, and the drawing ratio at temperatures >900 to 1500° C. is 115%.
[0107] Example 2
[0108] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0109] (a) providing fibers made from modified polyolefins;
[0110] 70 wt% of polypropylene, 10 wt% of polypentene, 10 wt% of poly-4-methyl-1-pentene and 10 wt% of maleic anhydride grafted polyethylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, pelletized and dried to obtain a modified polyolefin;
[0111] The modified polyolefin was placed in a melt spinning machine to prepare 7 μm fully drawn yarns, the spinning temperature was 180° C., the speed of the yarn collection roller was 3000 r / min, and fibers were obtained.
[0112] (b) subjecting the fiber to sulfonation treatment in three-stage concentrated acid bath and five-stage dilute acid bath, respectively, wherein the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drafting treatment is used during the sulfonation treatment to obtain an infusible fiber;
[0113] The first concentrated acid bath has a concentration of 98%, a temperature of 50°C, a draft ratio of 200%, and a sulfonation degree of the fiber in the first concentrated acid bath of 10%. The second concentrated acid bath has a concentration of 95%, a temperature of 120°C, a draft ratio of 180%, and a sulfonation degree of the fiber in the second concentrated acid bath of 60%. The third concentrated acid bath has a concentration of 98%, a temperature of 140°C, a draft ratio of 80%, and a sulfonation degree of the fiber in the third concentrated acid bath of 100%.
[0114] The concentration of the dilute acid used in the first dilute acid bath is 80%, the temperature is 120℃, and the draft ratio is 95%; the concentration of the dilute acid used in the second dilute acid bath is 70%, the temperature is 100℃, and the draft ratio is 100%; the concentration of the dilute acid used in the third dilute acid bath is 60%, the temperature is 50℃, and the draft ratio is 110%; the concentration of the dilute acid used in the fourth dilute acid bath is 40%, the temperature is 60℃, and the draft ratio is 110%; the concentration of the dilute acid used in the fifth dilute acid bath is 20%, the temperature is 30℃, and the draft ratio is 110%; the residence time of the fiber in the first dilute acid bath, the second dilute acid bath, the third dilute acid bath, the fourth dilute acid bath and the fifth dilute acid bath are 10min, 10min, 20min, 30min and 60min respectively.
[0115] The infusible fiber is washed in a 5-stage washing tank and stretched to obtain washed fiber; wherein, the first stage washing temperature is 90°C and the stretching ratio is 90%; the second stage washing temperature is 80°C and the stretching ratio is 90%; the third stage washing temperature is 60°C and the stretching ratio is 100%; the fourth stage washing temperature is 40°C and the stretching ratio is 120%; the fifth stage washing temperature is 30°C and the stretching ratio is 130%; the residence time of the fiber in the first stage washing, the second stage washing, the third stage washing, the fourth stage washing and the fifth stage washing are 20min, 20min, 30min, 30min and 40min respectively.
[0116] (c) treating the washed fiber with oil in an oil tank to obtain oiled fiber; wherein the oil is an aqueous solution of polyether-modified silicone oil, and the concentration of the polyether-modified silicone oil in the oil is 1.5 wt %.
[0117] (d) The oiled fiber is successively passed through 5 stages of drying hot rollers to obtain dry fiber; the temperatures of the first stage drying hot roller, the second stage drying hot roller, the third stage drying hot roller, the fourth stage drying hot roller and the fifth stage drying hot roller are 30°C, 40°C, 45°C, 50°C and 55°C respectively, the drafting ratios are all 130%, and the drying hot roller times are 5 min, 5 min, 5 min, 10 min and 10 min respectively.
[0118] (e) The dried fibers are carbonized in an inert atmosphere at a temperature ranging from 200 to 3000° C. to obtain continuous polyolefin-based carbon fibers; wherein the draw ratio at 200 to 700° C. is 130%, the draw ratio at temperatures >700 to 900° C. is 100%, the draw ratio at temperatures >900 to 1500° C. is 90%, and the draw ratio at temperatures >1500 to 3000° C. is 115%.
[0119] Example 3
[0120] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0121] (a) providing fibers made from modified polyolefins;
[0122] 55 wt% of polyethylene, 15 wt% of poly-1-hexene, 10 wt% of poly-3-methylbutene and 20% of maleic anhydride grafted polyethylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, pelletized and dried to obtain a modified polyolefin;
[0123] The modified polyolefin was placed in a melt spinning machine to prepare 50 μm fully drawn yarns, the spinning temperature was 180° C., the speed of the yarn collection roller was 1000 r / min, and fibers were obtained.
[0124] (b) subjecting the fiber to sulfonation treatment in two-stage concentrated acid bath and three-stage dilute acid bath, respectively, wherein the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drafting treatment is used during the sulfonation treatment to obtain an infusible fiber;
[0125] The concentration of concentrated acid used in the first concentrated acid bath is 99%, the temperature is 70℃, the draft ratio is 150%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 20%; the concentration of concentrated acid used in the second concentrated acid bath is 98%, the temperature is 130℃, the draft ratio is 50%, and the degree of sulfonation of the fiber in the second concentrated acid bath is 98%. The concentration of diluted acid used in the first dilute acid bath is 80%, the temperature is 100℃, and the draft ratio is 140%; the concentration of diluted acid used in the second dilute acid bath is 50%, the temperature is 80℃, and the draft ratio is 120%. The concentration of diluted acid used in the third dilute acid bath is 30%, the temperature is 15℃, and the draft ratio is 110%. The residence time of the fiber in the first dilute acid bath, the second dilute acid bath, and the third dilute acid bath is 10min, 20min, and 25min, respectively.
[0126] The infusible fiber is washed in a three-stage washing tank and stretched to obtain washed fiber; wherein, the first stage washing temperature is 90°C and the stretching ratio is 100%; the second stage washing temperature is 70°C and the stretching ratio is 120%; the third stage washing temperature is 15°C and the stretching ratio is 130%; the residence time of the fiber in the first stage washing, the second stage washing and the third stage washing are 20min, 30min and 60min respectively.
[0127] (c) treating the washed fiber with oil in an oil tank to obtain oiled fiber; wherein the oil is an aqueous solution of epoxy-modified silicone oil, and the concentration of the epoxy-modified silicone oil in the oil is 1.0 wt %.
[0128] (d) The oiled fiber is successively passed through three stages of drying hot rollers to obtain dry fiber; the temperatures of the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller are 30°C, 40°C and 55°C, respectively, and the draft ratio is 120%; the drying hot roller time of the fiber on the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller is 5 min, 15 min and 20 min, respectively.
[0129] (e) subjecting the dried fibers to a carbonization treatment in an inert atmosphere within a temperature range of 200-700° C. to obtain continuous polyolefin-based carbon fibers; wherein the drawing ratio at 200-700° C. is 100%.
[0130] Example 4
[0131] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0132] (a) providing fibers made from modified polyolefins;
[0133] 95 wt% of polyethylene, 2 wt% of polybutadiene, 2 wt% of polyisoprene and 1% of maleic anhydride grafted polyethylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, pelletized and dried to obtain a modified polyolefin;
[0134] The modified polyolefin was placed in a melt spinning machine to prepare 30 μm fully drawn yarns, the spinning temperature was 190° C., the speed of the yarn collection roller was 1500 r / min, and fibers were obtained.
[0135] (b) subjecting the fiber to sulfonation treatment in three-stage concentrated acid bath and four-stage dilute acid bath, respectively, wherein the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drafting treatment is used during the sulfonation treatment to obtain an infusible fiber;
[0136] The first concentrated acid bath has a concentration of 98%, a temperature of 90°C, a draft ratio of 60%, and a sulfonation degree of the fiber in the first concentrated acid bath of 10%. The second concentrated acid bath has a concentration of 98%, a temperature of 150°C, a draft ratio of 50%, and a sulfonation degree of the fiber in the second concentrated acid bath of 40%. The third concentrated acid bath has a concentration of 98%, a temperature of 140°C, a draft ratio of 30%, and a sulfonation degree of the fiber in the third concentrated acid bath of 90%.
[0137] The concentration of the dilute acid used in the first dilute acid bath is 75%, the temperature is 120℃, and the draft ratio is 130%; the concentration of the dilute acid used in the second dilute acid bath is 60%, the temperature is 100℃, and the draft ratio is 110%; the concentration of the dilute acid used in the third dilute acid bath is 45%, the temperature is 80℃, and the draft ratio is 90%; the concentration of the dilute acid used in the fourth dilute acid bath is 30%, the temperature is 15℃, and the draft ratio is 90%. The residence time of the fiber in the first dilute acid bath, the second dilute acid bath, the third dilute acid bath, and the fourth dilute acid bath are 10min, 10min, 20min, and 30min, respectively.
[0138] The infusible fiber is washed in a 4-stage washing tank and stretched to obtain washed fiber; wherein the first stage washing temperature is 90°C and the stretching ratio is 110%. The second stage washing temperature is 70°C and the stretching ratio is 120%. The third stage washing temperature is 30°C and the stretching ratio is 130%. The fourth stage washing temperature is 30°C and the stretching ratio is 120%. The residence time of the fiber in the first stage washing, the second stage washing and the third stage washing is 10 minutes, 30 minutes and 40 minutes respectively.
[0139] (c) treating the washed fiber with oil in an oil tank to obtain oiled fiber; wherein the oil is an aqueous solution of amino-modified silicone oil, and the concentration of the amino-modified silicone oil in the oil is 0.8 wt %.
[0140] (d) The oiled fiber is successively passed through three stages of drying hot rollers to obtain dry fiber; the temperatures of the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller are 30°C, 40°C and 55°C, respectively, and the draft ratio is 120%; the drying hot roller time of the fiber on the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller are 10 min, 10 min and 30 min, respectively.
[0141] (e) The dried fibers are carbonized in an inert atmosphere at a temperature ranging from 200 to 900° C. to obtain continuous polyolefin-based carbon fibers; wherein the drawing ratio at 200 to 700° C. is 110%, and the drawing ratio at temperatures greater than 700 to 900° C. is 80%.
[0142] Example 5
[0143] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0144] (a) providing fibers made from modified polyolefins;
[0145] 96 wt% of polypropylene, 1 wt% of polydicyclopentadiene, 2.2 wt% of polyethylene norbornene and 0.8 wt% of maleic anhydride grafted polypropylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, pelletized and dried to obtain a modified polyolefin;
[0146] The modified polyolefin was placed in a melt spinning machine to prepare 20 μm fully drawn yarns, the spinning temperature was 190° C., the speed of the yarn collection roller was 1800 r / min, and fibers were obtained.
[0147] (b) subjecting the fiber to sulfonation treatment in two-stage concentrated acid bath and three-stage dilute acid bath, respectively, wherein the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drafting treatment is used during the sulfonation treatment to obtain an infusible fiber;
[0148] The first concentrated acid bath has a concentration of 97%, a temperature of 100°C, a draft ratio of 60%, and a sulfonation degree of the fiber in the first concentrated acid bath of 70%. The second concentrated acid bath has a concentration of 98%, a temperature of 140°C, a draft ratio of 50%, and a sulfonation degree of the fiber in the second concentrated acid bath of 100%.
[0149] The concentration of the diluted acid used in the first dilute acid bath is 80%, the temperature is 90℃, and the draft ratio is 90%; the concentration of the diluted acid used in the second dilute acid bath is 60%, the temperature is 80℃, and the draft ratio is 100%. The concentration of the diluted acid used in the third dilute acid bath is 40%, the temperature is 50℃, and the draft ratio is 110%; the residence time of the fiber in the first dilute acid bath, the second dilute acid bath, and the third dilute acid bath is 10min, 20min, and 35min respectively.
[0150] The infusible fiber is washed in two-stage washing tanks and stretched to obtain washed fiber; wherein the first stage washing temperature is 90°C and the stretching ratio is 110%. The second stage washing temperature is 30°C and the stretching ratio is 120%. The fiber stays in the first stage washing and the second stage washing for 15 minutes and 25 minutes respectively.
[0151] (c) The washed fiber is subjected to oiling treatment in an oil agent tank to obtain oiled fiber; wherein the oil agent is an aqueous solution of polyvinyl alcohol, and the concentration of polyvinyl alcohol in the oil agent is 1.0 wt %.
[0152] (d) The oiled fiber is successively passed through three stages of drying hot rollers to obtain dry fiber; the temperatures of the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller are 30°C, 45°C and 60°C respectively, the draft ratio is 120% and the drying hot roller time is 10 min, 20 min and 5 min respectively.
[0153] (e) The dried fibers are carbonized in an inert atmosphere at a temperature ranging from 200 to 1200° C. to obtain continuous polyolefin-based carbon fibers; wherein the drawing ratio at 200 to 700° C. is 120%, the drawing ratio at 700 to 900° C. is 80%, and the drawing ratio at 900 to 1200° C. is 110%.
[0154] Example 6
[0155] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0156] (a) providing fibers made from modified polyolefins;
[0157] 98.5 wt% of polypropylene, 0.5 wt% of carbon nanotubes, 0.5 wt% of graphene nanosheets and 0.5 wt% of maleic anhydride grafted polypropylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, granulated and dried to obtain a modified polyolefin;
[0158] The modified polyolefin was placed in a melt spinning machine to prepare 15 μm fully drawn yarns, the spinning temperature was 190° C., the speed of the yarn collection roller was 2200 r / min, and fibers were obtained.
[0159] (b) The fiber is subjected to sulfonation treatment in three-stage concentrated acid bath and three-stage dilute acid bath, respectively, wherein the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drawing treatment is used during the sulfonation treatment to obtain an infusible fiber; wherein the concentration of the concentrated acid used in the first stage concentrated acid bath is 98%, the temperature is 90°C, the drawing ratio is 200%, and the degree of sulfonation of the fiber in the first stage concentrated acid bath is 20%; the concentration of the concentrated acid used in the second stage concentrated acid bath is 99%, the temperature is 130°C, the drawing ratio is 70%, and the degree of sulfonation of the fiber in the second stage concentrated acid bath is 50%; the concentration of the concentrated acid used in the third stage concentrated acid bath is 9 8%, temperature is 135℃, stretch ratio is 50%, and the sulfonation degree of the fiber in the third concentrated acid bath is 99%; the concentration of the dilute acid used in the first dilute acid bath is 90%, the temperature is 95℃, and the stretch ratio is 100%; the concentration of the dilute acid used in the second dilute acid bath is 60%, the temperature is 80℃, and the stretch ratio is 100%; the concentration of the dilute acid used in the third dilute acid bath is 30%, the temperature is 50℃, and the stretch ratio is 120%. The residence time of the fiber in the first dilute acid bath, the second dilute acid bath, and the third dilute acid bath are 10min, 30min, and 50min respectively.
[0160] The infusible fiber is washed in a three-stage washing tank and stretched to obtain washed fiber; wherein, the first stage washing temperature is 90°C and the stretching ratio is 110%; the second stage washing temperature is 50°C and the stretching ratio is 120%; the third stage washing temperature is 20°C and the stretching ratio is 130%; the residence time of the fiber in the first stage washing, the second stage washing and the third stage washing are 15min, 20min and 20min respectively.
[0161] (c) oiling the washed fiber in an oil tank to obtain oiled fiber; wherein the oil is an aqueous solution of carboxymethyl cellulose, and the concentration of the carboxymethyl cellulose in the oil is 0.6 wt %.
[0162] (d) The oiled fiber is successively passed through three stages of drying hot rollers to obtain dry fiber; the temperatures of the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller are 30°C, 50°C and 60°C, respectively, and the draft ratio is 120%; the drying hot roller time of the fiber on the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller is 20 min, 40 min and 60 min, respectively.
[0163] (e) The dried fibers are carbonized in an inert atmosphere at a temperature ranging from 200 to 1300° C. to obtain continuous polyolefin-based carbon fibers; wherein the draw ratio at 200 to 700° C. is 70%, the draw ratio at temperatures >700 to 900° C. is 110%, and the draw ratio at temperatures >900 to 1300° C. is 115%.
[0164] Example 7
[0165] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0166] (a) providing fibers made from modified polyolefins;
[0167] 98 wt% of polyethylene, 0.5 wt% of graphene oxide, 0.5 wt% of graphite, and 1% of maleic anhydride grafted polyethylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, pelletized and dried to obtain a modified polyolefin;
[0168] The modified polyolefin was placed in a melt spinning machine to prepare 18 μm fully drawn yarns, the spinning temperature was 190° C., the speed of the yarn collection roller was 2300 r / min, and fibers were obtained.
[0169] (b) The fiber is subjected to sulfonation treatment in three levels of concentrated acid bath and three levels of dilute acid bath, respectively, the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drawing treatment is adopted during the sulfonation treatment to obtain an infusible fiber; wherein the concentration of the concentrated acid used in the first level concentrated acid bath is 98%, the temperature is 90°C, the drawing ratio is 200%, and the degree of sulfonation of the fiber in the first level concentrated acid bath is 30%; the concentration of the concentrated acid used in the second level concentrated acid bath is 99%, the temperature is 130°C, the drawing ratio is 70%, and the degree of sulfonation of the fiber in the second level concentrated acid bath is 70%; the concentration of the concentrated acid used in the third level concentrated acid bath is 98%, the temperature is 135°C, the drawing ratio is 50%, and the degree of sulfonation of the fiber in the third level concentrated acid bath is 100%. The concentration of the dilute acid used in the first dilute acid bath is 90%, the temperature is 95℃, and the draft ratio is 100%; the concentration of the dilute acid used in the second dilute acid bath is 60%, the temperature is 80℃, and the draft ratio is 100%; the concentration of the dilute acid used in the third dilute acid bath is 30%, the temperature is 50℃, and the draft ratio is 120%; the residence time of the fiber in the first dilute acid bath, the second dilute acid bath, and the third dilute acid bath are 15min, 30min, and 40min, respectively.
[0170] The infusible fiber is washed in a three-stage washing tank and stretched to obtain washed fiber; wherein, the first stage washing temperature is 90°C and the stretching ratio is 110%; the second stage washing temperature is 50°C and the stretching ratio is 120%; the third stage washing temperature is 20°C and the stretching ratio is 130%; the residence time of the fiber in the first stage washing, the second stage washing and the third stage washing are 10min, 20min and 40min respectively.
[0171] (c) oiling the washed fiber in an oil tank to obtain oiled fiber; wherein the oil is an aqueous solution of polydiallyldimethylammonium chloride, and the concentration of polydiallyldimethylammonium chloride in the oil is 2.5 wt %.
[0172] (d) The oiled fiber is successively passed through three stages of drying hot rollers to obtain dry fiber; the temperatures of the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller are 30°C, 50°C and 60°C respectively, the draft ratio is 120% and the drying hot roller time is 20 min, 20 min and 30 min respectively.
[0173] (e) The dried fibers are carbonized in an inert atmosphere at a temperature ranging from 200 to 1400° C. to obtain continuous polyolefin-based carbon fibers; wherein the draw ratio at 200 to 700° C. is 130%, the draw ratio at temperatures >700 to 900° C. is 110%, and the draw ratio at temperatures >900 to 1400° C. is 115%.
[0174] Example 8
[0175] This embodiment provides a method for preparing continuous polyolefin-based carbon fibers, comprising the following steps:
[0176] (a) providing fibers made from modified polyolefins;
[0177] 98 wt% of polypropylene and 2% of maleic anhydride grafted polypropylene are mixed and placed in an internal mixer and a twin-screw extruder for uniform mixing, pelletized and dried to obtain a modified polyolefin;
[0178] The modified polyolefin was placed in a melt spinning machine to prepare 12 μm fully drawn yarns, the spinning temperature was 200° C., the speed of the yarn collection roller was 2500 r / min, and fibers were obtained.
[0179] (b) The fiber is subjected to sulfonation treatment in three levels of concentrated acid bath and three levels of dilute acid bath, respectively, the acid used in the sulfonation treatment is sulfuric acid, and a multi-stage drawing treatment is adopted during the sulfonation treatment to obtain an infusible fiber; wherein the concentration of the concentrated acid used in the first level concentrated acid bath is 98%, the temperature is 90°C, the drawing ratio is 200%, and the degree of sulfonation of the fiber in the first level concentrated acid bath is 30%; the concentration of the concentrated acid used in the second level concentrated acid bath is 98%, the temperature is 120°C, the drawing ratio is 90%, and the degree of sulfonation of the fiber in the second level concentrated acid bath is 60%; the concentration of the concentrated acid used in the third level concentrated acid bath is 98%, the temperature is 140°C, the drawing ratio is 60%, and the degree of sulfonation of the fiber in the third level concentrated acid bath is 100%. The concentration of the dilute acid used in the first dilute acid bath is 90%, the temperature is 95℃, and the draft ratio is 50%; the concentration of the dilute acid used in the second dilute acid bath is 60%, the temperature is 70℃, and the draft ratio is 70%; the concentration of the dilute acid used in the third dilute acid bath is 30%, the temperature is 30℃, and the draft ratio is 120%; the residence time of the fiber in the first dilute acid bath, the second dilute acid bath, and the third dilute acid bath are 25min, 15min, and 30min respectively.
[0180] The infusible fiber is washed in a three-stage washing tank and stretched to obtain washed fiber; wherein, the first stage washing temperature is 90°C and the stretching ratio is 110%; the second stage washing temperature is 70°C and the stretching ratio is 120%; the third stage washing temperature is 30°C and the stretching ratio is 130%; the residence time of the fiber in the first stage washing, the second stage washing and the third stage washing are 10min, 20min and 40min respectively.
[0181] (c) treating the washed fiber with oil in an oil tank to obtain oiled fiber; wherein the oil is an aqueous solution of polyether-modified silicone oil, and the concentration of the polyether-modified silicone oil in the oil is 1.0 wt %.
[0182] (d) The oiled fiber is successively passed through three stages of drying hot rollers to obtain dry fiber; the temperatures of the first stage drying hot roller, the second stage drying hot roller and the third stage drying hot roller are 30°C, 45°C and 55°C respectively, and the draft ratio is 120%; the drying hot roller time is 10 min, 10 min and 20 min respectively.
[0183] (e) The dried fibers are carbonized in an inert atmosphere at a temperature ranging from 200 to 1350° C. to obtain continuous polyolefin-based carbon fibers; wherein the draw ratio at 200 to 700° C. is 90%, the draw ratio at temperatures >700 to 900° C. is 100%, and the draw ratio at temperatures >900 to 1350° C. is 110%.
[0184] Comparative Example 1
[0185] This comparative example provides a method for preparing continuous polyolefin-based carbon fibers. Except that the raw material in step (a) is 100 wt % polypropylene and does not include maleic anhydride grafted polypropylene, the remaining steps and process parameters are the same as those in Example 8.
[0186] Comparative Example 2
[0187] This comparative example provides a method for preparing continuous polyolefin-based carbon fiber. Except that the sulfonation treatment process in the concentrated acid bath and the dilute acid bath in step (b), the water washing treatment, and the draw ratio in the carbonization stage in step (e) are all 0, the remaining steps and process parameters are the same as those in Example 8.
[0188] Comparative Example 3
[0189] This comparative example provides a method for preparing continuous polyolefin-based carbon fibers, except that the concentrated acid bath in step (b) is changed to a first-stage one (the concentration of the concentrated acid bath is 98%, the temperature is 120°C, and the stretching ratio is 90%) and the carbonization stage in step (e) at 200-1350°C with the stretching ratio being 200%, the remaining steps and process parameters are the same as those in Example 8.
[0190] Comparative Example 4
[0191] This comparative example provides a method for preparing continuous polyolefin-based carbon fiber, except that the concentrated acid bath in step (b) is changed to a first-stage one, the concentration of the concentrated acid bath is 98%, the temperature is 120°C, the drawing ratio is 90%, and the degree of sulfonation of the fiber in the concentrated acid bath is 100%. The remaining steps and process parameters are the same as those in Example 8.
[0192] Comparative Example 5
[0193] This comparative example provides a method for preparing continuous polyolefin-based carbon fiber, except that the dilute acid bath in step (b) is changed to a first-stage one, the concentration of the dilute acid bath is 60%, the temperature is 70°C, the drawing ratio is 70%, and the residence time of the dilute acid bath is 15 minutes. The remaining steps and process parameters are the same as those in Example 8.
[0194] Comparative Example 6
[0195] This comparative example provides a method for preparing continuous polyolefin-based carbon fibers. Except that the draw ratio in the carbonization stage (e) at 200-1350° C. is 90%, the remaining steps and process parameters are the same as those in Example 8.
[0196] Comparative Example 7
[0197] This comparative example provides a method for preparing continuous polyolefin-based carbon fibers, except that the oiling treatment in step (c) is not performed, that is, the washed fibers obtained in step (b) are directly subjected to step (d), and the remaining steps and process parameters are the same as those in Example 8.
[0198] In order to compare the technical effects of the above embodiments and comparative examples, the following experimental examples are specially designed.
[0199] Experimental Example 1
[0200] The properties of the carbon fibers prepared in the embodiments and comparative examples were tested, and the specific results are shown in Table 1. The diameter of the carbon fibers was measured according to GB / T 29762-2013, the bulk density of the carbon fibers was measured according to GB / T 30019-2013, and the tensile strength and tensile modulus of the carbon fibers were measured according to GB / T 31290-2014.
[0201] Table 1
[0202]
[0203]
[0204] It can be found from Example 8 and Comparative Example 1 that the introduction of polyolefin compatibilizer can significantly improve the mechanical properties of carbon fiber. It can be found from Example 8 and Comparative Examples 2 to 6 that multi-stage drafting optimizes the graphite microcrystalline structure of carbon fiber and improves the tensile strength and modulus of carbon fiber. By comparing Example 8 and Comparative Example 7, it can be seen that oiling treatment improves the fiber opening performance of sulfonated and carbonized fibers, reduces the fusion and damage of sulfonated fibers during drying and carbonization, and thus improves the tensile strength and modulus of carbon fiber.
[0205] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.
Claims
1. A method for preparing continuous polyolefin-based carbon fibers, characterized in that: The following steps are involved: (a) providing fibers made from modified polyolefins; (b) performing a multi-stage sulfonation treatment on the fiber using an acid, and performing a multi-stage drafting treatment during the multi-stage sulfonation treatment to obtain an infusible fiber; The infusible fiber is washed with water to obtain washed fiber; (c) the washed fiber is subjected to oiling treatment to obtain oiled fiber; (d) the oiled fiber is passed through a drying hot roller to obtain a dry fiber; (e) performing carbonization treatment on the dried fibers, and adopting a multi-stage drawing process during the carbonization process to obtain continuous polyolefin-based carbon fibers.
2. The method for preparing continuous polyolefin-based carbon fiber according to claim 1, characterized in that: In step (a), the modified polyolefin is obtained by modifying polyolefin using a polyolefin compatibilizer; Preferably, the polyolefin to be modified includes polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, poly-4-methyl-1-pentene, poly-1-hexene, poly-3-methylbutene-1, polybutadiene, polyisoprene, polydicyclopentadiene, polyethylene norbornene, polyethylene norbornene homopolymer and carbon nanofiller modified products thereof, binary, ternary, multi-component copolymers containing the above homopolymer structural units and carbon nanofiller modified products thereof or one or more thereof; further preferably, the mass fraction of the carbon nanofiller in the carbon nanofiller modified product of the polyolefin homopolymer or the carbon nanofiller modified product of the polyolefin copolymer is 0-5%; Preferably, the polyolefin compatibilizer is a modified product obtained by grafting a polar monomer onto a polyolefin, wherein the polar monomer comprises at least one of maleic anhydride, acrylic acid, α-methacrylic acid, acrylamide, glycidyl methacrylate or styrene, and the polyolefin comprises polyethylene or polypropylene; Preferably, the mass fraction of the polyolefin compatibilizer in the modified polyolefin is 0.5-20%.
3. The method for preparing continuous polyolefin-based carbon fiber according to claim 1, characterized in that: In step (b), the multi-stage sulfonation treatment comprises sequentially using 1 to 3 levels of concentrated acid baths for concentrated acid treatment and using 2 to 5 levels of dilute acid baths for dilute acid treatment; Preferably, in step (b), when the concentrated acid treatment is performed in two or three concentrated acid baths in the multi-stage sulfonation treatment, the draft ratio used in the third concentrated acid bath is smaller than the draft ratio used in the second concentrated acid bath, and the draft ratio used in the second concentrated acid bath is smaller than the draft ratio used in the first concentrated acid bath; Preferably, in step (b), the acid used in the multi-stage sulfonation treatment includes sulfuric acid.
4. The method for preparing continuous polyolefin-based carbon fiber according to claim 3, characterized in that: In step (b), when a concentrated acid treatment is performed in a first-level concentrated acid bath, the concentration of the concentrated acid used in the concentrated acid bath is 95-99%, the temperature is 110-160° C., the draft ratio is 50-320%, and the degree of sulfonation of the fiber in the first-level concentrated acid bath is 90-100%; preferably, the concentration of the concentrated acid used in the concentrated acid bath is 97.5-98.5%, the temperature is 120-140° C., and the draft ratio is 90-300%; the degree of sulfonation of the fiber in the first-level concentrated acid bath is 95-100%; Or, in step (b), when two-stage concentrated acid baths are used for concentrated acid treatment, the concentration of concentrated acid used in the first stage concentrated acid bath is 95-99%, the temperature is 50-120°C, the draft ratio is 60-200%, and the degree of sulfonation of the fiber in the first stage concentrated acid bath is 20-70%; the concentration of concentrated acid used in the second stage concentrated acid bath is 95-99%, the temperature is 100-160°C, the draft ratio is 50-180%, the degree of sulfonation of the fiber in the second stage concentrated acid bath is 90-100%, and the draft ratio used in the second stage concentrated acid bath is less than that used in the first stage concentrated acid bath. The draft ratio used; preferably, the concentration of the concentrated acid used in the first concentrated acid bath is 97.5-98.5%, the temperature is 60-110°C, the draft ratio is 70-150%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 30%-50%; the concentration of the concentrated acid used in the second concentrated acid bath is 97.5-98.5%, the temperature is 100-145°C, the draft ratio is 50-130%, the degree of sulfonation of the fiber in the second concentrated acid bath is 95-100%, and the draft ratio used in the second concentrated acid bath is less than the draft ratio used in the first concentrated acid bath; Or, in step (b), when three-stage concentrated acid baths are used for concentrated acid treatment, the concentration of concentrated acid used in the first-stage concentrated acid bath is 95-99%, the temperature is 50-120°C, the draft ratio is 60-200%, and the degree of sulfonation of the fiber in the first-stage concentrated acid bath is 10-50%; the concentration of concentrated acid used in the second-stage concentrated acid bath is 95-99%, the temperature is 100-160°C, the draft ratio is 40-180%, and the degree of sulfonation of the fiber in the second-stage concentrated acid bath is 40-70%; the concentration of concentrated acid used in the third-stage concentrated acid bath is 95-99%, the temperature is 100-160°C, the draft ratio is 30-120%, the degree of sulfonation of the fiber in the third-stage concentrated acid bath is 90-100%, and the draft ratio used in the third-stage concentrated acid bath is less than the draft ratio used in the second-stage concentrated acid bath, and the draft ratio used in the second-stage concentrated acid bath is less than the draft ratio used in the first-stage concentrated acid bath. Draft ratio; preferably, the concentration of concentrated acid used in the first concentrated acid bath is 97.5-98.5%, the temperature is 60-110 ° C, the draft ratio is 70-150%, and the degree of sulfonation of the fiber in the first concentrated acid bath is 20-40%; the concentration of concentrated acid used in the second concentrated acid bath is 97.5-98.5%, the temperature is 100-145 ° C, the draft ratio is 40-130%, and the fiber in the second concentrated acid bath is The degree of sulfonation is 50-70%; the concentration of concentrated acid used in the third concentrated acid bath is 97.5-98.5%, the temperature is 100-145°C, the draft ratio is 30-80%, and the degree of sulfonation of the fiber in the third concentrated acid bath is 95-100%; and the draft ratio used in the third concentrated acid bath is less than the draft ratio used in the second concentrated acid bath, and the draft ratio used in the second concentrated acid bath is less than the draft ratio used in the first concentrated acid bath.
5. The method for preparing continuous polyolefin-based carbon fiber according to claim 3, characterized in that: In step (b), when two-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first-stage dilute acid bath is 60-90%, the temperature is 15-120° C., and the draft ratio is 70-150%; the concentration of the dilute acid used in the second-stage dilute acid bath is 30-60%, the temperature is 15-90° C., and the draft ratio is 70-120%; the residence time of the fiber in the first-stage dilute acid bath and the second-stage dilute acid bath is independently 10-60 min; Or, in step (b), when three-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first stage dilute acid bath is 70-90%, the temperature is 15-120°C, and the draft ratio is 80-140%; the concentration of the dilute acid used in the second stage dilute acid bath is 50-70%, the temperature is 15-100°C, and the draft ratio is 80-120%; the concentration of the dilute acid used in the third stage dilute acid bath is 30-50%, the temperature is 15-80°C, and the draft ratio is 80-110%; the residence time of the fiber in the first stage dilute acid bath, the second stage dilute acid bath and the third stage dilute acid bath is independently 10-60 min; Or, in step (b), when four-stage dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first-stage dilute acid bath is 75-90%, the temperature is 15-120°C, and the draft ratio is 90-130%; the concentration of the dilute acid used in the second-stage dilute acid bath is 60-75%, the temperature is 15-100°C, and the draft ratio is 90-110%; the concentration of the dilute acid used in the third-stage dilute acid bath is 45-60%, the temperature is 15-80°C, and the draft ratio is 90-110%; the concentration of the dilute acid used in the fourth-stage dilute acid bath is 30-45%, the temperature is 15-60°C, and the draft ratio is 90-110%; the residence time of the fiber in the first-stage dilute acid bath, the second-stage dilute acid bath, the third-stage dilute acid bath and the fourth-stage dilute acid bath is independently 10-60 min; Or, in step (b), when 5 levels of dilute acid baths are used for dilute acid treatment, the concentration of the dilute acid used in the first level dilute acid bath is 80-90%, the temperature is 15-120° C., and the draft ratio is 95-120%; the concentration of the dilute acid used in the second level dilute acid bath is 70-80%, the temperature is 15-100° C., and the draft ratio is 95-120%; the concentration of the dilute acid used in the third level dilute acid bath is 60-70%, the temperature is 15-80° C., and the draft ratio is 95-110%; the concentration of the dilute acid used in the fourth level dilute acid bath is 40-60%, the temperature is 15-60° C., and the draft ratio is 95-110%; the concentration of the dilute acid used in the fifth level dilute acid bath is 20-40%, the temperature is 15-40° C., and the draft ratio is 95-110%. The residence time of the fiber in the first dilute acid bath, the second dilute acid bath, the third dilute acid bath, the fourth dilute acid bath and the fifth dilute acid bath is independently 10-60 minutes.
6. The method for preparing continuous polyolefin-based carbon fibers according to claim 1, characterized in that: In step (b), the infusible fiber is subjected to multi-stage water washing, the water flow rate is opposite to the direction of the infusible fiber transmission, the water washing temperature is 15-90° C., and the draft ratio of each stage of water washing is independently 90-130%.
7. The method for preparing continuous polyolefin-based carbon fibers according to claim 1, characterized in that: In step (c), the oil agent used for the oiling treatment includes a main agent and a solvent, and the main agent in the oil agent includes at least one of modified silicone oil, nonionic material, polycationic material or polyanionic material; Preferably, the modified silicone oil includes at least one of amino-modified silicone oil, polyether-modified silicone oil or epoxy-modified silicone oil; Preferably, the nonionic material comprises at least one of polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene glycol or polyacrylamide; Preferably, the polycationic material comprises at least one of polyamine, polyquaternium-5, polyquaternium-6, polyquaternium-7, polyquaternium-39, polyquaternium-1, polyquaternium-51, polyquaternium-47, polyquaternium-44, polyquaternium-22, polyquaternium-11, polyquaternium-28, polyquaternium-6, polyquaternium-32, polyquaternium-63, polyquaternium-33, polyvinylamine, cationic polyacrylamide, polyethyleneimine, cationic waterborne polyurethane or polydiallyldimethylammonium chloride; Preferably, the polyanionic material comprises at least one of sodium carboxymethylcellulose, polyacrylic acid, poly(methyl methacrylate), polyacrylamide or poly(styrene sulfonic acid) or anionic polyacrylamide); Preferably, the concentration of the main agent in the oil agent is 0.1-2.5wt%.
8. The method for preparing continuous polyolefin-based carbon fibers according to claim 1, characterized in that: In step (d), the oiled fiber passes through a multi-stage drying hot roller, the temperature of the drying hot roller is 30-150° C., and the draft ratio is 50-98%; Preferably, the temperature of the drying hot roller is 30-60° C., and the draft ratio is 50-98%.
9. The method for preparing continuous polyolefin-based carbon fibers according to any one of claims 1 to 8, characterized in that: In step (e), the dried fiber is carbonized at 200-3000° C. in an inert atmosphere; the draw ratio at 200-700° C. is 70-130%, the draw ratio at >700-900° C. is 80-120%, the draw ratio at >900-1500° C. is 90-115%, and the draw ratio at >1500-3000° C. is 100-115%.
10. A continuous polyolefin-based carbon fiber, characterized in that: The continuous polyolefin-based carbon fiber is prepared by the preparation method of any one of claims 1 to 9.