A method for selecting a composite admixture grinding process and its application

By grinding the components I and II, the abrasiveness and grinding limit time are judged, and the composite blending grinding process is optimized, which solves the problems of low production efficiency and difficult to guarantee product quality in the prior art. , achieving efficient grinding process selection and production efficiency improvement.

CN118791242BActive Publication Date: 2024-11-29SHANGHAI GEOPOLY NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411283602.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-29
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The prior art lacks scientific and reasonable methods to design composite blending grinding processes, resulting in low production efficiency and difficult to guarantee product quality, especially when the abrasiveness and grinding limit values ​​of different constituent materials are unclear.

Method used

By performing the first grinding treatment on components I and II, the fineness and activity index of the grinding material are detected, the ease of grinding and grinding limit time are judged, and the appropriate grinding process and time are selected to ensure that The grinding limit time and mixing ratio of components are optimized to improve production efficiency and product quality.

Benefits of technology

It has achieved test and verification of composite blends before mass production, understand the abrasionability and grinding limit time of each component raw material, select suitable grinding technology and time, ensure excellent product quality and maximize savings Production energy consumption and improve profit and harvest capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791242B_ABST
    Figure CN118791242B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of mineral composite admixtures, and discloses a method for selecting a composite admixture grinding process and an application thereof. The method is verified before the composite admixture is put into large-scale production, and the grindability and grinding limit time of each component of the admixture raw material within the production control time are learned, and a grinding process and grinding limit time suitable for the composite admixture are selected. Under the premise of ensuring that the product obtains excellent quality, production energy consumption is saved to the maximum extent, and it has higher market value and economic value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral composite admixtures, and in particular to a method for selecting a composite admixture grinding process and application thereof. Background Art

[0002] Industrial solid waste-based mineral composite admixture technology and products can significantly improve the comprehensive utilization of industrial solid waste while reducing the proportion of clinker in cement, generating good environmental, social and economic benefits. Composite admixtures formed by ultra-fine grinding and scientific matching of industrial solid waste can significantly increase the activity of various minerals and give full play to their micro-aggregate effect and particle morphology effect. After adding composite admixtures to cement, the particle size distribution is wider, thereby improving the various properties of cement; it is used in concrete to replace S95 mineral powder and part of cement, improve concrete strength and improve construction performance. Composite admixtures are an important direction for the development of modern concrete mineral admixture technology.

[0003] Due to the differences in active component content, chemical composition, physical form, fineness, etc. of various mineral admixtures, compared with single mineral admixtures, the composite use of different mineral admixtures can make up for the shortcomings of single mineral admixtures and give play to the super-superposition effect of multi-materials. Traditional mineral composite admixtures are mainly fly ash, blast furnace slag powder, silica fume and steel slag powder.

[0004] At present, there are two main grinding processes for the actual production of ultrafine admixtures, namely open circuit and closed circuit. Due to temperature restrictions, the open circuit mill reaches a certain temperature (above 150°C), which will cause agglomeration, and the mill efficiency will drop significantly, and even cannot be continuously produced. 2 / kg product requirements are difficult to adapt to, the closed-circuit system can control the temperature inside the mill at around 120℃, and can produce 700m 2 / kg or more specific surface area, even if the production specific surface area is less than 600m 2 / kg of admixture, the efficiency is also higher. The activity of the same ratio of raw materials (for example, mineral powder + fly ash) produced by the closed-circuit system is generally more than 5% higher than that produced by the open-circuit system. Therefore, the current admixture grinding process tends to use closed-circuit grinding.

[0005] Most of the domestic companies use a common grinding process, and use a variety of mixed materials. Due to the changes in the grindability of various materials, and the grinding body has a "selective grinding" function for the materials entering the mill, that is, the materials with good grindability are ground first, and the grinding degree of the materials with poor grindability is also poor. Then, before large-scale production, understanding the grindability and grinding limit of each component raw material is of great guiding significance for actual production. It can save production energy consumption to the maximum extent while ensuring the excellent quality of the product, and improve the company's profit ability in composite admixture products.

[0006] However, most of the existing pilot or small-scale verification methods usually adopt the method of directly mixing and grinding the raw materials of various alternative admixtures according to different proportions and ball milling times, and selecting an excellent preparation process through cross-testing. Although such methods can eventually prepare composite admixtures of qualified quality, they lack the understanding of the easy-to-grind characteristics of the raw materials, and cannot scientifically and rationally design an optimal preparation process based on the characteristics of each raw material.

[0007] Therefore, appropriate pilot or small-scale test verification methods are effective measures to solve the above problems. Summary of the invention

[0008] The purpose of the present invention is to provide a method for efficiently and accurately judging the grinding process of composite admixtures with different compositions.

[0009] In order to achieve the above object, the first aspect of the present invention provides a method for selecting a composite admixture grinding process, the method comprising:

[0010] (1) Subjecting component I and component II to a first grinding process respectively; defining the starting time of the first grinding process as t 0 , the end time is t n , 30min≤t n ≤50min, n is an integer of 3-5; in the process of the first grinding treatment, since t 0 Starting from the time, the fineness and activity index of the ground material subjected to the first grinding treatment are detected every 10 minutes;

[0011] Definition n-1 At the moment, the specific surface area of ​​the ground material is A1, and the mass percentage of the material with a particle size of ≤32 μm is B1; n At the moment, the specific surface area of ​​the ground material is A2, and the mass percentage of the material with a particle size of ≤32 μm is B2; n With t n-1 The difference is 10min; the unit of A1 and A2 is m 2 / kg;

[0012] If A2-A1≤10m 2 / kg, and B2-B1≤1.5wt%, then the grinding material subjected to the first grinding treatment is a non-grinding component; otherwise, it is an easy-to-grind component;

[0013] Definition i-1 At the moment, the 3d activity index of the ground material is C1, and the 28d activity index is D1; i At the moment, the 3d activity index of the ground material is C2, and the 28d activity index is D2; i With t i-1 The difference is 10min; i is a positive integer less than or equal to n;

[0014] As time goes by, if C2-C1≤3% and D2-D1≤3%, the grinding limit time of the grinding material for the first grinding process is t i-1 Otherwise, the grinding limit time is t n ;

[0015] The component I and the component II are components in the admixture raw material, and the component I and the component II are different and are each independently selected from one of mineral powder, fly ash, and steel slag powder;

[0016] (2) If both component I and component II are difficult to grind, the grinding process of the admixture raw material is process (a); otherwise, the grinding process is process (b);

[0017] (a) Process: each component in the admixture raw material containing the component I and the component II is subjected to a second grinding treatment, and then the ground components are mixed to obtain a composite admixture; wherein the time for the component I and the component II to be subjected to the second grinding treatment is the respective grinding limit time;

[0018] (b) Process: mixing the components in the admixture raw material containing the component I and the component II to obtain a mixture, and subjecting the mixture to a second grinding process to obtain a composite admixture;

[0019] The time for the mixture to undergo the second grinding process is defined as y, the mass proportions of the component I and the component II in the mixture are defined as x1 and x2, and the corresponding grinding limit times are defined as T1 and T2; the units of y, T1 and T2 are min;

[0020] y=0.8×(x1T1+x2T2).

[0021] In the present invention, t i With t i-1 The difference is 10min; i is a positive integer less than or equal to n. i The time is t0 to n Any time between t i Time and t n The moments overlap.

[0022] Preferably, based on the total mass of the admixture raw materials, the mass proportions of the component I and the component II are both ≥10%.

[0023] Preferably, the admixture raw material further contains gypsum, and based on the total mass of the admixture raw material, the mass proportion of the gypsum is less than 5%.

[0024] Preferably, the gypsum is desulfurized gypsum and has a water content of ≤15wt%.

[0025] Preferably, the mineral powder is S95 grade granulated blast furnace slag powder that meets the standard requirements of GB / T 18046-2017.

[0026] Preferably, the fly ash is secondary fly ash that meets the standard requirements of GB / T 1596-2017.

[0027] Preferably, the steel slag powder is primary steel slag powder or secondary steel slag powder that meets the standard requirements of GB / T 20491-2017.

[0028] According to a preferred specific implementation manner, the conditions of the first grinding treatment and the second grinding treatment are the same, and the conditions include: the mill speed is 40-50rpm, and the particle size of the material entering the mill is ≤7mm.

[0029] Preferably, the conditions of the composite admixture meet the following requirements: 30 μm sieve residue ≤ 0.35%, median particle size D 50 ≤10μm, 7d activity ≥70%, 28d activity ≥90%, fluidity ratio ≥95%.

[0030] The second aspect of the present invention provides the application of the method for selecting the composite admixture grinding process described in the first aspect in the field of mineral composite admixture preparation.

[0031] The third aspect of the present invention provides the use of a composite admixture prepared by the method for selecting a composite admixture grinding process as described in the first aspect in cement products.

[0032] Preferably, the composite admixture accounts for 10-20wt% of the total mass of the cement product.

[0033] Through the method for selecting the composite admixture grinding process provided by the present invention, it is possible to conduct pilot or small-scale tests before the composite admixture product is put into large-scale production, to learn the grindability and grinding limit time of each component raw material of the admixture within the production control time, and to select a grinding process and grinding time suitable for the composite admixture, which can ensure that the product obtains excellent quality, save the enterprise's production energy consumption to the maximum extent, and improve the enterprise's profit ability from the composite admixture product. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is the particle size distribution of mineral powder after different grinding times;

[0035] Figure 2 is the particle size distribution of fly ash after different grinding times;

[0036] Figure 3 It is the particle size distribution before and after the composite admixture replaces cement. DETAILED DESCRIPTION

[0037] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0038] As mentioned above, the first aspect of the present invention provides a method for selecting a composite admixture grinding process, the method comprising:

[0039] (1) Subjecting component I and component II to a first grinding process respectively; defining the starting time of the first grinding process as t 0 , the end time is t n , 30min≤t n ≤50min, n is an integer of 3-5; in the process of the first grinding treatment, since t 0 Starting from the time, the fineness and activity index of the ground material subjected to the first grinding treatment are detected every 10 minutes;

[0040] Definition n-1 At the moment, the specific surface area of ​​the ground material is A1, and the mass percentage of the material with a particle size of ≤32 μm is B1; n At the moment, the specific surface area of ​​the ground material is A2, and the mass percentage of the material with a particle size of ≤32 μm is B2; n With t n-1 The difference is 10min; the unit of A1 and A2 is m 2 / kg;

[0041] If A2-A1≤10m 2 / kg, and B2-B1≤1.5wt%, then the grinding material subjected to the first grinding treatment is a non-grinding component; otherwise, it is an easy-to-grind component;

[0042] Definition i-1 At the moment, the 3d activity index of the ground material is C1, and the 28d activity index is D1; i At the moment, the 3d activity index of the ground material is C2, and the 28d activity index is D2; i With t i-1 The difference is 10min; i is a positive integer less than or equal to n;

[0043] As time goes by, if C2-C1≤3% and D2-D1≤3%, the grinding limit time of the grinding material for the first grinding process is t i-1 Otherwise, the grinding limit time is t n ;

[0044] The component I and the component II are components in the admixture raw material, and the component I and the component II are different and are each independently selected from one of mineral powder, fly ash, and steel slag powder;

[0045] (2) If both component I and component II are difficult to grind, the grinding process of the admixture raw material is process (a); otherwise, the grinding process is process (b);

[0046] (a) Process: each component in the admixture raw material containing the component I and the component II is subjected to a second grinding treatment, and then the ground components are mixed to obtain a composite admixture; wherein the time for the component I and the component II to be subjected to the second grinding treatment is the respective grinding limit time;

[0047] (b) Process: mixing the components in the admixture raw material containing the component I and the component II to obtain a mixture, and subjecting the mixture to a second grinding process to obtain a composite admixture;

[0048] The time for the mixture to undergo the second grinding process is defined as y, the mass proportions of the component I and the component II in the mixture are defined as x1 and x2, and the corresponding grinding limit times are defined as T1 and T2; the units of y, T1 and T2 are min;

[0049] y=0.8×(x1T1+x2T2).

[0050] As mentioned above, in the present invention, t i With t i-1The difference is 10min; i is a positive integer less than or equal to n. i The time is t 0 to n Any time between t i Time and t n The moments overlap.

[0051] The fineness index of the present invention includes the specific surface area and the mass percentage of the material with a particle size of ≤32 μm, and the activity index includes a 3d hydration activity index and a 28d hydration activity index.

[0052] In the present invention, t n It represents the production control time, which refers to the longest grinding time of the product controlled by the manufacturer based on the production capacity of the grinding equipment.

[0053] Preferably, 30min≤t n ≤40min, n is 3 or 4.

[0054] Preferably, based on the total mass of the admixture raw materials, the mass proportions of the component I and the component II are both ≥10%, preferably ≥30%, and more preferably ≥47%.

[0055] Preferably, the admixture raw material further contains gypsum, and based on the total mass of the admixture raw material, the mass proportion of the gypsum is less than 5%.

[0056] Preferably, the gypsum is desulfurized gypsum, and the water content is ≤15wt%. The inventors found in their research that introducing the gypsum under the preferred conditions into the admixture raw material is more conducive to the powder processing of the composite admixture, and applying the composite admixture to cement products can significantly improve the particle gradation of cement, and improve the strength and working performance of cement.

[0057] According to a preferred specific embodiment, the process (a) described in the present invention comprises: subjecting the component I, the component II and the gypsum to the second grinding treatment respectively, and then mixing the ground components to obtain a composite admixture; wherein the time for the component I and the component II to undergo the second grinding treatment is respectively the grinding limit time of each.

[0058] The present invention has no particular limitation on the time for the second grinding treatment of the gypsum in process (a), as long as the specific surface area of ​​the gypsum powder is between 200 and 300 m 2 / kg condition is sufficient.

[0059] According to another preferred embodiment, the process (b) of the present invention comprises: mixing the component I, the component II and the gypsum to obtain a mixture, and performing a second grinding process on the mixture to obtain a composite admixture;

[0060] The time for the mixture to undergo the second grinding process is defined as y, the mass proportions of the component I and the component II in the mixture are defined as x1 and x2, and the corresponding grinding limit times are defined as T1 and T2; the units of y, T1 and T2 are min;

[0061] y=0.8×(x1T1+x2T2).

[0062] Preferably, the mineral powder is S95 grade granulated blast furnace slag powder that meets the standard requirements of GB / T 18046-2017.

[0063] Preferably, the fly ash is secondary fly ash that meets the standard requirements of GB / T 1596-2017.

[0064] Preferably, the steel slag powder is primary steel slag powder or secondary steel slag powder that meets the standard requirements of GB / T 20491-2017.

[0065] Preferably, the conditions of the first grinding process and the second grinding process are the same, and the conditions include: the mill speed is 40-50rpm, and the particle size of the material entering the mill is ≤7mm.

[0066] The present invention has no particular limitation on the type of equipment for performing the first powder treatment or the second grinding treatment. Those skilled in the art may select grinding equipment known in the art. The present invention exemplarily provides a preferred specific implementation manner in the following text, which should not be construed as a limitation on the present invention by those skilled in the art.

[0067] In the present invention, the composite admixture product control index can be formulated in combination with the enterprise production quality control and the group standard T / CBMF 194-2022 Ultrafine composite mineral admixtures.

[0068] Preferably, the composite admixture meets the following conditions: 30 μm sieve residue ≤ 0.35%, median particle size D 50 ≤10μm, 7d activity ≥70%, 28d activity ≥90%, fluidity ratio ≥95%.

[0069] The 30 μm sieve residue in the present invention refers to the percentage of the sieve residue obtained by sieving the composite admixture through a sieve with an aperture of 30 μm in the total mass of the composite admixture.

[0070] The fluidity ratio described in the present invention refers to the ratio of the mortar fluidity measured after the composite admixture is added to cement to the mortar fluidity of the benchmark cement without the composite admixture, and the amount of cement added to the composite admixture is to replace 20wt% of the cement.

[0071] As mentioned above, the second aspect of the present invention provides the application of the method for selecting the composite admixture grinding process described in the first aspect in the field of mineral composite admixture preparation.

[0072] As mentioned above, the third aspect of the present invention provides the use of the composite admixture prepared by the method for selecting the composite admixture grinding process described in the first aspect in cement products.

[0073] Preferably, the composite admixture accounts for 10-20wt% of the total mass of the cement product.

[0074] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the raw materials are all commercially available.

[0075] In the following test examples, a cement test mill (manufacturer is Hebei Dahong Experimental Instrument Co., Ltd., model SM500) and a pilot Φ3.2m×13m ball mill were used.

[0076] Mineral powder: S95 grade granulated blast furnace slag powder meeting the requirements of GB / T 18046-2017, with a specific surface area of ​​486m 2 / kg;

[0077] Fly ash: Secondary fly ash that meets the requirements of GB / T 1596-2017, with a specific surface area of ​​372m 2 / kg;

[0078] Steel slag powder: Secondary steel slag powder that meets the requirements of GB / T 20491-2017 standard, with a specific surface area of ​​420 m 2 / kg;

[0079] Cement: PO 42.5 cement produced by Jiangsu Baling Conch Cement Co., Ltd.

[0080] When testing quality indicators, the particle size analysis is carried out using a laser particle size analyzer (the model used is the British Malvern Mastersizer 2000), the specific surface area test refers to the standard GB / T 8074-2008 Cement Specific Surface Area Determination Method Blaine Method test, the activity index refers to the standard GB / T 18736-2017 Mineral Admixtures for High-Strength and High-Performance Concrete Test, the mortar strength refers to the standard GBT 17671-2021 Cement Mortar Strength Test Method (ISO Method) test, the setting time and water requirement refer to the standard GBT 1346-2011 Cement Standard Consistency Water Consumption, Setting Time, Stability Test Method Test, the fluidity refers to the standard GBT 2419-2005 Cement Mortar Fluidity Determination Method Test, the chloride ion, free calcium and sulfur trioxide content refer to the standard GBT 176-2017 Cement Chemical Analysis Method Test.

[0081] In the following example, the production control time t n =30min, n=3.

[0082] In the following examples, the conditions for powder grinding or ball grinding are met: the mill speed is 48 rpm, and the particle size of the material entering the mill is ≤ 7 mm.

[0083] Example 1

[0084] (1) The mineral powder, fly ash and steel slag powder were subjected to the first grinding treatment and the t 1 ,t 2 and t 3 The particle size distribution, median particle size, specific surface area, 3d activity index, and 28d activity index at the time t 1 =10min, t 2 =20min, t 3 = 30min. The test results of each sample are shown in Table 1 and Figure 1 , Figure 2 shown.

[0085] Table 1

[0086]

[0087] Note: SD10, SD20 and SD30 respectively represent ball milling of mineral powder for 10 min, ball milling of mineral powder for 20 min and ball milling of mineral powder for 30 min; YH10, YH20 and YH30 respectively represent ball milling of fly ash for 10 min, ball milling of fly ash for 20 min and ball milling of fly ash for 30 min; CZ10, CZ20 and CZ30 respectively represent ball milling of steel slag powder for 10 min, ball milling of steel slag powder for 20 min and ball milling of steel slag powder for 30 min.

[0088] From the data in Table 1, it can be seen that the specific surface area of ​​the mineral powder is significantly increased from 583m 2 / kg increased to 642m 2 / kg, the mass percentage of mineral powder with particle size ≤32μm increased by 1.56%, and the specific surface area increased by only 3m after ball milling for 20min to 30min. 2 / kg, the mass percentage of mineral powder with particle size ≤32μm increased by only 0.4% (combined with Figure 1 ), indicating that the relative grindability of the mineral powder within the production control time is poor, and it is a non-grinding component; Figure 1 It can also be seen that after the mineral powder was processed for 10-30 minutes, its particle size distribution curves almost overlapped without obvious deviation.

[0089] From the activity index, it can be seen that after ball milling for 10 to 20 minutes, the 3d activity index and 28d activity index of the mineral powder are improved, among which the 3d activity index increases by 12.1%. After ball milling for 20 to 30 minutes, the 28d activity index of the mineral powder increases by 5.1%. It can be seen that the proposed grinding limit time of the mineral powder is 30 minutes of production control time.

[0090] After ball milling for 10 to 20 minutes, the specific surface area of ​​fly ash increased significantly from 579m 2 / kg increased to 652m 2 / kg, the mass percentage of fly ash with particle size ≤32μm increased by 1.62%, and the specific surface area continued to increase by 53 m after ball milling for 20min to 30min. 2 / kg, the mass percentage of fly ash with particle size ≤32μm continued to increase by 2.04% (combined with Figure 2 ), indicating that fly ash has good relative grindability within the production control time and is an easily grinded component; Figure 2 It can be seen that with the extension of grinding time, the overall particle size distribution of fly ash material has an obvious left shift.

[0091] From the activity index point of view, after fly ash was ball-milled for 20 to 30 minutes, the 3-day activity index increased by 0.3%, while the 28-day activity index decreased by 2.6%. It can be seen that the maximum grinding time of fly ash is 20 minutes.

[0092] After ball milling for 20 to 30 minutes, the specific surface area of ​​steel slag powder increased by only 9m 2 / kg, the mass percentage of steel slag powder with particle size ≤32μm only increased by 0.87%, indicating that steel slag powder has poor relative grindability within the production control time and is a non-grinding component.

[0093] From the activity index point of view, the 3d activity index of steel slag powder increased by 3.2% after ball milling for 10min to 20min, decreased after ball milling for 20min to 30min, and the 28d activity index only increased by 1.0%. The maximum grinding time of steel slag powder is 20min.

[0094] (2) Using mineral powder and fly ash as admixture raw materials, the process (b) is used for grinding; specifically, the mineral powder and fly ash are mixed and ball-milled in a mass ratio of 5:5, and the ball-milling time is y = 0.8 × (0.5 × 30 + 0.5 × 20) = 20 min to prepare a composite admixture (SY5b).

[0095] Comparative Example 1-1

[0096] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0097] (2) Using mineral powder and fly ash as admixture raw materials, grinding them by process (a); specifically, ball milling the mineral powder and fly ash for 30 min and 20 min, respectively, and then mixing them in a mass ratio of 5:5 to prepare a composite admixture (SY5a).

[0098] Comparative Example 1-2

[0099] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0100] (2) Mineral powder and fly ash were used as admixture raw materials. The grinding process was as follows: the mineral powder and fly ash were mixed and ball-milled in a mass ratio of 5:5 for 25 min to prepare a composite admixture (SY5c).

[0101] Example 2

[0102] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0103] (2) Using mineral powder and fly ash as admixture raw materials, the process (b) is used for grinding; specifically, the mineral powder and fly ash are mixed and ball-milled in a mass ratio of 7:3, and the ball-milling time is y = 0.8 × (0.7 × 30 + 0.3 × 20) = 22 min to prepare a composite admixture (SY7b).

[0104] Comparative Example 2-1

[0105] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0106] (2) Using mineral powder and fly ash as admixture raw materials, the process (a) was used for grinding. Specifically, the mineral powder and fly ash were ball-milled for 30 min and 20 min, respectively, and then mixed in a mass ratio of 7:3 to prepare a composite admixture (SY7a).

[0107] Comparative Example 2-2

[0108] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0109] (2) Mineral powder and fly ash were used as admixture raw materials. The grinding process was as follows: the mineral powder and fly ash were mixed and ball-milled in a mass ratio of 7:3 for 30 min to prepare a composite admixture (SY7c).

[0110] Example 3

[0111] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0112] (2) Using mineral powder and steel slag powder as admixture raw materials, and grinding them by process (a); specifically, ball milling the mineral powder and steel slag powder for 30 min and 20 min, respectively, and then mixing them in a mass ratio of 5:5 to prepare a composite admixture (SC5a).

[0113] Comparative Example 3-1

[0114] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0115] (2) Using mineral powder and steel slag powder as admixture raw materials, the process (b) is used for grinding; specifically, the mineral powder and steel slag powder are mixed and ball-milled in a ratio of 5:5, and the ball-milling time is y = 0.8 × (0.5 × 30 + 0.5 × 20) = 20 min to prepare a composite admixture (SC5b).

[0116] Example 4

[0117] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0118] (2) Using mineral powder and steel slag powder as admixture raw materials, the process (a) was used for grinding. Specifically, the mineral powder and the steel slag powder were ball-milled for 30 min and 20 min, respectively, and then mixed in a mass ratio of 7:3 to prepare a composite admixture (SC7a).

[0119] Comparative Example 4-1

[0120] (1) According to the method of step (1) of Example 1, the mineral powder, fly ash and steel slag powder are determined to be a non-grinding component, a grinding component and a non-grinding component respectively; the grinding limit time of the mineral powder, fly ash and steel slag powder is 30 min, 20 min and 20 min respectively;

[0121] (2) Using mineral powder and steel slag powder as admixture raw materials, the process (b) is used for grinding; specifically, the mineral powder and steel slag powder are mixed and ball-milled in a mass ratio of 7:3, and the ball-milling time is y = 0.8 × (0.7 × 30 + 0.3 × 20) = 22 min to prepare a composite admixture (SC7b).

[0122] Test Example 1

[0123] The particle size distribution, median particle size, 3d activity index, 7d activity index, 28d activity index and fluidity ratio of the composite admixtures prepared above were tested respectively. The specific test results are shown in Table 2.

[0124] Table 2

[0125]

[0126] According to Table 2, the quality of each sample meets the production control index of the composite admixture. When the slag powder with relatively poor grindability and the fly ash with relatively good grindability are used as the raw material components of the admixture, whether the ratio of slag powder to fly ash is 5:5 or 7:3, the 30 μm sieve residue and D of the composite admixture prepared by the process (b) are higher than those prepared by the process (a) provided by the present invention. 50 The values ​​are all lower, while the 3d activity index, 7d activity index and 28d activity index are all higher, achieving better results.

[0127] When the mixing ball milling is performed by the process (b), the mixing ball milling time of the 5:5 ratio admixture is specifically controlled to be 20 minutes, and the mixing ball milling time of the 7:3 admixture is 22 minutes. By comparing the performance data of SY5b and SY5c and the performance data of SY7b and SY7c, it can be seen that even if a longer mixing ball milling time is used, the performance data of the prepared composite admixture are not improved, and some performance indicators even show a downward trend.

[0128] When mineral powder with relatively poor grindability and steel slag powder with relatively poor grindability are used as the raw material components of the admixture, the 3d activity index, 7d activity index and 28d activity index of the composite admixture prepared by the (b) process are all inferior to those of the composite admixture prepared by the (a) process provided by the present invention.

[0129] In summary, the technical solution provided by the present invention can reduce the grinding time and save production energy consumption to the maximum extent while ensuring product quality, and can also further improve the performance of the composite admixture product.

[0130] Test Example 2

[0131] According to the grinding process of Example 1, the mineral powder and fly ash are used as admixture raw materials for expanded production, the mineral powder and fly ash each account for 50% of the total mass of the admixture raw materials, and 3000 kg of composite admixture product is obtained by grinding. The quality of the composite admixture is evaluated according to the following test method.

[0132] The test was carried out in accordance with the standard T / CBMF 194-2022 Ultrafine Composite Mineral Admixtures, and the results are shown in Table 3.

[0133] To determine whether the product performance meets the composite requirements, composite admixtures are used to replace 20% of the cement by mass in the ordinary cement system to improve its particle grading, strength and working performance of the cement. The results are shown in Tables 4 and 5.

[0134] Table 3

[0135]

[0136] Table 4

[0137]

[0138] Table 5

[0139]

[0140] Table 5

[0141]

[0142] It can be seen from Table 3 that the composite admixture prepared by mixing and ball-milling the two raw materials (mineral powder: fly ash = 50%: 50%) for 20 minutes meets the requirements in all indicators, and the 7-day activity reaches 90.5%.

[0143] It can be seen from Table 4 that: ① After adding 20% ​​composite admixture, the density-to-surface area ratio of the sample increased, which is in line with the law; ② After adding 20% ​​composite admixture, the strength of mortar was significantly optimized, among which the 3d compressive strength was equal to that of cement, and the 7d and 28d compressive strengths were significantly improved, by 8.9% and 6.6% respectively; ③ The fluidity was improved from 216mm to 228mm; ④ The water demand was reduced from 28.9% to 26.3%; ⑤ The initial setting and final setting time were extended. It can be seen that the addition of 20% composite admixture to replace ordinary cement improves the working performance of cement.

[0144] The 3~30μm particles in cement play an important role in strength. Figure 3 It can be seen that after adding 20% ​​composite admixture into ordinary cement, the particle size distribution changes and the overall curve shifts to the left. 10 , D 50 , D 90 The particle size distribution is wider, the bulk density and particle size distribution are reasonable, and the content of particles with a diameter of 3-30 μm is increased, thereby improving the various properties of cement.

[0145] In summary, the composite admixtures made by replacing 20% ​​of cement in the ordinary cement system can improve its particle grading, and improve the strength and working performance of cement. Calculated by adding 10-20% composite admixtures to PO 42.5 cement, the clinker coefficient is reduced by 7-13%, and carbon emissions are reduced by 0.06-0.11 tons per ton of low-carbon cement produced, which increases the proportion of solid waste resources replacing clinker in the cement grinding process, reduces the clinker coefficient in cement products, reduces cement clinker consumption, and improves the level of solid waste utilization.

[0146] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for selecting a composite admixture grinding process, characterized in that: The method includes: (1) Subjecting component I and component II to a first grinding process respectively; defining the start time of the first grinding process as t0 and the end time as t n , 30min≤t n ≤50min, n is an integer of 3-5; during the first grinding process, starting from time t0, the fineness and activity index of the grinding material subjected to the first grinding process are detected every 10min; Definition n-1 At the moment, the specific surface area of ​​the ground material is A1, and the mass percentage of the material with a particle size of ≤32 μm is B1; n At the moment, the specific surface area of ​​the ground material is A2, and the mass percentage of the material with a particle size of ≤32 μm is B2; n With t n-1 The difference is 10min; the unit of A1 and A2 is m 2 / kg; If A2-A1≤10m 2 / kg, and B2-B1≤1.5wt%, then the grinding material subjected to the first grinding treatment is a non-grinding component; otherwise, it is an easy-to-grind component; Definition i-1 At the moment, the 3d activity index of the ground material is C1, and the 28d activity index is D1; i At the moment, the 3d activity index of the ground material is C2, and the 28d activity index is D2; i With t i-1 The difference is 10min; i is a positive integer less than or equal to n; As time goes by, if C2-C1≤3% and D2-D1≤3%, the grinding limit time of the grinding material for the first grinding process is t i-1 Otherwise, the grinding limit time is t n ; The component I and the component II are components in the admixture raw material, and the component I and the component II are different and are each independently selected from one of mineral powder, fly ash, and steel slag powder; (2) If both component I and component II are difficult to grind, the grinding process of the admixture raw material is process (a); otherwise, the grinding process is process (b); (a) Process: each component in the admixture raw material containing the component I and the component II is subjected to a second grinding treatment, and then the ground components are mixed to obtain a composite admixture; wherein the time for the component I and the component II to be subjected to the second grinding treatment is the respective grinding limit time; (b) Process: mixing the components in the admixture raw material containing the component I and the component II to obtain a mixture, and subjecting the mixture to a second grinding process to obtain a composite admixture; The time for the mixture to undergo the second grinding process is defined as y, the mass proportions of the component I and the component II in the mixture are defined as x1 and x2, and the corresponding grinding limit times are defined as T1 and T2; the units of y, T1 and T2 are min; y=0.8×(x1T1+x2T2).

2. The method according to claim 1, characterized in that Based on the total mass of the admixture raw materials, the mass proportions of the component I and the component II are both ≥10%.

3. The method according to claim 2, characterized in that The admixture raw material also contains gypsum, and based on the total mass of the admixture raw material, the mass proportion of the gypsum is less than 5%.

4. The method according to claim 3, characterized in that The gypsum is desulfurized gypsum, and the water content is ≤15wt%.

5. The method according to any one of claims 1 to 4, characterized in that: The mineral powder is S95 grade granulated blast furnace slag powder that meets the standard requirements of GB / T18046-2017; And / or, the fly ash is secondary fly ash that meets the standard requirements of GB / T 1596-2017; And / or, the steel slag powder is primary steel slag powder or secondary steel slag powder that meets the standard requirements of GB / T 20491-2017.

6. The method according to any one of claims 1 to 4, characterized in that: The conditions of the first grinding process and the second grinding process are the same, and the conditions include: the mill speed is 40-50rpm, and the particle size of the material entering the mill is ≤7mm.

7. The method according to any one of claims 1 to 4, characterized in that: The conditions of the composite admixture meet the following requirements: 30 μm sieve residue ≤ 0.35%, median particle size D 50 ≤10μm, 7d activity ≥70%, 28d activity ≥90%, fluidity ratio ≥95%.

8. Application of the method for selecting a composite admixture grinding process as described in any one of claims 1 to 7 in the field of preparing mineral composite admixtures.

9. Use of the composite admixture prepared by the method for selecting the composite admixture grinding process according to any one of claims 1 to 7 in cement products.

10. The use according to claim 9, characterized in that: The composite admixture accounts for 10-20wt% of the total mass of the cement product.

Citation Information

Patent Citations

  • Steel slag powder grinding aid for improving particle aggregation, and preparation method thereof

    CN109250953A

  • High-strength cement admixture production processing machine

    KR1019980025222A