Preparation device and preparation method of resin permeable ceramic material

By using a vacuum membrane and a temperature adjustment device in the resin infiltration ceramic material preparation device, resin infiltration and curing are carried out in the same device, solving the problems of incomplete resin penetration and low production efficiency, reducing resin loss and improving material performance.

CN118845487APending Publication Date: 2024-10-29SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410891415.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the existing resin-infiltrated ceramic material preparation process, incomplete resin penetration leads to reduced mechanical properties of the material, low production efficiency, and large resin loss, which limits production costs and efficiency.

Method used

Design a device that includes a feeding system, a infiltration system and a vacuum system. A vacuum membrane is used to form a closed space. The resin is input through the vacuum system and cured in the temperature adjustment device. The resin infiltration and curing are performed one after another in the same device.

Benefits of technology

It reduces unnecessary resin loss, reduces production costs, improves production efficiency, and improves the mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118845487A_ABST
    Figure CN118845487A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation device and a preparation method of a resin permeable ceramic material. The preparation device comprises a feeding system, a permeation system and a vacuum system, the permeation system comprises a bottom frame for placing a ceramic preform; the bottom frame is covered with a vacuum film; a closed space is formed between the vacuum film and the underframe; the two ends of the closed space are connected to the feeding system and the vacuum system respectively. During working, the vacuum membrane can be tightly attached to the ceramic prefabricated body through the internal and external pressure difference of the permeation system, and the resin permeation ceramic material can be prepared only by inputting a proper amount of resin. Compared with a high-pressure chamber adopting a rigid structure device in the prior art, the method has the advantages that the soft vacuum film is adopted to construct the closed space as the preparation space of the resin permeation ceramic material, the ineffective permeation space is less, only a small amount of resin adheres to the prepared vacuum film, and unnecessary resin loss is reduced. And permeation and curing of the resin can be carried out in the same device in succession, so that the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dental restoration material preparation, in particular to a preparation device and a preparation method for a resin-infiltrated ceramic material. Background Art

[0002] The type of material used in dental restorations directly affects the performance and restoration effect of the restoration. PICN is a dental restoration material with an interpenetrating network structure of resin and ceramic formed by the resin penetrating into porous ceramics under capillary force and then solidified. It has good biocompatibility, excellent chemical stability and excellent aesthetic properties, and has therefore attracted widespread attention.

[0003] Insufficient resin penetration during the preparation of PICN will lead to a reduction in the content of the tough phase in the material, resulting in pores inside the material, which will seriously affect the mechanical properties of PICN. The current mainstream resin infiltration ceramic process is to infiltrate the porous ceramic after interface modification in a well-mixed and well-mixed resin, remove the air in the porous ceramic by vacuuming, and allow the resin to enter the pores of the porous ceramic under capillary force. Since the pores of the porous ceramic after sintering are small, and the resin viscosity is high, and the capillary force under a vacuum environment alone is not enough to completely fill the pores with resin, incomplete penetration occurs, requiring multiple infiltrations and repeated vacuuming, and low production efficiency.

[0004] CN115998624A discloses a device and method for making dental resin-infiltrated ceramic materials, the device comprising a raw material storage unit, a raw material pressurizing unit, an infiltration unit and a vacuum unit connected in sequence; the infiltration unit comprises an infiltration chamber; the infiltration chamber is divided into an upper vacuum chamber and a lower high-pressure chamber; the vacuum chamber and the high-pressure chamber are separated by a perforated partition; the high-pressure chamber is used to place porous ceramic materials, and utilizes the dual effects of high pressure and vacuum to fully fill the resin into the micropores of the porous ceramic materials, thereby improving the infiltration effect.

[0005] It has the following technical problems:

[0006] After the porous ceramics are infiltrated with resin, a large amount of resin will remain in the high-pressure chamber, causing unnecessary resin loss; the resin infiltration and curing cannot be carried out successively in the same device, limiting production efficiency. Summary of the invention

[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a preparation device and a preparation method for resin-infiltrated ceramic materials, which can reduce unnecessary resin loss and reduce production costs when preparing resin-infiltrated ceramic materials; resin infiltration and curing can be carried out successively in the same device, thereby improving production efficiency.

[0008] In order to achieve the above object, the present invention adopts the following technical solution:

[0009] A preparation device for resin-infiltrated ceramic material, comprising a feeding system, an infiltration system and a vacuum system;

[0010] The infiltration system includes a base frame for placing the ceramic preform;

[0011] The chassis is covered with a vacuum film;

[0012] A closed space is formed between the vacuum film and the base frame;

[0013] The two ends of the closed space are respectively connected to the feeding system and the vacuum system.

[0014] Furthermore, a temperature regulating device is provided on the chassis, the vacuum film covers the temperature regulating device, the temperature regulating device is used to place the ceramic preform and control the temperature of the infiltration system, and a closed space is formed between the vacuum film and the temperature regulating device. With this structure, the infiltration and curing of the resin can be carried out successively in the same device, thereby improving production efficiency.

[0015] Furthermore, the temperature regulating device comprises a heating plate, the vacuum film covers the heating plate, the heating plate is used to place the ceramic preform, and a closed space is formed between the vacuum film and the heating plate.

[0016] Furthermore, the temperature regulating device comprises a refrigeration pipe connected to the heating plate.

[0017] Furthermore, a drainage groove is provided on the heating plate, and the drainage groove is used for placing the ceramic preform.

[0018] Furthermore, a release film is provided between the drainage groove and the vacuum film, and the release film is used to cover the ceramic preform.

[0019] Furthermore, a permeable medium is provided between the vacuum film and the release film.

[0020] Furthermore, the vacuum system includes a recovery tank and a vacuum pump, and two ends of the recovery tank are connected to the permeation system and the vacuum pump respectively.

[0021] Furthermore, the infiltration system is connected with a flow sensor and a temperature sensor; the flow sensor is used to monitor the resin flow input into the infiltration system; the temperature sensor is used to monitor the temperature in the infiltration system.

[0022] A method for preparing a resin-infiltrated ceramic material, using the above-mentioned device for preparing a resin-infiltrated ceramic material, comprises the following steps:

[0023] placing a ceramic preform on a base frame;

[0024] Covering the ceramic preform with a vacuum film so that a closed space is formed between the vacuum film and the base frame;

[0025] Connect the two ends of the confined space to the feeding system and the vacuum system respectively;

[0026] The vacuum system is turned on to evacuate the confined space, and the resin is fed into the confined space by the feeding system, so that the resin penetrates into the ceramic preform in the confined space;

[0027] After the infiltration is completed, the vacuum system is turned off, and the temperature regulating device is turned on to solidify the resin. After the solidification is completed, the vacuum film is torn off to obtain the resin-infiltrated ceramic material.

[0028] In general, the present invention has the following advantages:

[0029] During operation, a vacuum film is covered on the base frame to form a closed space between the vacuum film and the base frame, the vacuum system is turned on to evacuate the closed space, and the resin is input into the closed space by the feeding system, so that the resin penetrates into the ceramic preform in the closed space; after the penetration is completed, the vacuum system is closed, and the temperature regulating device is turned on to solidify the resin. After the solidification is completed, the vacuum film is torn off to obtain the resin-infiltrated ceramic material. The internal and external pressure difference of the infiltration system can make the vacuum film close to the ceramic preform, so that the preparation of the resin-infiltrated ceramic material can be completed by only inputting an appropriate amount of resin into the closed space. Compared with the prior art that uses a high-pressure chamber of a rigid structure device as the preparation space of the resin-infiltrated ceramic material, the present invention uses a soft vacuum film to construct a closed space as the preparation space of the resin-infiltrated ceramic material, with less invalid penetration space. After the preparation is completed, only a small amount of resin adheres to the vacuum film, which reduces unnecessary resin loss and reduces production costs. The penetration and solidification of the resin can be carried out successively in the same device, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the structure of a preparation device for resin-infiltrated ceramic materials.

[0031] Figure 2 Schematic diagram of the infiltration system.

[0032] In the figure:

[0033] 1-feeding system, 2-permeation system, 3-vacuum system, 4-control system, 5-storage tank, 6-gate valve, 7-boosting pump, 8-flow control valve, 9-flow guide tube, 10-flow sensor, 11-temperature sensor, 12-control cable, 13-data acquisition equipment, 14-resin input port, 15-resin output port, 16-base frame, 17-stabilizing frame, 18-vacuum sealant, 19-vacuum film, 20-permeation medium, 21-release film, 22-ceramic preform, 23-drainage trough, 24-heating plate, 25-refrigeration pipe, 26-recovery tank, 27-vacuum pump. DETAILED DESCRIPTION

[0034] The present invention will be described in further detail below.

[0035] like Figure 1 , Figure 2 As shown, a preparation device for resin-infiltrated ceramic material comprises a feeding system 1, an infiltration system 2, a vacuum system 3 and a control system 4 connected in sequence;

[0036] The feeding system 1 is used to input resin raw materials into the sealed infiltration system 2;

[0037] The infiltration system 2 is provided with a soft closed space, and the ceramic preform 22 to be infiltrated with resin is placed in the closed space of the infiltration system 2, the ceramic preform 22 is a porous ceramic, and the infiltration system 2 is used for resin infiltration of the porous ceramic;

[0038] The vacuum system 3 provides a vacuum environment for the infiltration system 2;

[0039] The control system 4 is used to adjust the injection flow rate, infiltration temperature and curing temperature of the resin input by the feeding system 1 to the infiltration system 2.

[0040] Furthermore, the feeding system 1 includes a storage tank 5, a gate valve 6, a booster pump 7, a flow control valve 8, and a flow guide tube 9. The flow control valve 8 is located between the booster pump 7 and the flow sensor 10, and is used to adjust the resin infusion flow rate. The booster pump 7 is located between the storage tank 5 and the flow control valve 8, and is used to pressurize the resin as one of the power sources for the resin infiltration of the ceramic preform 22. The pressurized resin enters the closed space of the infiltration system 2 from the resin input port 14 through the flow guide tube 9.

[0041] Preferably, the controllable pressure range of the booster pump 7 is 0 MPa-5 MPa.

[0042] Furthermore, the infiltration system 2 includes a base frame 16, a stabilizing frame 17, a vacuum sealant 18, a vacuum film 19, a permeable medium 20, a release film 21, a ceramic preform 22, a drainage groove 23, a heating plate 24, and a refrigeration tube 25. The vacuum film 19 is covered on the base frame 16 and is bonded to the heating plate 24 on the base frame 16 by the vacuum sealant 18. The vacuum film 19 and the base frame 16 form a closed space, and the permeable medium 20, the release film 21, the ceramic preform 22, and the drainage groove 23 are placed in the closed space from top to bottom in sequence, wherein the permeability of the permeable medium 20 is much higher than the permeability of the ceramic preform 22, which can increase the resin penetration speed. During the penetration, the resin seeps out of the permeable medium 20, and the drainage groove 23 arranges a fast flow channel on the surface of the ceramic preform 22, which can increase the resin fluidity and improve the resin penetration speed at the same time. The release film 21 is used to peel off the ceramic preform 22 after the resin has penetrated and solidified. The heating plate 24 and the cooling pipe 25 are located between the bottom frame 16 and the drainage groove 23, and are used to heat or cool the resin in the infiltration system 2 to accurately control the infiltration temperature and the curing temperature.

[0043] Preferably, the temperature control range of the heating plate 24 is 0°C-200°C; the temperature control range of the refrigeration pipe 25 is -10°C-0°C. The permeable medium 20 is a high-porosity woven fiber; the width of the drainage groove 23 is 3mm-6mm; the groove spacing of the drainage groove 23 is 25mm-75mm.

[0044] Furthermore, the vacuum system 3 includes a recovery tank 26 and a vacuum pump 27, wherein one end of the resin outlet 15 of the infiltration system 2 is connected to the closed space of the infiltration system 2, and the recovery tank 26 is connected to the other end of the resin outlet 15 of the infiltration system 2 via the guide tube 9, for collecting excess resin in the infiltration system 2 and preventing the resin from entering the vacuum pump 27. The vacuum pump 27 is located behind the recovery tank 26 and is used to maintain the vacuum environment of the infiltration system 2 as one of the power sources for the resin infiltration of the ceramic preform 22; the vacuum pressure of the vacuum environment can be controlled within a range of -1×10 -1 MPa–-1×10 -4 MPa.

[0045] Furthermore, the control system 4 includes a flow sensor 10, a temperature sensor 11, a control cable 12, and a data acquisition device 13. The flow sensor 10 is located at the resin input port 14 of the infiltration system 2, and is connected to the data acquisition device 13 through the control cable 12, and is used to monitor the flow data of the resin input port 14 of the infiltration system 2. The temperature sensor 11 is located above the drainage groove 23, and is used to monitor the temperature in the infiltration system 2, and is connected to the data acquisition device 13 through the control cable 12, and is used for temperature control in the infiltration system 2.

[0046] In a specific embodiment, the present invention also provides a method for preparing a resin-infiltrated ceramic material, comprising the following steps:

[0047] S1. The resin raw materials urethane dimethacrylate (UDMA) and triethylene glycol dimethacrylate (TEGDMA) were mixed in a ratio of 1:1 to obtain a resin raw material, 0.5 wt% initiator benzoyl peroxide (BPO) was added, and an electric stirrer was used to stir at a speed of 300 r / min for 6 h. After the mixture was evenly mixed, it was heated at -1×10 -1 MPa vacuum environment for defoaming, and after defoaming, slowly pour into the storage tank 5 and store at room temperature away from light;

[0048] The sodium aluminum silicate ceramic powder was mixed with a polyvinyl alcohol (PVA) binder with a concentration of 5wt%, and 10wt% alcohol was added for dispersion. After being mixed evenly, the mixture was dried at 40°C, crushed with a mortar, and sieved for granulation. The powder with a particle size between 100 mesh and 200 mesh was collected and pressed into a green body. The pressure was 100MPa, the pressing rate was 0.2mm / min, the holding time was 20min, and the demolding rate was 0.3mm / min. The demolded ceramic block was left to stand at room temperature.

[0049] In order to make the ceramic block heated evenly, the ceramic block was embedded with zirconium oxide or aluminum oxide powder and placed in a sintering furnace for two-stage sintering. During the first sintering process, the heating rate was 2℃ / min, and the temperature was raised to 550℃ for debonding. The temperature was kept for 100 minutes to ensure that the binder was fully removed. During the second sintering process, the heating rate was 10℃ / min, and the temperature was raised to 800℃ to sinter the internal part of the ceramic to form a sintering neck. After keeping the temperature for 100 minutes, the ceramic block was cooled to room temperature with the furnace and taken out.

[0050] S2, mixing 3 vol% of silane coupling agent with deionized water and anhydrous ethanol, wherein the ratio of deionized water to anhydrous ethanol is 1:1, adding acetic acid to adjust the pH to 3-4, to obtain a silane solution, immersing the ceramic block in the silane solution for vacuum infiltration, and drying after the infiltration to obtain a ceramic preform 22;

[0051] S3, place the ceramic preform 22 on the drainage groove 23 coated with the release agent twice, place the release film 21, the permeation medium 20 and the vacuum film 19 on the ceramic preform 22 in order from bottom to top, stick the vacuum film 19 on the heating plate 24 with the organic silicon liquid resin vacuum sealant 18 and check the air tightness. If the air tightness is good, start the vacuum pump 27 to make the vacuum pressure in the permeation system 2 be -1×10 -2 MPa;

[0052] Preheat the heating plate 24 to 50° C., open the gate valve 6, adjust the output pressure of the booster pump 7 to 0.8 MPa, so that the resin in the storage tank 5 is pressurized by the booster pump 7 and enters the infiltration system 2 from the resin input port 14 through the guide pipe 9 to perform resin infiltration of the ceramic preform 22, read the flow data collected by the flow sensor 10 in the control system 4, and adjust the infusion flow rate to 10 mL / min through the flow control valve 8;

[0053] After the infiltration is completed, the temperature of the heating plate 24 is raised to 100° C. to cure the resin. After the curing is completed, wait for the infiltration system 2 to cool down and turn off the vacuum pump 27, tear off the vacuum film 19 and the release film 21, remove the excess resin on the surface to obtain a dental resin-infiltrated ceramic composite material.

[0054] The following are typical but non-limiting embodiments of the present invention:

[0055] Example 1

[0056] This embodiment is carried out using the preparation device described in the specific embodiment, and the method is based on the preparation method in the specific embodiment, wherein the process conditions of S1 and S2 remain unchanged, and in S3, the vacuum pressure is -1×10 -2 MPa, preheat the heating plate 24 to 50°C, open the gate valve 6, adjust the output pressure of the booster pump 7 to 0.8MPa for resin infiltration, adjust the infusion flow rate to 11mL / min, and raise the temperature of the heating plate 24 to 100°C after 5 minutes of infiltration for resin curing. After curing, wait for the infiltration system 2 to cool down and turn off the vacuum pump 27, tear off the vacuum film 19 and the release film 21, remove the excess resin on the surface to obtain a dental resin-infiltrated ceramic composite material.

[0057] The bending strength and fracture toughness specimens were cut out with a diamond cutting machine, and after grinding and polishing, the bending strength and fracture toughness were tested with a universal mechanical testing machine according to ISO 6872:2015. The bending strength was 220.0 MPa and the fracture toughness was 2.0 MPa·m. 1 / 2 The Vickers hardness of the sample was measured with a Vickers hardness tester and was found to be 2.6 GPa. The excess resin in the recovery tank 26 was weighed with an electronic balance and the resin loss rate was calculated to be 20.0%.

[0058] Example 2

[0059] This embodiment is carried out using the preparation device described in the specific embodiment, and the method is based on the preparation method in the specific embodiment, wherein the process conditions of S1 and S2 remain unchanged, and in S3, the vacuum pressure is -2×10 -2MPa, preheat the heating plate 24 to 50°C, open the gate valve 6, adjust the output pressure of the booster pump 7 to 0.9MPa for resin infiltration, adjust the infusion flow rate to 12mL / min, and raise the temperature of the heating plate 24 to 100°C after 4 minutes of infiltration for resin curing. After curing, wait for the infiltration system 2 to cool down and turn off the vacuum pump 27, tear off the vacuum film 19 and the release film 21, remove the excess resin on the surface to obtain a dental resin infiltrated ceramic composite material.

[0060] The bending strength and fracture toughness specimens were cut out with a diamond cutting machine, and after grinding and polishing, the bending strength and fracture toughness were tested with a universal mechanical testing machine according to ISO 6872:2015. The bending strength was 230.0 MPa and the fracture toughness was 2.2 MPa·m. 1 / 2 The Vickers hardness of the sample was measured with a Vickers hardness tester and was found to be 2.7 GPa. The excess resin in the recovery tank 26 was weighed with an electronic balance and the resin loss rate was calculated to be 15.0%.

[0061] Example 3

[0062] This example is carried out using the preparation device described in the specific embodiment, and the method is based on the preparation method in the specific embodiment, wherein the process conditions of S1 and S2 remain unchanged, and in S3, the vacuum pressure is -3×10 -2 MPa, preheat the heating plate 24 to 50°C, open the gate valve 6, adjust the output pressure of the booster pump 7 to 1.0 MPa for resin infiltration, adjust the infusion flow rate to 13 mL / min, and raise the temperature of the heating plate 24 to 100°C after 3 minutes of infiltration for resin curing. After curing, wait for the infiltration system 2 to cool down and turn off the vacuum pump 27, tear off the vacuum film 19 and the release film 21, remove the excess resin on the surface to obtain a dental resin-infiltrated ceramic composite material.

[0063] The bending strength and fracture toughness specimens were cut out with a diamond cutting machine, and after grinding and polishing, the bending strength and fracture toughness were tested with a universal mechanical testing machine according to ISO 6872:2015. The bending strength was 240.0 MPa and the fracture toughness was 2.4 MPa·m. 1 / 2 The Vickers hardness of the sample was measured with a Vickers hardness tester and was found to be 2.8 GPa. The excess resin in the recovery tank 26 was weighed with an electronic balance and the resin loss rate was calculated to be 10.0%.

[0064] Example 4

[0065] This example is carried out using the preparation device described in the specific embodiment, and the method is based on the preparation method in the specific embodiment, wherein the process conditions of S1 and S2 remain unchanged, and in S3, the vacuum pressure is maintained at -1×10 -2MPa remains unchanged, preheat the heating plate 24 to 55°C, open the gate valve 6, adjust the output pressure of the booster pump 7 to 0.8MPa for resin infiltration, adjust the infusion flow rate to 10mL / min, and raise the temperature of the heating plate 24 to 100°C after 5 minutes of infiltration for resin curing. After curing, wait for the infiltration system 2 to cool down and turn off the vacuum pump 27, tear off the vacuum film 19 and the release film 21, remove the excess resin on the surface to obtain a dental resin infiltrated ceramic composite material.

[0066] The bending strength and fracture toughness specimens were cut out with a diamond cutting machine, and after grinding and polishing, the bending strength and fracture toughness were tested with a universal mechanical testing machine according to ISO 6872:2015. The bending strength was 220.0 MPa and the fracture toughness was 2.0 MPa·m. 1 / 2 The Vickers hardness of the sample was measured with a Vickers hardness tester and was found to be 2.6 GPa. The excess resin in the recovery tank 26 was weighed with an electronic balance and the resin loss rate was calculated to be 20.0%.

[0067] Example 5

[0068] This example is carried out using the preparation device described in the specific embodiment, and the method is based on the preparation method in the specific embodiment, wherein the process conditions of S1 and S2 remain unchanged, and in S3, the vacuum pressure is maintained at -1×10 -2 MPa remains unchanged, preheat the heating plate 24 to 60°C, open the gate valve 6, adjust the output pressure of the booster pump 7 to 0.8MPa for resin infiltration, adjust the infusion flow rate to 10mL / min, and raise the temperature of the heating plate 24 to 100°C after 4 minutes of infiltration for resin curing. After curing, wait for the infiltration system 2 to cool down and turn off the vacuum pump 27, tear off the vacuum film 19 and the release film 21, remove excess resin on the surface to obtain a dental resin-infiltrated ceramic composite material.

[0069] The bending strength and fracture toughness specimens were cut out with a diamond cutting machine, and after grinding and polishing, the bending strength and fracture toughness were tested with a universal mechanical testing machine according to ISO 6872:2015. The bending strength was 230.0 MPa and the fracture toughness was 2.2 MPa·m. 1 / 2 The Vickers hardness of the sample was measured with a Vickers hardness tester and was found to be 2.7 GPa. The excess resin in the recovery tank 26 was weighed with an electronic balance and the resin loss rate was calculated to be 15.0%.

[0070] Example 6

[0071] This example is carried out using the preparation device described in the specific embodiment, and the method is based on the preparation method in the specific embodiment, wherein the process conditions of S1 and S2 remain unchanged, and in S3, the vacuum pressure is maintained at -1×10 -2MPa remains unchanged, preheat the heating plate 24 to 65°C, open the gate valve 6, adjust the output pressure of the booster pump 7 to 0.8MPa for resin infiltration, adjust the infusion flow rate to 10mL / min, and raise the temperature of the heating plate 24 to 100°C after 3 minutes of infiltration for resin curing. After curing, wait for the infiltration system 2 to cool down and turn off the vacuum pump 27, tear off the vacuum film 19 and the release film 21, remove the excess resin on the surface to obtain a dental resin infiltrated ceramic composite material.

[0072] The bending strength and fracture toughness specimens were cut out with a diamond cutting machine, and after grinding and polishing, the bending strength and fracture toughness were tested with a universal mechanical testing machine according to ISO 6872:2015. The bending strength was 240.0 MPa and the fracture toughness was 2.4 MPa·m. 1 / 2 The Vickers hardness of the sample was measured with a Vickers hardness tester and was found to be 2.8 GPa. The excess resin in the recovery tank 26 was weighed with an electronic balance and the resin loss rate was calculated to be 10.0%.

[0073] Comparative Example 1

[0074] This comparative example provides a method for preparing a dental resin-infiltrated ceramic material, the method comprising: using the ceramic preform 22 obtained after steps S1 and S2 in the specific embodiment, immersing 3 / 4 of the ceramic preform 22 in the resin raw material described in S1, transferring the container containing the resin into a vacuum device, and adjusting the vacuum pressure to -1×10 -2 MPa, and vacuum was repeatedly drawn for 3 times, each time for 60 min, until no incompletely penetrated white area was observed with naked eyes in the center of the ceramic preform 22, and the ceramic preform 22 was taken out, and resin was cured at 100°C. After cooling, excess resin on the surface was removed to obtain dental resin-infiltrated ceramics.

[0075] The bending strength and fracture toughness specimens were cut out with a diamond cutting machine, and after grinding and polishing, the bending strength and fracture toughness were tested with a universal mechanical testing machine according to ISO 6872:2015. The bending strength was 180.0 MPa and the fracture toughness was 1.8 MPa·m. 1 / 2 The Vickers hardness of the sample was measured with a Vickers hardness tester and was found to be 2.3 GPa. The excess resin in the container containing the resin raw material was weighed with an electronic balance and the resin loss rate was calculated to be 30.0%.

[0076] The process parameters and performance test results of each embodiment and comparative example are shown in Table 1 and Table 2.

[0077] Table 1 Process parameters of each embodiment and comparative example

[0078]

[0079] Table 2 Performance test results of various embodiments and comparative examples

[0080]

[0081] The present invention provides a dental resin infiltration ceramic material preparation device and preparation method with fully accurate and controllable flow rate, temperature and vacuum pressure, which integrates infiltration and curing. The infusion flow rate, infiltration temperature and curing temperature can be adjusted for different resin systems and ceramic preforms 22 with different porosities and pore sizes to ensure the quality of dental resin infiltration ceramic composite materials. The prepared resin infiltration ceramic composite materials have good mechanical properties, with a bending strength of more than 220.0 MPa and a fracture toughness of 2.0 MPa·m 1 / 2 The Vickers hardness is above 2.6 GPa, which can ensure the penetration quality, and the resin loss rate is reduced to below 20.0%, reducing the production cost. At the same time, the penetration time is shortened to 5 minutes. Resin penetration and curing can be carried out successively in the same device. The ceramic blocks after penetration do not need additional storage and transfer, which improves the production efficiency and has a good application prospect.

[0082] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A device for preparing resin-infiltrated ceramic materials, Features: Including feeding system, permeation system and vacuum system; The infiltration system includes a base frame for placing the ceramic preform; The chassis is covered with a vacuum film; A closed space is formed between the vacuum film and the base frame; The two ends of the closed space are respectively connected to the feeding system and the vacuum system.

2. The preparation device of a resin-infiltrated ceramic material according to claim 1, Features: A temperature regulating device is arranged on the bottom frame, and the vacuum film covers the temperature regulating device. The temperature regulating device is used for placing the ceramic preform and controlling the temperature of the infiltration system, and a closed space is formed between the vacuum film and the temperature regulating device.

3. The device for preparing a resin-infiltrated ceramic material according to claim 2, Features: The temperature regulating device comprises a heating plate, a vacuum film covers the heating plate, the heating plate is used for placing the ceramic preform, and a closed space is formed between the vacuum film and the heating plate.

4. The device for preparing a resin-infiltrated ceramic material according to claim 2, Features: The temperature regulating device comprises a refrigeration pipe, and the refrigeration pipe is connected to the heating plate.

5. The device for preparing a resin-infiltrated ceramic material according to claim 3, Features: A drainage groove is arranged on the heating plate, and the drainage groove is used for placing the ceramic preform.

6. The device for preparing a resin-infiltrated ceramic material according to claim 5, Features: A release film is arranged between the drainage groove and the vacuum film, and the release film is used for covering the ceramic preform.

7. The device for preparing a resin-infiltrated ceramic material according to claim 6, Features: A permeable medium is arranged between the vacuum film and the release film.

8. The device for preparing a resin-infiltrated ceramic material according to claim 1, Features: The vacuum system comprises a recovery tank and a vacuum pump, and two ends of the recovery tank are respectively connected to the permeation system and the vacuum pump.

9. The device for preparing a resin-infiltrated ceramic material according to claim 1, Features: The infiltration system is connected with a flow sensor and a temperature sensor; the flow sensor is used to monitor the resin flow input into the infiltration system; the temperature sensor is used to monitor the temperature in the infiltration system.

10. A method for preparing a resin-infiltrated ceramic material, Features: The device for preparing a resin-infiltrated ceramic material according to any one of claims 1 to 9 comprises the following steps: placing a ceramic preform on a base frame; Covering the ceramic preform with a vacuum film so that a closed space is formed between the vacuum film and the base frame; Connect the two ends of the confined space to the feeding system and the vacuum system respectively; The vacuum system is turned on to evacuate the confined space, and the resin is fed into the confined space by the feeding system, so that the resin penetrates into the ceramic preform in the confined space; After the infiltration is completed, the vacuum system is turned off, and the temperature regulating device is turned on to solidify the resin. After the solidification is completed, the vacuum film is torn off to obtain the resin-infiltrated ceramic material.