Biomimetic mineralization stent with bone induction activity as well as preparation method and application of biomimetic mineralization stent
By simulating the collagen-inorganic mineral structure of the tendon-bone interface in a bionic mineralized scaffold and utilizing the design of an organic-inorganic composite gradient scaffold, the problem of insufficient osteoinductive activity in the existing technology is solved and effective repair of the tendon-bone interface is achieved. and biocompatibility, demonstrating excellent osteoinductive properties.
Patent Information
- Application Number
- CN202410832642.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
AI Technical Summary
Existing biomimetic mineralized scaffolds lack osteoinductive activity and cannot effectively simulate the collagen-inorganic mineral structure of the tendon-bone interface, which limits their application in tendon-bone repair.
By semi-demineralizing the allogeneic cancellous bone fragments, using Tris-HCl buffer and amorphous calcium salts, phosphate salts and polyanionic electrolytes to prepare a mineralization solution, and performing mineralization treatment to form needle-like hydroxyapatite. The organic-inorganic composite gradient scaffold of stone and collagen fibers simulates the structure of the tendon-bone interface.
It achieves good osteoinductive properties and biocompatibility of the tendon-bone interface, simulates the structure of natural bone tissue, and provides a new tendon-bone injury repair strategy.
Smart Images

Figure CN118846237A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and particularly relates to a bionic mineralized scaffold with bone induction activity and a preparation method and application thereof. Background Art
[0002] Tendon / ligament injuries are common in clinical practice, with the two most common injury sites being the rotator cuff tendons of the shoulder and the anterior cruciate ligament of the knee. As the natural healing rate of tendon to bone is slow, reconstructing the interface between tendon and bone is key in various tendon repair surgeries. The tendon-bone interface is a transitional structure from soft tissue to hard tissue and can be divided into tendon, non-mineralized fibrocartilage, mineralized fibrocartilage, and bone. From tendon to bone, the organic collagen fibers gradually decrease and the inorganic mineral content gradually increases, forming a unique transition zone.
[0003] In recent years, scaffolds and stem cells have been widely used in tendon-bone repair in tissue engineering. However, the scaffolds used in these studies lack intrinsic bioactivity and cannot simulate the transition structure of collagen-inorganic minerals between tendon and bone, which limits their application to a certain extent. By designing osteoinductive scaffolds with gradient mineralization, the interface where natural tendons or ligaments are attached to bones can be well simulated, which has great potential in promoting interface healing.
[0004] Chinese invention patent CN116850349A discloses a hydrogel that enhances tendon-bone healing and its preparation method. The invention mixes methacrylated hyaluronic acid, sodium alginate and cell microvesicles, and photocrosslinks them through a photoinitiator to obtain a hydrogel that enhances tendon-bone healing. The macroporous directional structure hydrogel functionalized with small extracellular vesicles provided by the invention can promote the repair of the supraspinatus tendon on the one hand, and improve the osteoporosis of the humerus after rotator cuff repair on the other hand; it can repair bones and tendons at the same time. However, the photoinitiator added in the invention is cytotoxic and cannot simulate the structure of the tendon-bone collagen-inorganic interface.
[0005] Therefore, developing a tendon-bone repair scaffold with excellent osteoinductive properties while mimicking the bionic structure of collagen-inorganic minerals has great potential in promoting tendon-bone interface healing. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a bionic mineralized scaffold with bone induction activity and its preparation method and application. Compared with the existing bionic mineralized scaffolds, it has excellent bone induction performance and a bionic structure of collagen-inorganic minerals for tendon-bone interface repair, and has better application prospects.
[0007] The present invention provides a biomimetic mineralized scaffold with bone induction activity. The biomimetic mineralized scaffold has bone induction activity, nano mineral crystals grow on the surface of the scaffold and are arranged in order along the long axis; needle-shaped hydroxyapatite mineralized on the surface of the biomimetic mineralized scaffold and a small amount of calcium phosphate and collagen fibers inside the bone matrix scaffold form an organic-inorganic composite gradient scaffold.
[0008] The present invention also provides a method for preparing a biomimetic mineralized scaffold with osteoinductive activity, comprising the following steps:
[0009] (1) semi-demineralizing allogeneic cancellous bone slices with dilute hydrochloric acid to obtain a bone matrix scaffold;
[0010] (2) using Tris-HCl buffer as a solvent, adding amorphous calcium salt, phosphate salt and polyanion electrolyte to prepare a mineralization solution precursor;
[0011] (3) Immersing the bone matrix scaffold obtained in step (1) in a mineral solution precursor for mineralization treatment, and obtaining a biomimetic mineralized scaffold with bone induction activity through mineralization and freeze drying.
[0012] Preferably, the concentration of the dilute hydrochloric acid in step (1) is 0.3-0.8M.
[0013] Preferably, the bone matrix scaffold in step (1) contains 20 to 200 ng / g of BMP-2 protein.
[0014] Preferably, the calcium content of the bone matrix scaffold in step (1) is 8%-12%.
[0015] Preferably, the amorphous calcium salt in step (2) is one or more of calcium chloride and calcium nitrate; the amorphous phosphate salt is one or more of disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, and potassium dihydrogen phosphate; and the polyanion electrolyte is one or more of polyaspartic acid, polyglutamic acid, polyacrylic acid, and polyallylamine hydrochloride.
[0016] Preferably, in the mineralization solution precursor in step (2), the concentration of calcium salt solution is 5-15 mM; the concentration of phosphate solution is 2-8 mM; and the concentration of polyanion electrolyte is 50-500 mg / L.
[0017] Preferably, the volume ratio of the calcium salt solution to the phosphate salt solution is 0.5-2.5:1.
[0018] Preferably, the mineralization treatment temperature in step (3) is 24-40° C., and the treatment time is 3-7 days.
[0019] The present invention also provides an application of a bionic mineralized scaffold with bone induction activity in tendon-bone injury repair.
[0020] Beneficial Effects
[0021] (1) The present invention retains the endogenous growth factor BMP-2 and natural collagen fiber structure of cancellous bone, and the mineralized hydroxyapatite presents an oriented structure similar to that of natural bone tissue, and has good osteoinductive properties and biocompatibility.
[0022] (2) The present invention can simulate the transition structure of collagen-inorganic minerals in the tendon-bone interface, providing a new strategy for the bionic repair of tendon-bone injuries and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 XRD patterns of the biomimetic mineralized scaffolds prepared in Examples 1, 2, and 3.
[0024] Figure 2 Infrared spectral images of the biomimetic mineralized scaffold and the unmineralized bone matrix scaffold prepared in Example 1.
[0025] Figure 3 This is a scanning electron microscope image of the biomimetic mineralized scaffold prepared in Example 1.
[0026] Figure 4 EDS spectra of the outside (a) and inside (b) of the biomimetic mineralized scaffold prepared in Example 2.
[0027] Figure 5 This is a picture of osteoblast adhesion on the biomimetic mineralized scaffold prepared in Example 1.
[0028] Figure 6 HE staining images of ectopic osteogenesis of the biomimetic mineralized scaffolds prepared in Example 1. (a) Example 1, (b) Example 2, (c) Example 3. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0030] Example 1
[0031] This embodiment provides a method for preparing a biomimetic mineralized scaffold with osteoinductive activity, comprising the following steps:
[0032] (1) semi-demineralizing allogeneic cancellous bone chips with 0.6M dilute hydrochloric acid to obtain a bone matrix scaffold; the bone matrix scaffold contains 120 ng / g of BMP-2 protein and a calcium content of 9%;
[0033] (2) Using 0.02 mM pH = 7.4 Tris-HCl buffer as solvent, calcium chloride and dipotassium hydrogen phosphate as solutes, 10 mM calcium salt and 5 mM phosphate solution were prepared. Polyaspartic acid was dissolved in the phosphate solution at a concentration of 200 mg / L, and the calcium salt and phosphate solutions were mixed to obtain a charged polymer-stabilized mineralization solution precursor.
[0034] (3) The bone matrix scaffold obtained in step (1) is immersed in a mineral solution precursor for mineralization treatment at 32° C. for 5 days, and a biomimetic mineralized scaffold with bone induction activity is obtained after mineralization and freeze-drying.
[0035] Example 2
[0036] This embodiment provides a method for preparing a biomimetic mineralized scaffold with osteoinductive activity, comprising the following steps:
[0037] (1) semi-demineralizing allogeneic cancellous bone chips with 0.3M dilute hydrochloric acid to obtain a bone matrix scaffold; the bone matrix scaffold contains 150 ng / g of BMP-2 protein and a calcium content of 12%;
[0038] (2) Using 0.02 mM pH = 7.4 Tris-HCl buffer as solvent, calcium chloride and dipotassium hydrogen phosphate as solutes, 15 mM calcium salt and 8 mM phosphate solution were prepared. Polyaspartic acid was dissolved in the phosphate solution at a concentration of 200 mg / L, and the calcium salt and phosphate solutions were mixed to obtain a charged polymer-stabilized mineralization solution precursor.
[0039] (3) The bone matrix scaffold obtained in step (1) is immersed in a mineral solution precursor for mineralization treatment at 32° C. for 5 days, and a biomimetic mineralized scaffold with bone induction activity is obtained after mineralization and freeze-drying.
[0040] Example 3
[0041] This embodiment provides a method for preparing a biomimetic mineralized scaffold with osteoinductive activity, comprising the following steps:
[0042] (1) semi-demineralizing allogeneic cancellous bone chips with 0.8M dilute hydrochloric acid to obtain a bone matrix scaffold; the bone matrix scaffold contains 200 ng / g of BMP-2 protein and a calcium content of 8%;
[0043] (2) Using 0.02 mM pH = 7.4 Tris-HCl buffer as solvent, calcium chloride and dipotassium hydrogen phosphate as solutes, 5 mM calcium salt and 2 mM phosphate solution were prepared. Polyaspartic acid was dissolved in the phosphate solution at a concentration of 500 mg / L, and the calcium salt and phosphate solutions were mixed to obtain a charged polymer-stabilized mineralization solution precursor.
[0044] (3) The bone matrix scaffold obtained in step (1) is immersed in a mineral solution precursor for mineralization treatment at 32° C. for 5 days, and a biomimetic mineralized scaffold with bone induction activity is obtained after mineralization and freeze-drying.
[0045] Comparative Example 1
[0046] This comparative example provides a method for preparing a collagen mineralized scaffold, comprising the following steps:
[0047] (1) Using 0.02 mM pH = 7.4 Tris-HCl buffer as solvent, calcium chloride and dipotassium hydrogen phosphate as solutes, 5 mM calcium salt and 2 mM phosphate solution were prepared. Polyaspartic acid was dissolved in the phosphate solution at a concentration of 500 mg / L, and the calcium salt and phosphate solutions were mixed to obtain a charged polymer-stabilized mineralization solution precursor.
[0048] (2) The collagen scaffold is immersed in a mineralization solution precursor for mineralization treatment at 32° C. for 5 days, and the collagen mineralized scaffold is obtained after mineralization and freeze-drying.
[0049] Depend on Figure 1 It can be seen that the XRD spectra of the mineralized products of Examples 1, 2, and 3 show the physical phase of hydroxyapatite, and several characteristic peaks of hydroxyapatite in the spectra can be clearly distinguished, indicating that the mineralized hydroxyapatite has good crystallinity.
[0050] Depend on Figure 2 It can be seen that the mineralized scaffold of Example 1 exhibits bending vibration and stretching vibration peaks of PO in the infrared spectrum, which are typical peaks of hydroxyapatite phosphate groups.
[0051] Depend on Figure 3 It can be seen that the mineralized hydroxyapatite in Example 1 is deposited on the surface of the stent in an oriented needle-like structure, the diameter of the hydroxyapatite nanocrystals is 20-50 nm, and the length distribution range is relatively large, ranging from 50-200 nm.
[0052] Depend on Figure 4 From the EDS spectrum of the mineralized scaffold in Example 2, it can be seen that the calcium content of the outside of the scaffold is 28.10%, and the calcium content of the inside is 13.01%, indicating that the outside and inside of the mineralized scaffold present a transitional structure of hydroxyapatite mineral-collagen.
[0053] MC3T3-E1 osteoblasts were inoculated onto the surface of the mineralized scaffold of Example 1, and the cells were dehydrated after 4 days. The growth of osteoblasts on the surface of the scaffold was then observed using a scanning electron microscope. Figure 5 It can be seen that osteoblasts adhere well to the scaffold surface, and the cells diffuse well on the scaffold surface through filopodia, indicating that the scaffold has good biocompatibility.
[0054] The osteoinductive activity of the scaffolds of Examples 1, 2 and 3 was evaluated by a nude mouse ectopic osteogenesis test, and the collagen mineralized scaffold was used as a control group. One month after implantation, the samples were taken for HE staining. Figure 6 It can be seen that the gaps between the mineralized scaffold materials contain a large number of active osteoblasts and bone marrow cavity tissues, indicating that the bionic mineralized scaffold has excellent osteoinductive properties; while the collagen mineralized scaffold of Comparative Example 1 did not show obvious osteoinductive activity.
Claims
1. A biomimetic mineralized scaffold with osteoinductive activity, characterized in that: The bionic mineralized scaffold has bone induction activity, nano mineral crystals grow on the surface of the scaffold and are orderly arranged along the long axis; the rod-shaped hydroxyapatite mineralized on the surface of the bionic mineralized scaffold and the natural fibrous hydroxyapatite inside the bone matrix scaffold form an organic-inorganic composite gradient scaffold.
2. A method for preparing a biomimetic mineralized scaffold with osteoinductive activity, comprising the following steps: (1) semi-demineralizing allogeneic cancellous bone slices with dilute hydrochloric acid to obtain a bone matrix scaffold; (2) using Tris-HCl buffer as a solvent, adding amorphous calcium salt, phosphate salt and polyanion electrolyte to prepare a mineralization solution precursor; (3) Immersing the bone matrix scaffold obtained in step (1) in a mineral solution precursor for mineralization treatment, and obtaining a biomimetic mineralized scaffold with bone induction activity through mineralization and freeze drying.
3. The preparation method according to claim 2, characterized in that: The concentration of the dilute hydrochloric acid in step (1) is 0.3-0.8M.
4. The preparation method according to claim 2, characterized in that: The bone matrix scaffold in step (1) contains 20 to 200 ng / g of BMP-2 protein.
5. The preparation method according to claim 2, characterized in that: The calcium content of the bone matrix scaffold in step (1) is 8%-12%.
6. The preparation method according to claim 2, characterized in that: The amorphous calcium salt in step (2) is one or more of calcium chloride and calcium nitrate; the amorphous phosphate salt is one or more of disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, and potassium dihydrogen phosphate; and the polyanion electrolyte is one or more of polyaspartic acid, polyglutamic acid, polyacrylic acid, and polyallylamine hydrochloride.
7. The preparation method according to claim 2, characterized in that: The concentration of the calcium salt solution in the mineralization solution precursor in step (2) is 5-15 mM; the concentration of the phosphate salt solution is 2-8 mM; and the concentration of the polyanion electrolyte is 50-500 mg / L.
8. The preparation method according to claim 7, characterized in that: The volume ratio of the calcium salt solution to the phosphate salt solution is 0.5-2.5:
1.
9. The preparation method according to claim 2, characterized in that: The mineralization treatment temperature in step (3) is 24-40° C., and the treatment time is 3-7 days.
10. Use of the bionic mineralized scaffold with osteoinductive activity as claimed in claim 1 in tendon-bone injury repair.