Method for recovering diamond abrasive in silicon carbide wafer wire cutting waste mortar

By adding water to the silicon carbide wafer wire cutting waste mortar and performing ultrasonic treatment, combined with high-speed centrifugation and acid-base treatment, the efficient separation of diamond abrasives is achieved, solving the problem of low diamond abrasive recovery efficiency in the existing technology, and improving the efficiency of diamond abrasive recovery. Cutting fluid improves cutting efficiency and reduces production costs.

CN118851169APending Publication Date: 2024-10-29SHANDONG UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410893163.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively separate diamond abrasives and silicon carbide fragments during wire cutting of silicon carbide wafers, resulting in low diamond abrasive recovery efficiency, affecting the cutting efficiency of the cutting fluid and causing environmental pollution problems.

Method used

By adding water to the cutting waste mortar and performing ultrasonic treatment, followed by high-speed centrifugation, hot alkali, acidification, and finally natural sedimentation in an ethanol aqueous solution, high-purity diamond abrasives are isolated.

Benefits of technology

It improves the extraction rate of diamond abrasives and the cutting efficiency of cutting fluid, reduces production costs, and avoids environmental pollution. It is suitable for mass production and the process is simple and safe.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851169A_ABST
    Figure CN118851169A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recovering diamond abrasives in silicon carbide wafer wire cutting waste mortar, which comprises the following steps: adding water into the cutting waste mortar, stirring, and carrying out ultrasonic treatment to obtain mixed slurry A; performing high-speed centrifugal treatment on the mixed slurry A to obtain a solid B; mixing the solid B with a hot alkali solution, carrying out ultrasonic treatment, and naturally settling to obtain a solid C; mixing the solid C with a strong acid solution, and performing ultrasonic treatment to obtain a solid D; and stirring and dispersing the solid D in an ethanol water solution, and naturally settling to obtain a solid E, namely the diamond abrasive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicon carbide wafer wire cutting, and more specifically, to a method for recovering diamond abrasives in waste slurry from silicon carbide wafer wire cutting. The present invention is applicable to the silicon carbide wafer cutting process in semiconductor manufacturing technology, especially to the recovery of diamond abrasives involved in wire cutting on silicon carbide wafers. Background Art

[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] Silicon carbide (SiC) is a widely used third-generation semiconductor material. Due to its advantages such as excellent thermal conductivity, high temperature stability and high electron mobility, it is widely used in power devices, radio frequency devices and optoelectronic devices. Silicon carbide devices can not only achieve higher power density and meet higher operating temperatures, but also reduce energy loss, and are expected to promote technological progress in the fields of electronic power, automotive electronics and solar energy conversion.

[0004] With the prosperity of the semiconductor industry, the demand for silicon carbide wafers is also rising. In the process of cutting silicon carbide wafers, oil-based cutting fluid containing diamond particles is mainly used. The main components are base oil, solvent oil, suspending agent, surfactant, corrosion inhibitor and extreme pressure agent. When the silicon carbide wafer is repeatedly cut using cutting mortar, a large amount of cut silicon carbide fragments exist in the cutting fluid, resulting in a decrease in cutting efficiency. Diamond powder is expensive, and recovering diamond powder from cutting waste mortar can significantly reduce the cost of raw materials. In addition, the treatment of cutting waste mortar can also effectively avoid environmental pollution problems. Therefore, recycling these cutting waste fluids is of great significance.

[0005] In addition to diamond abrasives, the solid particles generated during the cutting process also include broken silicon carbide fragments and metal impurities generated by cutting line wear. Due to the high viscosity of oil-based cutting fluids, small silicon carbide fragments tend to agglomerate and form groups with a particle size close to that of diamond abrasives. Therefore, how to separate the two is a difficult problem in the recycling process.

[0006] In the prior art, some people have tried to separate silicon carbide and diamond abrasives to effectively recycle diamond abrasives. However, the inventors found that when using the existing method for separation, a large number of fine silicon carbide fragments are easily adhered to the surface of the recovered diamond abrasives, and there are still a large number of silicon carbide particle agglomerates with a size similar to that of diamond particles. When reused, the fine silicon carbide particles are more likely to adhere to the cutting line, resulting in a decrease in the diamond carrying efficiency and affecting the cutting efficiency of the cutting fluid. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for recovering diamond abrasives in waste slurry from wire-cutting of silicon carbide wafers. The method of the present invention has the advantages of simple process, low cost, suitable for mass production, non-toxic and non-flammable degreasing liquid and high degreasing efficiency.

[0008] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0009] A method for recovering diamond abrasive in waste slurry from wire-cutting of silicon carbide wafers comprises the following steps:

[0010] Adding water to the waste cutting mortar, stirring and ultrasonically treating, to obtain a mixed slurry A;

[0011] The mixed slurry A is subjected to high-speed centrifugation to obtain solid B;

[0012] Solid B is mixed with hot alkaline solution, and after ultrasonic treatment, it is naturally precipitated to obtain solid C;

[0013] After mixing solid C with a strong acid solution, and then subjecting to ultrasonic treatment, solid D is obtained;

[0014] The solid D is stirred and dispersed in an ethanol aqueous solution, and solid E is obtained after natural sedimentation, which is the diamond abrasive.

[0015] In the prior art, in order to effectively improve the use efficiency of the cutting fluid, the waste slurry is sedimented or centrifuged, the obtained oil-solid mixture is cleaned, and the diamond particles are extracted.

[0016] However, the inventors found that the oil-solid mixture obtained by directly sedimenting or centrifuging the waste cutting mortar cannot be effectively separated, and the ultrafine silicon carbide particles will be adsorbed and wrapped on the surface of the diamond particles through the viscosity of the oil, and cannot be cleaned and separated by conventional methods to obtain high-purity diamond particles. In order to effectively improve the diamond extraction rate, it is necessary to perform multiple batches of repeated cleaning and separation operations on the oil-solid mixture, and the process is complicated. The ultrafine silicon carbide fragments or agglomerates attached to the surface of the diamond particles will be carried on the cutting line with the repeated configuration process of the mortar, reducing the adhesion rate of the diamond on the cutting line and resulting in a decrease in cutting efficiency. The inventors found through experiments that when water is added to the waste cutting mortar and ultrasonic treatment is performed, the oil-based waste mortar can be effectively diluted, the agglomerated fine silicon carbide particles can be dispersed, and the concentration of residual oil on the surface of the silicon carbide particles can be reduced, reducing its adhesion performance, and achieving an effective removal effect.

[0017] When the well-dispersed solid mixture is subjected to hot alkali ultrasonic treatment, the residual oil on the surface of the solid particles can be removed, thereby avoiding the re-agglomeration of silicon carbide particles and the adhesion of silicon carbide particles to the surface of diamond particles, and improving the surface cleanliness of the recovered diamond particles. When the extracted diamond abrasives are used to prepare cutting fluid again, the cutting efficiency and use time of the cutting fluid can be effectively improved.

[0018] In addition, the inventors have found through experiments that when separating diamond abrasives and silicon carbide particles in the natural sedimentation step, if additives such as dispersants are added to improve the separation efficiency, these additives will remain on the surface of the diamond abrasives to form a film, affecting the cutting performance of the diamond abrasives.

[0019] In the present invention, the diamond abrasive grains and silicon carbide grains can be naturally separated by sedimentation in ethanol water, and the ethanol and water remaining on the surface of the separated diamond abrasive grains can be effectively removed during the drying process, thereby ensuring the cleanliness of the surface of the diamond abrasive grains and ensuring the cutting performance of the reconfigured cutting fluid.

[0020] In some embodiments, the volume ratio of the cutting waste slurry to water is 1:0.5-10, preferably 3-10.

[0021] Preferably, when preparing the mixed slurry A, the ultrasonic treatment time is 1-10 h and the ultrasonic temperature is 20-90°C.

[0022] Preferably, the mixed slurry A is centrifuged at a speed of 5000-15000 g and the centrifugation time is 30-150 min.

[0023] Preferably, the temperature of high-speed centrifugation of the mixed slurry A is 0-35°C.

[0024] In some embodiments, the alkaline substance in the hot alkaline solution is one of potassium hydroxide, sodium hydroxide or potassium carbonate or a mixture thereof.

[0025] Preferably, the mass fraction of alkaline substances in the hot alkaline solution is 5%-50%. To ensure the removal effect of oil pollution, the amount of alkaline substances should not be too low; to save costs, the amount of drugs should not be too high.

[0026] Preferably, the temperature of the hot alkaline solution is 50-90°C.

[0027] Preferably, after the solid B is mixed with the hot alkaline solution, the ultrasonic treatment time is 1-10 hours. Too low ultrasonic time and temperature will lead to incomplete removal of oil stains, thereby affecting the separation effect.

[0028] In some embodiments, the strong acid is selected from sulfuric acid, nitric acid or hydrofluoric acid or a mixture thereof.

[0029] Preferably, the concentration of the strong acid in the strong acid solution is 0.1-5 M. To ensure that the metal impurities in the waste mortar are thoroughly cleaned, the concentration of the strong acid solution should not be too low; to save costs, the concentration of the strong acid should not be too high.

[0030] Preferably, after the strong acid solution is mixed with the solid C, the temperature of the ultrasonic treatment is 20-90° C., and the time of the ultrasonic treatment is 1-10 hours. To ensure that the acid cleaning is thorough, the time and temperature of the ultrasonic treatment should not be too low.

[0031] In some embodiments, the volume fraction of ethanol in the ethanol aqueous solution is 10%-80%.

[0032] Preferably, in the ethanol aqueous solution, the volume fraction of ethanol is 10%-80%, preferably 20%-50%, and more preferably 30%-50%.

[0033] Preferably, the solid D is stirred in the ethanol aqueous solution for 10-60 minutes. Too low or too high ethanol concentration will affect the sedimentation rate of silicon carbide particles in the solution; to ensure that the solid particles are evenly mixed in the solution, the stirring time should not be too short.

[0034] Preferably, the natural sedimentation time of the solid in the ethanol aqueous solution is 12-20 hours each time, and the sedimentation is repeated 3-10 times, preferably 3-6 times.

[0035] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0036] The present invention adds water to the waste mortar of cutting fluid, and then centrifuges at high speed after ultrasonic treatment to obtain a solid mixture of diamond powder; then, a strong alkaline solution is added. Under high temperature conditions, the viscosity of the oil is reduced, making it easier to mix with the alkaline solution, thereby accelerating the reaction rate. Acidification treatment is then performed. The metal impurities in the waste mortar are mainly iron elements. The addition of a strong acid solution can remove the metal impurities introduced during the processing; finally, an ethanol aqueous solution is added to the waste mortar. Since the diamond abrasive grains and silicon carbide particles have different sedimentation rates in the ethanol aqueous solution, the diamond abrasive can be recovered and separated through natural sedimentation. The method of the present invention has the advantages of simple process, low cost, and suitability for mass production. The degreasing liquid is non-toxic, non-flammable, and highly effective in degreasing. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0038] Figure 1 It is solid B obtained by high-speed centrifugation of waste mortar;

[0039] Figure 2is a scanning electron microscope (SEM) image of solid E (diamond) recovered in Example 1;

[0040] Figure 3 is a scanning electron microscope (SEM) image of solid E (diamond) recovered in Comparative Example 1. DETAILED DESCRIPTION

[0041] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0042] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0043] Example 1

[0044] A method for recovering diamond abrasive in waste slurry from wire-cutting of silicon carbide wafers comprises the following steps:

[0045] Step 1: Mix 2kg of cutting waste mortar and 500g of deionized water at a stirring speed of 200r / min -1 , the time is 2h to obtain mixed slurry A;

[0046] Step 2: centrifuging the mixed slurry A at 30° C. and 5000 g for 40 min to obtain solid B;

[0047] Step 3: Mix solid B with a 10% by mass potassium hydroxide solution, and ultrasonicate at 60° C. for 2 h to obtain solid C;

[0048] Step 4: Mix solid C with 1 M nitric acid and ultrasonicate at 40° C. for 2 h to obtain solid D;

[0049] Step 5: Disperse solid D in 30% ethanol aqueous solution, stir for 20 min, settle for 12 h each time, settle 5 times, and dry to obtain solid E (diamond).

[0050] Example 2

[0051] A method for recovering diamond abrasive in waste slurry from wire-cutting of silicon carbide wafers comprises the following steps:

[0052] Step 1: Mix 2kg of cutting waste mortar and 1kg of deionized water at a stirring speed of 200r / min -1 , the time is 2h to obtain mixed slurry A;

[0053] Step 2: centrifuge the mixed slurry A at 30°C and 7000g for 30 minutes to obtain solid B;

[0054] Step 3: Mix solid B with a 20% by mass potassium hydroxide solution, and ultrasonicate at 30° C. for 2 h to obtain solid C;

[0055] Step 4: Mix solid C with 1M hydrochloric acid and ultrasonicate at 40°C for 2h to obtain solid D;

[0056] Step 5: Disperse solid D in 30% ethanol aqueous solution, stir for 20 min, settle for 12 h each time, settle 5 times, and dry to obtain solid E (diamond).

[0057] Example 3

[0058] A method for recovering diamond abrasive in waste slurry from wire-cutting of silicon carbide wafers comprises the following steps:

[0059] Step 1: Mix 2kg of cutting waste mortar and 2kg of deionized water at a stirring speed of 200r / min -1 , the time is 2h to obtain mixed slurry A;

[0060] Step 2: centrifuge the mixed slurry A at 30° C. and 8000 g for 40 min to obtain solid B;

[0061] Step 3: Mix solid B with a 15% by mass potassium hydroxide solution, and ultrasonicate at 40° C. for 2 h to obtain solid C;

[0062] Step 4: Mix solid C with 0.5 M nitric acid and ultrasonicate at 40 °C for 2 h to obtain solid D;

[0063] Step 5: Disperse solid D in 40% ethanol aqueous solution, stir for 20 min, settle for 6 h each time, settle 5 times, and dry to obtain solid E (diamond).

[0064] Comparative Example 1

[0065] The difference from Example 1 is that the hot alkali ultrasonic cleaning step is omitted.

[0066] A method for recovering diamond abrasive in waste slurry from wire-cutting of silicon carbide wafers comprises the following steps:

[0067] Step 1: Mix 2kg of waste mortar and 500g of deionized water at a stirring speed of 200r / min -1 , the time is 2h to obtain mixed slurry A;

[0068] Step 2: centrifuging the mixed slurry A at 30° C. and 5000 g for 40 min to obtain solid B;

[0069] Step 3: Mix solid B with 1 M nitric acid and ultrasonicate at 40° C. for 2 h to obtain solid D;

[0070] Step 4: Disperse solid D in 30% ethanol aqueous solution, stir for 20 min, settle for 12 h each time, settle 5 times, and dry to obtain solid E (diamond).

[0071] Figure 2 is a SEM image of solid E (diamond) recovered in Example 1, Figure 3 This is the SEM image of the diamond recovered in Comparative Example 1. Figure 3 The surface of diamond abrasive grains that have not been cleaned with hot alkaline solution adsorbs a large amount of silicon carbide particles, which is caused by the residual oil stains that have not been cleaned; Figure 2 There are only a few silicon carbide particles on the surface of the diamond abrasive grains after cleaning, which shows that cleaning with hot alkaline solution is important for recovering diamond powder with clean surface from waste mortar.

[0072] Comparative Example 2

[0073] The difference from Example 1 is that the step of mixing the waste cutting mortar with deionized water in step 1 of Example 1 is omitted, and the waste cutting mortar is directly centrifuged to obtain solid B. The other steps are the same as those in Example 1.

[0074] A method for recovering diamond abrasive in waste slurry from wire-cutting of silicon carbide wafers comprises the following steps:

[0075] Step 1: 2 kg of cutting waste mortar is centrifuged at 30° C. and 5000 g for 40 min to obtain solid A;

[0076] Step 2: solid A is mixed with a 10% by mass potassium hydroxide solution, and subjected to ultrasonic treatment at 60° C. for 2 h to obtain solid B;

[0077] Step 4: Mix solid B with 1 M nitric acid and ultrasonicate at 40° C. for 2 h to obtain solid C;

[0078] Step 5: Disperse solid C in 30% ethanol aqueous solution, stir for 20 min, settle for 12 h each time, settle 5 times, and dry to obtain solid D (diamond). The surface of the recovered diamond abrasive grains adsorbs a large amount of silicon carbide particles.

[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for recovering diamond abrasive from waste slurry from wire-cutting of silicon carbide wafers. Features: The steps include: Adding water to the waste cutting mortar, stirring and ultrasonically treating, to obtain a mixed slurry A; The mixed slurry A is subjected to high-speed centrifugation to obtain solid B; Solid B is mixed with hot alkaline solution, and after ultrasonic treatment, it is naturally precipitated to obtain solid C; After mixing solid C with a strong acid solution, and then subjecting to ultrasonic treatment, solid D is obtained; The solid D is stirred and dispersed in an ethanol aqueous solution, and solid E is obtained after natural sedimentation, which is the diamond abrasive.

2. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 1, Features: The volume ratio of the waste cutting mortar to water is 1:0.5-10, preferably 3-10; Preferably, when preparing the mixed slurry A, the ultrasonic treatment time is 1-10h and the ultrasonic temperature is 20-90°C; Preferably, the mixed slurry A is centrifuged at a speed of 5000-15000 g for a time of 30-150 min; Preferably, the temperature of high-speed centrifugation of the mixed slurry A is 0-35°C.

3. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 1, Features: The alkaline substance in the hot alkaline solution is one of potassium hydroxide, sodium hydroxide or potassium carbonate or a mixture thereof; Preferably, the mass fraction of the alkaline substance in the hot alkaline solution is 5%-50%.

4. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 3, Features: The temperature of the hot alkali solution is 50-90°C; Preferably, after the solid B is mixed with the hot alkaline solution, the ultrasonic treatment time is 1-10 hours.

5. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 1, Features: The strong acid is selected from sulfuric acid, nitric acid or hydrofluoric acid or a mixture thereof.

6. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 5, Features: The concentration of the strong acid in the strong acid solution is 0.1-5M.

7. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 5, Features: After the strong acid solution is mixed with the solid C, the temperature of ultrasonic treatment is 20-90° C., and the time of ultrasonic treatment is 1-10 h.

8. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 1, Features: In the ethanol aqueous solution, the volume fraction of ethanol is 10%-80%.

9. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 8, Features: In the ethanol aqueous solution, the volume fraction of ethanol is 30%-50%.

10. The method for recovering diamond abrasive from waste slurry produced by wire sawing of silicon carbide wafers according to claim 9, Features: The stirring time of solid D in the ethanol aqueous solution is 10-6 0min; Preferably, the natural sedimentation time of solid D in the ethanol aqueous solution is 12-20 hours each time, and the sedimentation is repeated 3-10 times, preferably 3-6 times.

Citation Information

Patent Citations

  • Process for recovering polyethylene glycol and silicon carbide in waste mortar from silicon wafer wire cutting

    CN101474511A

  • Diamond abrasive material impurity removing method

    CN104624358A

  • Recovery method of silicon carbide crystal mortar linear cutting waste liquid

    CN112209380A

  • Method for recycling diamond abrasive resources after silicon carbide fine grinding

    CN112978728A

  • Method for recovering abrasive particles and basic solvent in silicon carbide wafer multi-wire cutting mortar