Preparation method of hollow laser fiber and method for detecting silver ions
By sequentially coating the inner surface of a silica glass tube with polymer, elemental Ag and silver iodide layers, a hollow laser fiber is prepared, which solves the problem of large transmission loss of mid-infrared electromagnetic radiation in the existing technology and achieves lower loss and higher Hollow laser fiber for transmitting power.
Patent Information
- Application Number
- CN202410732593.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-29
AI Technical Summary
Existing flexible hollow fiber waveguides suffer large losses when transmitting mid-infrared electromagnetic radiation and cannot withstand large transmission powers, making it difficult to meet the transmission needs of high-energy CO2 lasers.
The inner surface of a silica glass tube is coated with a polymer layer, an elemental Ag layer and a silver iodide layer in sequence. The elemental Ag layer is formed through the reaction of the silver ammonia complex and the reducing agent solution, and then a silver iodide layer is generated on the elemental Ag layer to prepare a hollow Laser fiber.
It achieves lower loss when transmitting mid-infrared electromagnetic radiation in a near-Gaussian mode, and can withstand greater transmission power, especially the loss at 3μm wavelength is less than 0.5dB/m, and does not melt under 30W power.
Smart Images

Figure CN118851594A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hollow waveguides, and in particular relates to a method for preparing a hollow laser optical fiber and a method for detecting silver ions. Background Art
[0002] CO2 lasers are widely used in medicine, industry and military, and a large number of optical fibers and hollow waveguides are used as transmission media for lasers. Compared with the quartz optical fibers used for communications in the past, cavity waveguides have been proven to have excellent transmission characteristics for high-energy CO2 lasers with relatively large wavelengths, which has huge commercial advantages.
[0003] Hollow waveguides with dielectric coatings for transmitting electromagnetic waves were studied as early as 1950. However, it was not until 1983 that hollow waveguides with dielectric layers for transmitting infrared light in the CO2 laser band were successfully developed. Since then, other researchers have proposed various methods for manufacturing hollow waveguides. Hollow waveguides are now widely used in various fields such as medical treatment, industrial processing and optical transmission. In particular, lasers with wavelengths of 10.6μm and 0.6328μm are particularly suitable for transmission in hollow waveguides.
[0004] U.S. Patent US005440664A discloses a flexible hollow fiber waveguide for transmitting mid-infrared radiation with low attenuation and a method for manufacturing such a waveguide, which meets the demand for a flexible mid-infrared laser transmission medium with relatively low loss. The waveguide provided is used to transmit mid-infrared electromagnetic radiation in a near-Gaussian mode, with a loss of less than 1.5 dB / m.
[0005] However, the loss of the flexible hollow fiber waveguide disclosed in the above-mentioned US patent is still relatively large. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a hollow laser optical fiber and a method for detecting silver ions. The hollow laser optical fiber obtained by the preparation method provided by the present invention has lower loss when used as a waveguide for transmitting mid-infrared electromagnetic radiation in a near-Gaussian mode and can withstand a larger transmission power.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a hollow laser optical fiber, wherein the hollow laser optical fiber comprises a silica glass tube, a polymer layer, a single substance Ag layer and a silver iodide layer sequentially arranged on the inner surface of the silica glass tube; the preparation method comprises the following steps:
[0009] Coating a polymer on the inner surface of the silica glass tube to obtain a silica glass tube with the inner surface coated with the polymer;
[0010] Injecting a silver-ammine complex solution and a reducing agent solution into a silica glass tube whose inner surface is coated with a polymer to react, thereby obtaining a single-substance Ag layer on the surface of the polymer, and obtaining a silica glass tube having a single-substance Ag layer on the inner surface;
[0011] An organic solution containing iodine is injected into a silicon dioxide glass tube having a single substance Ag layer on the inner surface for reaction, and a silver iodide layer is generated on the surface of the single substance Ag layer; and the hollow laser optical fiber is obtained.
[0012] Preferably, the method for preparing the silver ammonia complex solution comprises the following steps:
[0013] (1) adding an ammonium hydroxide aqueous solution dropwise to a silver nitrate aqueous solution to obtain a silver nitrate / ammonium hydroxide solution;
[0014] (2) mixing the silver nitrate / ammonium hydroxide solution and the sodium hydroxide aqueous solution to obtain a mixed solution;
[0015] (3) Adding an aqueous ammonium hydroxide solution dropwise to the mixed solution to obtain a silver ammine complex solution.
[0016] Preferably, the molar concentration of the silver nitrate aqueous solution is 0.1-0.2 mol / L.
[0017] Preferably, the mass percentage of the aqueous ammonium hydroxide solution used in step (1) and step (3) is 10-20%.
[0018] Preferably, the mass ratio of the silver nitrate in the silver nitrate aqueous solution to the sodium hydroxide in the sodium hydroxide aqueous solution is (1-1.3):0.22.
[0019] Preferably, the reducing solution is a dextrose aqueous solution, and the mass percentage of the dextrose aqueous solution is 3-10%.
[0020] Preferably, the volume ratio of the silver-ammine complex solution to the reducing solution is 1:1.
[0021] Preferably, the organic solution containing elemental iodine comprises elemental iodine and cyclohexane; the ratio of the mass of the elemental iodine to the volume of the cyclohexane is (1-2) g:100 mL.
[0022] The present invention provides a method for detecting silver ions, comprising the following steps:
[0023] Mix the silver ammine complex solution, reducing agent solution and EDTA, and observe whether a silver mirror reaction occurs.
[0024] Preferably, the method for preparing the silver ammonia complex solution comprises the following steps:
[0025] (1) adding an ammonium hydroxide aqueous solution dropwise to a silver nitrate aqueous solution to obtain a silver nitrate / ammonium hydroxide solution;
[0026] (2) mixing the silver nitrate / ammonium hydroxide solution and the sodium hydroxide aqueous solution to obtain a mixed solution;
[0027] (3) adding an aqueous ammonium hydroxide solution dropwise to the mixed solution to obtain a silver ammine complex solution;
[0028] The mass ratio of silver nitrate to ethylenediaminetetraacetic acid in the silver nitrate aqueous solution is (1-1.3):2.
[0029] The present invention provides a method for preparing a hollow laser optical fiber, the hollow laser optical fiber comprising a silica glass tube, a polymer layer, a single substance Ag layer and a silver iodide layer sequentially arranged on the inner surface of the silica glass tube; the preparation method comprises the following steps: coating a polymer on the inner surface of the silica glass tube to obtain a silica glass tube with a polymer coated on the inner surface; injecting a silver ammonia complex solution and a reducing agent solution into the silica glass tube with a polymer coated on the inner surface for reaction, obtaining a single substance Ag layer on the polymer surface, and obtaining a silica glass tube with a single substance Ag layer on the inner surface; injecting an organic solution containing single substance iodine into the silica glass tube with a single substance Ag layer on the inner surface for reaction, generating a silver iodide layer on the surface of the single substance Ag layer; and obtaining the hollow laser optical fiber. The hollow laser optical fiber prepared by the preparation method provided by the present invention has lower loss when used for waveguides that transmit mid-infrared electromagnetic radiation in a near-Gaussian mode, and can withstand greater transmission power. The results of the examples show that the hollow laser fiber prepared by the preparation method provided by the present invention can withstand considerable power, will not melt when transmitting a power of 30 W, and has a loss of less than 0.5 dB / m at a wavelength of 3 μm. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a physical picture of the carbon dioxide hollow laser optical fiber prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing a hollow laser optical fiber, wherein the hollow laser optical fiber comprises a silica glass tube, a polymer layer, a single substance Ag layer and a silver iodide layer sequentially arranged on the inner surface of the silica glass tube; the preparation method comprises the following steps:
[0032] Coating a polymer on the inner surface of the silica glass tube to obtain a silica glass tube with the inner surface coated with the polymer;
[0033] Injecting a silver-ammine complex solution and a reducing agent solution into a silica glass tube whose inner surface is coated with a polymer to react, thereby obtaining a single-substance Ag layer on the surface of the polymer, and obtaining a silica glass tube having a single-substance Ag layer on the inner surface;
[0034] An organic solution containing iodine is injected into a silicon dioxide glass tube having a single substance Ag layer on the inner surface for reaction, and a silver iodide layer is generated on the surface of the single substance Ag layer; and the hollow laser optical fiber is obtained.
[0035] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0036] The present invention provides a method for preparing a hollow laser fiber, wherein the hollow laser fiber comprises a silica glass tube, a polymer layer, a single Ag layer and a silver iodide layer sequentially arranged on the inner surface of the silica glass tube. The polymer layer preferably comprises polymethyl acrylate (PMMA) or polyvinyl alcohol (PVA).
[0037] The present invention coats the inner surface of the silica glass tube with a polymer to obtain a silica glass tube with the inner surface coated with a polymer. In the present invention, the polymer preferably includes polymethyl acrylate (PMMA) or polyvinyl alcohol (PVA).
[0038] After obtaining the silica glass tube with the inner surface coated with the polymer, the present invention injects the silver ammonia complex solution and the reducing agent solution into the silica glass tube with the inner surface coated with the polymer to react, obtains a single substance Ag layer on the surface of the polymer, and obtains the silica glass tube with the single substance Ag layer on the inner surface.
[0039] In the present invention, the method for preparing the silver ammonia complex solution preferably comprises the following steps:
[0040] (1) adding an ammonium hydroxide aqueous solution dropwise to a silver nitrate aqueous solution to obtain a silver nitrate / ammonium hydroxide solution;
[0041] (2) mixing the silver nitrate / ammonium hydroxide solution and the sodium hydroxide aqueous solution to obtain a mixed solution;
[0042] (3) Adding an aqueous ammonium hydroxide solution dropwise to the mixed solution to obtain a silver ammine complex solution.
[0043] The present invention drips an aqueous solution of ammonium hydroxide into an aqueous solution of silver nitrate to obtain a silver nitrate / ammonium hydroxide solution. The method for preparing the aqueous solution of silver nitrate is preferably: dissolving the silver nitrate in water to obtain the aqueous solution of silver nitrate. The purity of the silver nitrate is preferably 99.999%. The water used for the dissolution is preferably distilled deionized water. The molar concentration of the aqueous solution of silver nitrate is preferably 0.1-0.2 mol / L, more preferably 0.1692 mol / L. The mass percentage of the aqueous solution of ammonium hydroxide is preferably 10-20%. The dripping speed is preferably 1-2 mL / min (observe the reaction progress, adjust the dripping speed, ensure that the reaction proceeds at an appropriate rate, and the precipitation is formed uniformly.). During the dripping process, silver nitrate and ammonium hydroxide react to generate silver hydroxide, thereby forming a brown precipitate to obtain the silver nitrate / ammonium hydroxide solution. The volume ratio of the aqueous solution of silver nitrate to the aqueous solution of ammonium hydroxide is preferably 1:1.
[0044] After obtaining the silver nitrate / ammonium hydroxide solution, the present invention mixes the silver nitrate / ammonium hydroxide solution and the sodium hydroxide aqueous solution to obtain a mixed solution. In the present invention, the method for preparing the sodium hydroxide aqueous solution is preferably: dissolving the sodium hydroxide in water to obtain the sodium hydroxide aqueous solution. The water used for the dissolution is preferably distilled water, and the ratio of the mass of the sodium hydroxide to the volume of the water is preferably (1-1.3) g:100 mL, and specifically preferably 0.22 g:100 mL. The mass ratio of the silver nitrate in the silver nitrate aqueous solution to the sodium hydroxide in the sodium hydroxide aqueous solution is preferably (1-1.3):0.22, and more preferably 1.15:0.22. In the present invention, the sodium hydroxide aqueous solution is added to the silver nitrate / ammonium hydroxide solution as a regulator to adjust the speed of the subsequent reduction reaction. The sodium hydroxide aqueous solution is a speed regulator of the reduction reaction. As the alkalinity in the solution increases, the reduction speed is accelerated. However, if the alkalinity of the solution is too high, it will promote the self-decomposition of the silver ammonia complex solution. Therefore, the amount of sodium hydroxide aqueous solution added should be controlled, otherwise the brown silver hydroxide precipitate will immediately decompose into a dark brown silver oxide precipitate.
[0045] After obtaining the mixed solution, the present invention drips an aqueous ammonium hydroxide solution into the mixed solution to obtain a silver ammonia complex solution. In the present invention, the mass percentage of the aqueous ammonium hydroxide solution is 10-20%, more preferably 15%. The volume ratio of the mixed solution to the aqueous ammonium hydroxide solution is preferably 1:1. The dripping speed is preferably 1-2 mL / min. The present invention drips an aqueous ammonium hydroxide solution into the mixed solution, and the mass percentage of the aqueous ammonium hydroxide solution is preferably 10-20%, which can form a colorless and transparent silver ammonia complex solution, and then drips an aqueous sodium hydroxide solution, the stability of the silver ammonia complex ion is increased, which is beneficial to improve the stability of the silver ammonia complex solution (plating solution).
[0046] In the present invention, the reducing solution is preferably a dextrose aqueous solution, and the mass percentage of the dextrose aqueous solution is preferably 3-10%, more preferably 5%.
[0047] In the present invention, the volume ratio of the silver-ammine complex solution to the reducing solution is preferably 1:1.
[0048] The present invention places the silica glass tube horizontally or vertically, and passes the silver ammonia complex solution and the reducing solution into the silica glass tube for silver mirror reaction. In the present invention, when the pore size of the silica glass tube (hollow laser fiber) is 320-700 μm, the flow rate of the silver ammonia complex solution during the mixing is preferably 100-250 mL / hour, and the flow rate of the reducing solution is preferably 100-250 mL / hour. In a specific embodiment of the present invention, the pore size of the silica glass tube (hollow laser fiber) is preferably 700 μm, the flow rate of the silver ammonia complex solution during the mixing is preferably 250 mL / hour, and the flow rate of the reducing solution is preferably 250 mL / hour. In a specific embodiment of the present invention, the pore size of the silica glass tube (hollow laser fiber) is preferably 530 μm or 320 μm, the flow rate of the silver ammonia complex solution during the mixing is preferably 100 mL / hour, and the flow rate of the reducing solution is preferably 100 mL / hour.
[0049] As one or more embodiments of the present invention, the present invention pressurizes the reaction solution obtained by the silver ammonia complex solution and the reducing solution, and passes the reaction solution into the silica glass tube to perform a silver mirror reaction, and the pressurization is preferably performed using a peristaltic pump.
[0050] As one or more embodiments of the present invention, the present invention forms a negative pressure in the silica glass tube by evacuating one end of the silica glass tube, so that a reaction solution obtained by a silver ammonia complex solution and a reducing solution is passed through the other end of the silica glass tube to carry out a silver mirror reaction.
[0051] As one or more embodiments of the present invention, when the silica glass tube is placed horizontally, the silica glass tube is preferably rotated along the long axis direction during the silver mirror reaction, and the rotation angle is preferably 180°. The present invention preferably can prepare a more uniform single-substance Ag layer by preferably rotating the silica glass tube along the long axis direction during the silver mirror reaction.
[0052] As one or more embodiments of the present invention, during the silver mirror reaction, the present invention changes the flow direction of the reaction solution. The specific implementation of changing the flow direction of the reaction solution is preferably: changing the port through which the reaction solution enters the silica glass tube, or making the reaction solution flow in the silica glass tube in reverse. The number of changes in the flow direction is preferably 1.
[0053] As one or more embodiments of the present invention, after the reaction solution passes through the silica glass tube, the obtained post-reaction solution is preferably recycled.
[0054] In the present invention, the temperature of the silver mirror reaction is preferably room temperature, and the thickness of the single-substance Ag layer obtained after the silver mirror reaction is preferably 7 to 10 μm. (The time of the silver mirror reaction is preferably 10 to 15 minutes.)
[0055] After the silver mirror reaction is completed, a plated tube is obtained. The present invention preferably rinses and dries the plated tube in sequence, wherein the rinsing is preferably performed with a non-reactive rinsing solution, wherein the non-reactive solution is preferably an ethanol aqueous solution, wherein the mass percentage of ethanol in the ethanol aqueous solution is preferably 91%. The drying is preferably performed with compressed air purging and nitrogen purging in sequence. The nitrogen purging time is preferably 120 minutes.
[0056] After obtaining the silica glass tube with a single substance Ag layer on the inner surface, the present invention injects an organic solution containing single substance iodine into the silica glass tube with a single substance Ag layer on the inner surface to react, thereby generating a silver iodide layer on the surface of the single substance Ag layer; and obtaining the hollow laser optical fiber.
[0057] In the present invention, the organic solution containing elemental iodine preferably comprises elemental iodine and cyclohexane; the ratio of the mass of the elemental iodine to the volume of the cyclohexane is preferably (1-2) g:100 mL.
[0058] As one or more embodiments of the present invention, the pore size of the silica glass tube (hollow laser fiber) is preferably 700 μm: when a peristaltic pump is used, the flow rate of the organic solution containing iodine should be set to about 22 mL / 5 minutes. When a vacuum pump is used, the flow rate of the organic solution containing iodine should be set to about 50 mL / 4.5 minutes.
[0059] As one or more embodiments of the present invention, the pore size of the silica glass tube (hollow laser fiber) is preferably 530 μm: when a peristaltic pump is used, the flow rate of the organic solution containing iodine should be set to about 20 mL / 4 minutes. When a vacuum pump is used, the flow rate of the organic solution containing iodine is set to about 40-60 mL / 4 minutes.
[0060] As one or more embodiments of the present invention, the pore size of the silica glass tube (hollow laser fiber) is preferably 320 μm: when a peristaltic pump is used, the flow rate of the organic solution containing elemental iodine is set to about 10-20 mL / 3 minutes.
[0061] After the silver iodide layer is prepared, a double-plated tube is obtained. The present invention preferably rinses and dries the double-plated tube in sequence, and the rinsing is preferably carried out using a non-reactive rinsing solution, and the non-reactive solution is preferably an ethanol aqueous solution, and the mass percentage of ethanol in the ethanol aqueous solution is preferably 91%. The drying is preferably carried out by compressed air purging and nitrogen purging in sequence. The compressed air time is preferably 120 minutes. The nitrogen purging time is preferably 120 minutes.
[0062] The present invention provides a method for detecting silver ions, comprising the following steps:
[0063] Mix the silver ammine complex solution, reducing agent solution and EDTA, and observe whether a silver mirror reaction occurs.
[0064] In the present invention, the preparation methods of the silver ammonia complex solution and the reducing solution are the same as those described above, and will not be described again.
[0065] In the present invention, the mass ratio of silver nitrate to ethylenediaminetetraacetic acid in the silver nitrate aqueous solution used in preparing the silver ammonia complex solution is preferably (1-1.3):2, and specifically preferably 1.15:2. In the present invention, the role of adding EDTA when the silver ammonia complex solution and the reducing solution are mixed is to detect the concentration of silver ions. The higher the purity of the silver ions detected, the more optimized the optical fiber transmission efficiency is. It can be understood that "the higher the purity of the silver ions, the better the silver plating effect, and the better the transmission efficiency of the finished product.
[0066] In the detection method provided by the present invention, the higher the purity of EDTA, the higher the concentration of silver ions detected by EDTA. High-purity EDTA can ensure accuracy and reproducibility, and can reduce the influence of foreign impurities on the test results. For EDTA, generally speaking, the higher the purity, the better. The role of adding EDTA is to form a complex with the silver ions in the solution through complexation, thereby separating the silver ions from the reducing agent and facilitating detection. The complex formed by EDTA and silver ions is stable, so the concentration of silver ions can be accurately measured.
[0067] The method for preparing a hollow laser optical fiber provided by the present invention comprises the following steps: after obtaining a silica glass tube with a polymer coated on the inner surface, the present invention preferably prepares a silver ammonia complex solution and a reducing agent solution, and then, according to the method for detecting silver ions provided by the present invention: mixing the silver ammonia complex solution, the reducing agent solution and EDTA, observing whether a silver mirror reaction occurs, and if a silver mirror reaction occurs, injecting the silver ammonia complex solution and the reducing agent solution into the silica glass tube with a polymer coated on the inner surface for reaction, obtaining a single substance Ag layer on the surface of the polymer, and obtaining a silica glass tube with a single substance Ag layer on the inner surface.
[0068] The hollow laser fiber prepared in the present invention is preferably a CO2 hollow laser fiber.
[0069] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0070] Example 1
[0071] The inner surface of the silica glass tube is coated with a polymer, wherein the polymer is polymethyl acrylate (PMMA) or polyvinyl alcohol (PVA), and the adhesion of silver is improved and the surface is protected by coating the polymer on the inner surface of the silica glass tube.
[0072] A. Silver ammonia complex solution
[0073] 1.15 g of 99.999% pure silver nitrate (AgNO3) was dissolved in 400 mL of distilled deionized water (H2O) to prepare a silver nitrate solution with a molar concentration of 0.1692 mol / L.
[0074] As the thickness increases, 1-2 mL of ammonium hydroxide aqueous solution (NH4OH; 15%) is added drop by drop each time, and a brown silver hydroxide precipitate begins to form. The chemical reaction that occurs is: AgNO3+NH4OH→Ag(OH)↓+NH4NO3, forming a brown precipitate to obtain a silver nitrate / ammonium hydroxide solution. Then 0.22 g of sodium hydroxide (NaOH) is dissolved in 100 mL of distilled water to form a sodium hydroxide solution as a regulator, which is added to 10-20 mL of silver nitrate / ammonium hydroxide solution to regulate the reduction reaction rate. The reduction reaction cannot react too fast. Sodium hydroxide is a rate regulator. As the alkalinity increases, the reduction rate increases. If the alkalinity is too high, it will promote the self-decomposition of the silver ammonia complex solution. The amount added should be controlled, otherwise the brown silver hydroxide precipitate will immediately decompose into a dark brown silver oxide precipitate. The chemical reaction that occurs is: 2AgOH→Ag2O↓+H2O. 3 mL of ammonium hydroxide aqueous solution (NH4OH; 15 wt%) was added to form a colorless and transparent silver ammonia complex solution, and the chemical reaction occurred was: Ag2O+4NH4OH→2Ag(NH3)2OH+3H2O. After adding sodium hydroxide solution, the stability of silver ammonia complex ions increased, which was beneficial to improve the stability of silver ammonia complex solution (plating solution).
[0075] B. Reducing agent solution
[0076] The reducing solution used was a dextrose aqueous solution (C6H 12 O6; 5wt% weight). The function of the reducing solution is to reduce the individual silver ions, and the chemical reaction that occurs is: Ag(NH3)2OH+C6H 12 O6→Ag↓+2NH3+H2O.
[0077] C. Silver-plated
[0078] 1. Preparation of mixed solution:
[0079] Prepare materials and equipment:
[0080] Silver ammine complex solution: Prepare in advance to ensure the appropriate concentration of silver ions.
[0081] Reducing agent solution: Prepared with dextrose, ensuring the concentration is 3%-10%, 5% in this embodiment.
[0082] Solid ethylenediaminetetraacetic acid (EDTA): used to detect free silver ions.
[0083] Precision electronic balance: used to accurately weigh EDTA.
[0084] Graduated cylinder: Measure the required volume of solution respectively.
[0085] Agitators and containers: used to mix solutions.
[0086] Steps:
[0087] 1. Use a measuring cylinder to measure 1 liter of the silver-ammine complex solution prepared in step A and 1 liter of the reducing agent solution prepared in step B. 2. Pour the silver-ammine complex solution into a stirring container and turn on the agitator to stir at a moderate speed. 3. Slowly add 1 liter of the reducing agent solution and continue stirring to ensure that the solution is evenly mixed. 4. Use a precision electronic balance to weigh 2 grams of solid EDTA. 5. Slowly add the weighed EDTA to the mixed solution and continue stirring until the EDTA is completely dissolved. 6. Check the solution and confirm the presence of silver ions in the solution by observing whether the silver mirror reaction occurs. The appearance of the silver mirror reaction indicates that there is a sufficient amount of silver ions in the solution. Let the mixed solution stand to ensure that the reaction is complete.
[0088] 2. Silver plating process:
[0089] Prepare silica glass tubes:
[0090] Select a silica glass tube with an appropriate pore size, usually 700 μm. Place the glass tube horizontally on the workbench, making sure both ends can be connected to the peristaltic pump delivery pipe.
[0091] Solution injection:
[0092] 1. Pour the mixed silver-ammine complex solution and reducing agent solution into the liquid storage container of the peristaltic pump. 2. Connect the delivery pipe of the peristaltic pump and insert one end of the pipe into the inlet end of the silica glass tube. 3. Set the flow parameters of the peristaltic pump so that the solution is evenly injected into the glass tube at a rate of 400-600mL / 2 hours. 4. Start the peristaltic pump and inject the mixed solution into the glass tube at a constant pressure to ensure that the solution flows evenly inside the glass tube.
[0093] Rotation of glass tube:
[0094] Use a dedicated rotating device to slowly rotate the glass tube at a speed of 0.5 rpm, so that it rotates 180° on the long axis each time. This operation helps to form a uniform silver coating on the inner wall of the glass tube and prevent uneven coating thickness due to gravity.
[0095] Rinse and dry:
[0096] 1. After the silver plating process is completed, rinse the inner wall of the glass tube with 91wt% ethanol solution to ensure that the residual chemicals are completely removed. 2. Use compressed air at a pressure of 10psi to purge the inside of the glass tube for 120 minutes for preliminary drying. 3. Then, use 99.999% pure nitrogen at a pressure of 10psi to purge the inside of the glass tube again for 120 minutes to ensure that the inside is completely dry to avoid residual solution or water vapor affecting subsequent processes.
[0097] D. Iodination Steps
[0098] First, 100 mL of cyclohexane is precisely mixed with 1-2 g of iodine in a warm ultrasonic bath to ensure that the iodine is fully dissolved. After mixing, the resulting solution is cooled to room temperature. Next, the volume of the resulting iodine / cyclohexane solution is precisely measured to form an optimal silver iodide layer with minimal loss and diffraction limitation (i.e., spatially coherent or Gaussian beam output) based on the desired aperture, target wavelength, and type of pump used.
[0099] The specific implementation steps are as follows:
[0100] 1. For 700μm optical fiber:
[0101] When using a peristaltic pump, the solution flow rate should be set to approximately 22 mL / 5 minutes.
[0102] When using a vacuum pump, the solution flow rate should be set to approximately 50 mL / 4.5 minutes.
[0103] 2. For 530μm optical fiber:
[0104] When using a peristaltic pump, the solution flow rate should be set to approximately 20 mL / 4 minutes.
[0105] When using a vacuum pump, the solution flow rate should be set to approximately 40-60 mL / 4 minutes.
[0106] 3. For 320μm optical fiber:
[0107] When using a peristaltic pump, the solution flow rate should be set to approximately 10-20 mL / 3 minutes.
[0108] NOTE: For this aperture, a vacuum pump cannot be used because the solution might freeze inside the waveguide.
[0109] After the plating is completed, the plated tube with the silver iodide layer needs to be rinsed with an ethanol solution. 91 wt% ethanol (chemical formula CH3CH2OH) is used for rinsing to remove the residues in the plated tube after the silver mirror reaction.
[0110] Finally, the rinsed plated tube needs to be dried. The specific steps of drying are as follows:
[0111] 1. Use compressed air to blow for 120 minutes to ensure initial drying.
[0112] 2. Then, nitrogen was purged for 120 minutes to further remove residual solvent and moisture.
[0113] After the above steps, a hollow optical fiber for CO2 laser can be obtained, which has excellent optical properties and low loss characteristics.
[0114] Figure 1This is a physical picture of the carbon dioxide hollow laser optical fiber prepared in Example 1 of the present invention.
[0115] The carbon dioxide hollow laser optical fiber prepared in this embodiment can withstand considerable power and does not melt when transmitting a power of about 30 W.
[0116] The carbon dioxide hollow laser fiber prepared in this embodiment is used as a waveguide for transmitting mid-infrared electromagnetic radiation in a near-Gaussian mode, and has a loss of less than 0.5 dB / m at a wavelength of 3 μm.
[0117] Example 2
[0118] The preparation method is basically the same as that of Example 1, except that: in step C. silver plating:
[0119] The flow rates of the silver-ammine complex solution and the reducing solution used for the 530 μm pore diameter optical fiber were both 100 mL / hour.
[0120] Example 3
[0121] The preparation method is basically the same as that of Example 1, except that: in step C. silver plating:
[0122] The flow rates of the silver-ammine complex solution and the reducing solution used for the 320 μm pore diameter optical fiber were both 100 mL / hour.
[0123] The optical fiber products prepared in the above-mentioned embodiments 1 to 3 were inspected by the Tianjian Medical Device Preparation Supervision and Inspection Center of the State Food and Drug Administration and were found to be qualified products.
[0124] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a hollow laser optical fiber, characterized in that: The hollow laser optical fiber comprises a silica glass tube, a polymer layer, a single substance Ag layer and a silver iodide layer sequentially arranged on the inner surface of the silica glass tube; the preparation method comprises the following steps: Coating a polymer on the inner surface of the silica glass tube to obtain a silica glass tube with the inner surface coated with the polymer; Injecting a silver-ammine complex solution and a reducing agent solution into a silica glass tube whose inner surface is coated with a polymer to react, thereby obtaining a single-substance Ag layer on the surface of the polymer, and obtaining a silica glass tube having a single-substance Ag layer on the inner surface; An organic solution containing iodine is injected into a silicon dioxide glass tube having a single substance Ag layer on the inner surface for reaction, and a silver iodide layer is generated on the surface of the single substance Ag layer; and the hollow laser optical fiber is obtained.
2. The preparation method according to claim 1, characterized in that: The preparation method of the silver ammine complex solution comprises the following steps: (1) adding an ammonium hydroxide aqueous solution dropwise to a silver nitrate aqueous solution to obtain a silver nitrate / ammonium hydroxide solution; (2) mixing the silver nitrate / ammonium hydroxide solution and the sodium hydroxide aqueous solution to obtain a mixed solution; (3) Adding an aqueous ammonium hydroxide solution dropwise to the mixed solution to obtain a silver ammine complex solution.
3. The preparation method according to claim 2, characterized in that: The molar concentration of the silver nitrate aqueous solution is 0.1-0.2 mol / L.
4. The preparation method according to claim 2, characterized in that: The mass percentage of the ammonium hydroxide aqueous solution used in step (1) and step (3) is 10-20%.
5. The preparation method according to claim 2, characterized in that: The mass ratio of the silver nitrate in the silver nitrate aqueous solution to the sodium hydroxide in the sodium hydroxide aqueous solution is (1-1.3):0.
22.
6. The preparation method according to claim 1, characterized in that: The reducing solution is a dextrose aqueous solution, and the mass percentage of the dextrose aqueous solution is 3-10%.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The volume ratio of the silver-ammine complex solution to the reducing solution is 1:
1.
8. The preparation method according to claim 1, characterized in that: The organic solution containing elemental iodine includes elemental iodine and cyclohexane; the ratio of the mass of the elemental iodine to the volume of the cyclohexane is (1-2) g:100 mL.
9. A method for detecting silver ions, characterized in that: The following steps are involved: Mix the silver ammine complex solution, reducing agent solution and EDTA, and observe whether a silver mirror reaction occurs.
10. The preparation method according to claim 9, characterized in that: The preparation method of the silver ammine complex solution comprises the following steps: (1) adding an ammonium hydroxide aqueous solution dropwise to a silver nitrate aqueous solution to obtain a silver nitrate / ammonium hydroxide solution; (2) mixing the silver nitrate / ammonium hydroxide solution and the sodium hydroxide aqueous solution to obtain a mixed solution; (3) adding an aqueous ammonium hydroxide solution dropwise to the mixed solution to obtain a silver ammine complex solution; The mass ratio of silver nitrate to ethylenediaminetetraacetic acid in the silver nitrate aqueous solution is (1-1.3):2.