A preparation method and application of multilayer silicon carbide etchant material
By regulating the crystal plane orientation and interface layer morphology of the silicon carbide layer, the problem of the multi-layer interface layer of SiC etchant material affecting thermal conductivity is solved, and the preparation of high-purity and high-density multi-layer silicon carbide material is achieved, which improves thermal conductivity Performance and structural stability extend service life.
Patent Information
- Application Number
- CN202411355373.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The multi-layer interface layer of SiC etchant material affects thermal conductivity and structural stability, resulting in its short service life in high-temperature etching environments and cannot operate at high speed for a long time.
By regulating the crystal plane orientation of the silicon carbide layer and the crystal morphology of the interface layer, a multi-layer silicon carbide etchant material is used, including graphite substrate deposition, graphite burning and high-temperature heat treatment to form a multi-purity and high-density multi-layer silicon carbide etchant material, including graphite substrate deposition, graphite burning and high-temperature heat treatment, to form a multi-purity and high-density The silicon carbide layer eliminates the influence of the interface layer and improves thermal conductivity.
The thermal conductivity and structural stability of the multi-layer silicon carbide etchant material are improved, so that it can maintain high-speed operation in a long-term etching environment and extend its service life.
Smart Images

Figure CN118851799B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon carbide etching bodies, in particular to a multilayer silicon carbide etching body material and a preparation method and application thereof. Background Art
[0002] SiC etching material is a key consumable in the plasma etching process of semiconductor materials. SiC etching material has extremely high purity requirements, so only CVD process can be used to grow SiC thick block, but due to the current CVD growth rate of SiC, a thick layer of SiC etching material needs to be deposited multiple times, but this process will produce multiple layers of silicon carbide interface layers, and the bonding strength and structure between different silicon carbide layers will affect the transmission of phonon electrons, which will seriously affect the thermal conductivity of the multi-layer silicon carbide etching material, making the temperature of the entire etching material uneven, resulting in a shortened service life of the SiC etching material, making it unable to operate uninterruptedly for a long time in a high-temperature etching environment; in addition, the uneven thermal conductivity of the SiC etching material will also cause an increase in thermal stress in some parts of its interior, seriously affecting the internal structure, thereby causing the material to crack, and it is impossible to guarantee long-term high-speed operation in an etching environment. Summary of the invention
[0003] In order to improve the above problems existing in the prior art, the present invention provides a method for preparing a multi-layer silicon carbide etchant material and the application of the multi-layer silicon carbide etchant material in ion etching technology. The multi-layer silicon carbide etchant material of the present invention has the characteristics of high purity and high density, avoids the influence of the interface layer between the multi-layer structure, so that the thermal conductivity of the multi-interface layer multi-layer silicon carbide etchant material formed is high, and can maintain high-speed operation in a long-term etching environment.
[0004] In order to achieve the above object, a first aspect of the present invention provides a method for preparing a multilayer silicon carbide etched body material, comprising the following steps:
[0005] (1) placing a graphite substrate in a deposition furnace so that it is parallel to the gas inlet of the deposition furnace, maintaining the pressure in the deposition furnace at 150 Pa to 350 Pa and the temperature at 400 to 600 ° C under vacuum for 15 to 30 minutes; introducing argon gas to the deposition pressure and raising the temperature to the deposition temperature;
[0006] (2) introducing MTS and hydrogen into the deposition furnace of step (1) at a molar mass ratio of 1:(20-40), maintaining the deposition pressure and deposition temperature in step (1), and performing a deposition process to obtain a first silicon carbide layer attached to the graphite substrate;
[0007] (3) subjecting the material obtained in step (2) to graphite sintering in a muffle furnace to obtain the first silicon carbide layer;
[0008] (4) placing the first silicon carbide layer obtained in step (3) into the deposition furnace again as a substrate, introducing MTS and hydrogen at a molar mass ratio of 1:(1-19), maintaining the deposition pressure and deposition temperature in step (1), and performing deposition treatment again to obtain a second silicon carbide layer attached to the first silicon carbide layer;
[0009] (5) Repeating steps (2) and (4) 2-3 times to obtain a multilayer silicon carbide layer in which the first silicon carbide layer and the second silicon carbide layer are stacked in sequence, and subjecting the multilayer silicon carbide layer to high-temperature heat treatment to obtain a multilayer silicon carbide etched body material;
[0010] The peak value of the (111) crystal plane orientation of the second silicon carbide layer accounts for 85% to 89%, and the peak value of the (222) crystal plane orientation accounts for 0.5% to 1.5%;
[0011] The grains included in the second silicon carbide layer are columnar crystals, and the width of the columnar crystals is 0.5 μm to 1.5 μm;
[0012] The grains contained in the first silicon carbide layer are granular, and the grain size thereof is 0.5 μm to 1.5 μm;
[0013] In step (1), step (2) and step (4), the conditions of the deposition treatment include: the deposition temperature is 900° C. to 1650° C., the deposition pressure is 9500 Pa to 80000 Pa, and the deposition time is 4 h to 12 h;
[0014] In step (5), argon gas is introduced during the high temperature heat treatment, the temperature of the high temperature heat treatment is 1700-1900°C, and the duration is 4-6 hours.
[0015] The second aspect of the present invention provides the use of the multi-layer silicon carbide etchant material prepared by the method for preparing the multi-layer silicon carbide etchant material described in the first aspect of the present invention in plasma etching technology.
[0016] Through the above technical solution, the present invention has at least the following advantages compared with the prior art:
[0017] The preparation method of the multilayer silicon carbide etching material of the present invention increases the bonding strength between different silicon carbide layers by regulating the crystal plane orientation of the silicon carbide layer and the crystal morphology and size of the interface layer, thereby improving the heat transfer efficiency of the multilayer silicon carbide etching body material and reducing the energy consumed by phonons during the transmission process to avoid scattering thereof, thereby improving the overall thermal conductivity of the multilayer silicon carbide etching body material.
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a SEM schematic diagram of columnar crystals provided in an embodiment of the present invention.
[0020] Figure 2 A SEM schematic diagram of a layered structure formed by a multi-layer silicon carbide etchant material provided in an embodiment of the present invention.
[0021] Figure 3 This is a SEM schematic diagram of the second silicon carbide layer provided in an embodiment of the present invention.
[0022] Figure 4 This is a schematic diagram of XRD of the second silicon carbide layer provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0023] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0024] A first aspect of the present invention provides a method for preparing a multilayer silicon carbide etchant material, comprising the following steps:
[0025] (1) placing a graphite substrate in a deposition furnace so that it is parallel to the gas inlet of the deposition furnace, maintaining the pressure in the deposition furnace at 150 Pa to 350 Pa and the temperature at 400 to 600 ° C under vacuum for 15 to 30 minutes; introducing argon gas to the deposition pressure and raising the temperature to the deposition temperature;
[0026] (2) introducing MTS and hydrogen into the deposition furnace of step (1) at a molar mass ratio of 1:(20-40), maintaining the deposition pressure and deposition temperature in step (1), and performing a deposition process to obtain a first silicon carbide layer attached to the graphite substrate;
[0027] (3) subjecting the material obtained in step (2) to graphite sintering in a muffle furnace to obtain the first silicon carbide layer;
[0028] (4) placing the first silicon carbide layer obtained in step (3) into the deposition furnace again as a substrate, introducing MTS and hydrogen at a molar mass ratio of 1:(1-19), maintaining the deposition pressure and deposition temperature in step (1), and performing deposition treatment again to obtain a second silicon carbide layer attached to the first silicon carbide layer;
[0029] (5) Repeating steps (2) and (4) 2-3 times to obtain a multilayer silicon carbide layer in which the first silicon carbide layer and the second silicon carbide layer are stacked in sequence, and subjecting the multilayer silicon carbide layer to high-temperature heat treatment to obtain a multilayer silicon carbide etched body material;
[0030] The peak value of the (111) crystal plane orientation of the second silicon carbide layer accounts for 85% to 89%, and the peak value of the (222) crystal plane orientation accounts for 0.5% to 1.5%;
[0031] The grains included in the second silicon carbide layer are columnar crystals, and the width of the columnar crystals is 0.5 μm to 1.5 μm;
[0032] The grains contained in the first silicon carbide layer are granular, and the grain size thereof is 0.5 μm to 1.5 μm;
[0033] In step (1), step (2) and step (4), the conditions of the deposition treatment include: the deposition temperature is 900° C. to 1650° C., the deposition pressure is 9500 Pa to 80000 Pa, and the deposition time is 4 h to 12 h;
[0034] In step (5), argon gas is introduced during the high temperature heat treatment, the temperature of the high temperature heat treatment is 1700-1900°C, and the duration is 4-6 hours.
[0035] From a microscopic perspective, the heat transfer mode of solid materials can be mainly divided into lattice vibration phonon heat transfer and electron free movement heat transfer. The main heat conduction mechanism of SiC material is its lattice vibration heat transfer, that is, phonon heat conduction. The atoms of non-metallic materials interact with each other to form a lattice network. The higher the temperature, the greater the thermal disorder of the particles, and the greater the amplitude of the atomic thermal vibration. The atoms with large thermal amplitude will drive the atoms with smaller thermal amplitude around them to vibrate together. As a result, the amplitude of the particles with weaker thermal amplitude will also increase, causing the transmission and transfer of phonons, triggering the transfer of heat. The existence of multiple interface layers will seriously hinder the transmission of phonon vibrations, consume the energy of phonon transmission, and reduce the heat transfer efficiency to eliminate the influence of the interface layer. Therefore, based on the above problems, the present invention stacks silicon carbide layers with different grain morphologies in sequence, and regulates the crystal plane orientation of the silicon carbide layer, the crystal morphology and size of the interface layer, so that after high-temperature heat treatment, new bonds can be formed between layers. Specifically, the small iodine grains at the interface between the first silicon carbide layer and the second silicon carbide layer will grow into large-sized grains together with the columnar crystals of the second silicon carbide layer after high-temperature heat treatment, thereby eliminating the influence of the interface layer between the multiple silicon carbide layers, reducing the energy consumed by phonon transmission of the multi-layer silicon carbide etching material, and improving the thermal conductivity of the material.
[0036] According to the preparation method of the present invention, in step (1), the graphite substrate is placed in a deposition furnace so that it is parallel to the gas inlet of the deposition furnace, which can improve the uniformity of deposition gas adhesion during chemical vapor deposition.
[0037] According to the preparation method of the present invention, in step (1), the pressure in the deposition furnace is 150Pa~350Pa, the temperature is 400~600°C, and the duration is 15~30min; the above process is a preheating process of the graphite substrate, which can remove impurities and oxides on the surface of the substrate and ensure that the gas contacts the pure substrate surface during the reaction process, thereby improving the quality of the deposited silicon carbide layer.
[0038] According to the preparation method of the present invention, in step (2), the molar mass ratio of MTS to hydrogen is 1:(20-40). Exemplarily, the molar mass ratio of MTS to hydrogen can be 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29, 1:30, 1:31, 1:32, 1:33, 1:34, 1:35, 1:36, 1:37, 1:38, or 1:40.
[0039] According to the preparation method of the present invention, in step (2), argon gas is introduced to the deposition pressure, and the temperature is raised to the deposition temperature. The introduction of argon gas during the deposition process can dilute the reaction gas, avoid defects in the silicon carbide layer caused by too fast a reaction, and further improve the overall quality of the deposited silicon carbide layer.
[0040] According to the preparation method of the present invention, in step (3), the material obtained in step (2) is subjected to graphite sintering in a muffle furnace to obtain a first silicon carbide layer. After the sintering treatment, the graphite substrate can be completely removed, leaving a pure silicon carbide layer as a substrate for the next deposition, i.e., the first silicon carbide layer.
[0041] According to the preparation method of the present invention, in step (4), the first silicon carbide layer obtained in step (3) is placed in the deposition furnace again as a substrate, MTS and hydrogen are introduced at a molar mass ratio of 1:(1-19), the deposition pressure and deposition temperature in step (1) are maintained, and the deposition process is performed again to obtain a second silicon carbide layer attached to the first silicon carbide layer. The second silicon carbide layer is deposited on the surface of the first silicon carbide layer;
[0042] In step (4), the molar mass ratio of MTS to hydrogen is 1:(1-19). Exemplarily, the molar mass ratio of MTS to hydrogen can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, or 1:19.
[0043] According to the preparation method of the present invention, in step (5), steps (2) and (4) are repeated 2 to 3 times to obtain a multilayer silicon carbide layer in which the first silicon carbide layer and the second silicon carbide layer are sequentially stacked. It should be noted that in the process of repeating step (2), a new first silicon carbide layer will be deposited on the surface of the second silicon carbide layer substrate, and step (4) will be continued to be repeated, and a new second silicon carbide layer will be deposited on the surface of the new first silicon carbide layer substrate, and so on, which will not be repeated.
[0044] According to the preparation method of the present invention, the peak value proportion of the (111) crystal plane orientation of the second silicon carbide layer is 85%-89%. Exemplarily, the peak value proportion of the (111) crystal plane orientation of the second silicon carbide layer can be 85%, 86%, 87%, 88%, and 89%; the peak value proportion of the (222) crystal plane orientation is 0.5%-1.5%. Exemplarily, the peak value proportion of the (222) crystal plane orientation can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, and 1.5%; the second silicon carbide layer deposited by the preparation method of the present invention has a high (111) crystal plane orientation, which can induce the epitaxial layer to grow in the same direction and present a large-size columnar crystal morphology at the growth interface, thereby realizing precise control of the crystal orientation of the epitaxial layer, such as Figure 4 shown.
[0045] According to the preparation method of the present invention, the grains contained in the second silicon carbide layer are columnar crystals, and the width of the columnar crystals is 0.5μm~1.5μm. Exemplarily, the width of the columnar crystals can be 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm. Since the second silicon carbide layer has a high (111) crystal plane orientation, it can induce the epitaxial layer to grow in the same direction, and the grown grains are columnar. The width of the columnar crystals is 0.5μm~1.5μm, such as Figure 1 shown.
[0046] In a specific embodiment, the length of the columnar crystal is 30 μm to 120 μm. For example, the length of the columnar crystal can be 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, or 120 μm. The width of the columnar crystal of the second silicon carbide layer is narrower, and the length is relatively longer than the width. The length of the columnar crystal is 30 μm to 120 μm. Figure 3 As shown, the generation of grains of this shape can further optimize the propagation path of heat flow, improve the thermal stability and thermal conduction efficiency of the material in a high temperature environment, and thus improve the overall thermal conductivity of the multilayer silicon carbide etched body material.
[0047] In a specific embodiment, the grains contained in the first silicon carbide layer are granular, and the grain size thereof is 0.5 μm to 1.5 μm. Exemplarily, the grain size of the grains contained in the first silicon carbide layer can be 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, and 1.5 μm. The grains contained in the first silicon carbide layer are granular, and the width size is similar to that of the columnar crystals of the second silicon carbide layer. This design is more conducive to the growth of the columnar grain structure in the silicon carbide deposition layer when the first silicon carbide layer is used as a substrate, and it also helps to further improve the heat conduction at the interface of the multilayer silicon carbide etching material and improve the overall thermal conductivity of the material.
[0048] In a specific embodiment, the interface between the adjacent first silicon carbide layers is in the form of columnar crystals connected through the second silicon carbide layer. The first silicon carbide layer can provide a better growth substrate for the second silicon carbide layer, but the heat conduction may be slightly poor. Therefore, the present invention adopts a design of a first silicon carbide layer and a second silicon carbide layer stacked in sequence, such as Figure 2 As shown, the interface between adjacent first silicon carbide layers can be in the form of columnar crystals connected through the second silicon carbide layer, and efficient heat conduction between the interface layers can also be achieved, further eliminating uneven heat conduction inside the material.
[0049] In a specific embodiment, the total thickness of the adjacent first silicon carbide layer and the second silicon carbide layer between the two layers is 90μm~180μm. Exemplarily, the total thickness can be 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm. The adjacent first silicon carbide layer and the second silicon carbide layer between the two layers can form a relatively independent heat transfer unit. The total thickness of the heat transfer unit can reflect the size of the mixed grain structure formed by the granular grains and columnar crystal grains in the unit. The thickness ranges from 90μm to 180μm, indicating that the mixed grains in the heat transfer unit have a large size, which is more conducive to heat conduction inside the material.
[0050] In a specific embodiment, the thickness ratio of the first silicon carbide layer to the second silicon carbide layer is (1.1-1.3): 1. For example, the thickness ratio of the first silicon carbide layer to the second silicon carbide layer may be 1.1: 1, 1.2: 1, or 1.3: 1. By further adjusting the thickness ratio of the two silicon carbide layers, the overall thermal conductivity of the multilayer silicon carbide etching material can also be further improved.
[0051] In a specific embodiment, in step (1), step (2) and step (4), the conditions of the deposition treatment include: the deposition temperature is 900°C-1650°C, and illustratively, the deposition temperature can be 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C, 1550°C, 1600°C, 1650°C; the deposition pressure is 9500Pa-80000Pa ... pressure can be 9000Pa-1650°C. Typically, the deposition pressure may be 9500Pa, 10000Pa, 10500Pa, 11000Pa, 11500Pa, 12000Pa, 12500Pa, 13000Pa, 13500Pa, 14000Pa, 14500Pa, 15000Pa, 15500Pa, 16000Pa, 20000Pa, 30000Pa, 40000Pa, 50000Pa, 60000Pa, 70000Pa, 80000Pa; and the deposition time is 4-12h. It should be noted that the deposition temperature, deposition pressure and deposition time for depositing the first silicon carbide layer and the deposition of the second silicon carbide layer may be different, as long as they are within the given range.
[0052] In a specific embodiment, in step (3), oxygen is introduced during the graphite sintering process, and the graphite sintering temperature is 500-800°C. For example, the graphite sintering temperature can be 500°C, 600°C, 700°C, or 800°C. The duration is 10-20 hours. The graphite sintering process can completely remove the graphite, leaving pure silicon carbide as the next deposition substrate.
[0053] In a specific embodiment, in step (5), argon gas is introduced during the high temperature heat treatment, and the temperature of the high temperature heat treatment is 1700-1900°C. Exemplarily, the temperature of the high temperature heat treatment can be 1700°C, 1800°C, or 1900°C; and the duration is 4-6 hours.
[0054] The second aspect of the present invention provides the use of the multi-layer silicon carbide etchant material prepared by the method for preparing the multi-layer silicon carbide etchant material described in the first aspect of the present invention in plasma etching technology.
[0055] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] Unless otherwise specified, the materials and instruments used in the following examples are commercially available.
[0057] Example 1
[0058] For preparing a multi-layer silicon carbide etching body material, the method specifically comprises the following steps:
[0059] (1) Providing a graphite substrate, placing the graphite substrate in a deposition furnace so that it is parallel to the gas inlet of the deposition furnace, evacuating the furnace, maintaining the pressure in the deposition furnace at 250 Pa and the temperature at 500 ° C for 30 min; then introducing inert gas Ar and heating to a deposition temperature of 1250 ° C and a deposition pressure of 9500 Pa;
[0060] (2) The reaction gas MTS (methyltrichlorosilane) and hydrogen were introduced into the chemical vapor deposition equipment at a ratio of 1:30; the deposition temperature was maintained at 1250°C and the deposition pressure was maintained at 9500Pa;
[0061] (3) After chemical vapor deposition is completed, stop introducing the reaction gas and continue to introduce protective gas argon to cool down the temperature.
[0062] (4) The deposited silicon carbide with graphite as the substrate is placed in a muffle furnace and oxygen is introduced. It is calcined at 500°C for 4 hours to completely remove the graphite, leaving a pure SiC layer as the substrate for the next deposition. The SiC layer is the first silicon carbide layer. The grain size distribution of the formed first silicon carbide layer is in the range of 0.5μm to 1.5μm.
[0063] (5) The above SiC layer is placed as a deposition substrate in a CVD deposition furnace, and the reaction gas MTS (methyltrichlorosilane) and hydrogen are introduced into the chemical vapor deposition equipment at a ratio of 1:10; the deposition temperature is maintained at 1150°C and the deposition pressure is 30000Pa to obtain a double-layer deposited SiC layer, in which the upper layer is the newly deposited second silicon carbide layer, and its SEM image is as shown in the figure. Figure 1 and Figure 3 As shown, columnar crystal grains with a width in the range of 1 μm to 1.5 μm and a length in the range of 30 μm to 40 μm are formed; in addition, the XRD schematic diagram of the second silicon carbide layer is shown in Figure 4 As shown, the peak of the (111) crystal plane orientation accounts for 89%, and the peak of the (222) crystal plane orientation accounts for 0.5%.
[0064] (7) Repeat the above deposition process until the thickness of the SiC ceramic reaches the required size, such as Figure 2 As shown, the first silicon carbide layer is deposited three times, and the second silicon carbide layer is deposited twice, forming a multi-layer SiC material with 4 interfaces.
[0065] (8) subjecting the SiC ceramic material of the multilayer interface to high temperature heat treatment, wherein the selected high temperature heat treatment temperature is 1800° C. and the time is 6 h, and finally a multilayer silicon carbide etched body material is obtained; wherein, Figure 2 As shown, the total thickness of the adjacent first silicon carbide layer and the second silicon carbide layer between the two layers is 95-105 μm.
[0066] Example 2
[0067] Example 2 is carried out with reference to Example 1, except that the ratio of the reaction gas, the deposition temperature and the deposition pressure in step (2) are changed, as shown below:
[0068] The reaction gas MTS (methyltrichlorosilane) and hydrogen were introduced into the chemical vapor deposition equipment at a ratio of 1:40; the deposition temperature was maintained at 1650° C. and the deposition pressure was maintained at 10000 Pa.
[0069] Example 3
[0070] Example 3 is carried out with reference to Example 1, except that the ratio of the reaction gas, the deposition temperature and the deposition pressure in step (2) are changed, as shown below:
[0071] The reaction gas MTS (methyltrichlorosilane) and hydrogen were introduced into the chemical vapor deposition equipment at a ratio of 1:20; the deposition temperature was maintained at 1450°C and the deposition pressure was maintained at 9800Pa.
[0072] Example 4
[0073] Example 4 is carried out with reference to Example 1, except that the ratio of the reaction gas, the deposition temperature and the deposition pressure in step (4) are changed, as shown below:
[0074] The reaction gas MTS (methyltrichlorosilane) and hydrogen were introduced into the chemical vapor deposition equipment at a ratio of 1:5; the deposition temperature was maintained at 1050°C and the deposition pressure was maintained at 35000Pa.
[0075] Example 5
[0076] Example 5 is carried out with reference to Example 1, except that the ratio of the reaction gas, the deposition temperature and the deposition pressure in step (4) are changed, as shown below:
[0077] The reaction gas MTS (methyltrichlorosilane) and hydrogen were introduced into the chemical vapor deposition equipment at a ratio of 1:10; the deposition temperature was maintained at 950°C and the deposition pressure was maintained at 50000Pa.
[0078] Comparative Example 1
[0079] Comparative Example 1 was carried out with reference to Example 1, except that in step (5), the SiC layer as a deposition substrate was placed in a CVD deposition furnace, and reaction gases MTS (methyltrichlorosilane) and hydrogen were introduced into the chemical vapor deposition equipment at a ratio of 1:30; the deposition temperature was maintained at 1250° C. and the deposition pressure was maintained at 9500 Pa to obtain a double-layer deposited SiC layer, in which the upper and lower layers were both the first silicon carbide layer, and the process was repeated multiple times to form a multi-layer silicon carbide etching material, the grains of which were all granular.
[0080] Comparative Example 2
[0081] Comparative Example 2 was carried out with reference to Example 1, except that in step (2), the reaction gas MTS (methyltrichlorosilane) and hydrogen were introduced into the chemical vapor deposition equipment at a ratio of 1:10; the deposition temperature was maintained at 1150° C. and the deposition pressure was 30000 Pa; step (3) was the same as in Example 1; step (4) the silicon carbide with graphite as the substrate obtained by deposition was placed in a muffle furnace and oxygen was introduced, and calcined at 500° C. for 4 h to completely remove the graphite, leaving a pure SiC layer as the substrate for the next deposition, the SiC layer being the second silicon carbide layer, and the size distribution of the grains of the formed second silicon carbide layer was in the range of 0.5 μm to 1.5 μm; step (5) was the same as in Example 1, at this time, the upper and lower layers were both the second silicon carbide layers, and the process was repeated multiple times to form a multilayer silicon carbide etching material, the grains of which were all columnar crystals.
[0082] Test Case
[0083] (1) Thermal conductivity test
[0084] The multilayer silicon carbide etched body materials prepared in the above examples and comparative examples were tested for thermal conductivity. The test method was based on the national standard GB_T 22588-2008 flash method to measure the room temperature thermal conductivity, also known as thermal conductivity coefficient, in units of W / (m·K). The test results are recorded in Table 1.
[0085] (2) Cracking resistance test
[0086] The multilayer silicon carbide etched body material prepared in the above embodiments and comparative examples is placed in the sample chamber of a plasma etching device, an etching gas is introduced, the gas is excited by a radio frequency (RF) power source, a plasma is generated, and the etching program is started. The ions and free radicals in the plasma begin to react with the SiC surface. After the etching is completed, the RF power source is turned off and the gas flow is stopped. The multilayer silicon carbide etched body material is taken out and visually inspected to see if cracks occur. If no cracks occur, the above operation is repeated and the material is placed in the etching environment for operation until obvious cracks occur on the surface of the material. The number of tests is recorded, and the test results are recorded in Table 1.
[0087] (3) Bonding strength test
[0088] The multilayer silicon carbide etched body materials prepared in the above embodiments and comparative examples were subjected to a bonding strength test. The test method referred to the national standard GB_T 31541-2015 Fine ceramic interface tensile strength test method cross-cross method to test the bonding strength between the layers of the multilayer silicon carbide etched body materials in MPa, and the test results are recorded in Table 1.
[0089] Table 1
[0090]
[0091] It can be seen from Table 1 that the multi-layer silicon carbide etching material prepared by the preparation method of the present invention avoids the influence of the multi-layer interface layer, the thermal conductivity of the material is high, and it can maintain high-speed operation in a long-term etching environment.
[0092] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a multilayer silicon carbide etched body material, characterized in that: The steps include: (1) placing the graphite substrate in a deposition furnace so that it is parallel to the air inlet of the deposition furnace, maintaining the pressure in the deposition furnace at 150 Pa to 350 Pa and the temperature at 400 to 600 ° C under a vacuum state for 15 to 30 minutes; Introduce argon gas to the deposition pressure, and raise the temperature to the deposition temperature; (2) introducing MTS and hydrogen into the deposition furnace of step (1) at a molar mass ratio of 1:(20-40), maintaining the deposition pressure and deposition temperature in step (1), and performing a deposition process to obtain a first silicon carbide layer attached to the graphite substrate; (3) subjecting the material obtained in step (2) to graphite sintering in a muffle furnace to obtain the first silicon carbide layer; (4) placing the first silicon carbide layer obtained in step (3) into the deposition furnace again as a substrate, introducing MTS and hydrogen at a molar mass ratio of 1:(1-19), maintaining the deposition pressure and deposition temperature in step (1), and performing deposition treatment again to obtain a second silicon carbide layer attached to the first silicon carbide layer; (5) Repeating steps (2) and (4) 2-3 times to obtain a multilayer silicon carbide layer in which the first silicon carbide layer and the second silicon carbide layer are stacked in sequence, and subjecting the multilayer silicon carbide layer to high-temperature heat treatment to obtain a multilayer silicon carbide etched body material; The peak value of the (111) crystal plane orientation of the second silicon carbide layer accounts for 85% to 89%, and the peak value of the (222) crystal plane orientation accounts for 0.5% to 1.5%; The grains included in the second silicon carbide layer are columnar crystals, and the width of the columnar crystals is 0.5 μm to 1.5 μm; The grains contained in the first silicon carbide layer are granular, and the grain size thereof is 0.5 μm to 1.5 μm; In step (1), step (2) and step (4), the conditions of the deposition treatment include: the deposition temperature is 900° C. to 1650° C., the deposition pressure is 9500 Pa to 80000 Pa, and the deposition time is 4 h to 12 h; In step (5), argon gas is introduced during the high temperature heat treatment, the temperature of the high temperature heat treatment is 1700-1900°C, and the duration is 4-6 hours.
2. The method for preparing a multilayer silicon carbide etchant material according to claim 1, characterized in that: The length of the columnar crystals is 30 μm to 120 μm.
3. The method for preparing a multilayer silicon carbide etchant material according to claim 1, characterized in that: The interface between adjacent first silicon carbide layers is in the form of columnar crystals connected by the second silicon carbide layer.
4. The method for preparing a multilayer silicon carbide etchant material according to claim 1, characterized in that: The total thickness of the adjacent first silicon carbide layers and the second silicon carbide layer between two adjacent first silicon carbide layers is 90 μm to 180 μm.
5. The method for preparing a multilayer silicon carbide etchant material according to claim 1, characterized in that: The thickness ratio of the first silicon carbide layer to the second silicon carbide layer is (1.1~1.3):
1.
6. The method for preparing a multilayer silicon carbide etchant material according to claim 1, characterized in that: In step (3), oxygen is introduced during the graphite sintering process. The graphite sintering process is carried out at a temperature of 500-800° C. and lasts for 10-20 hours.
7. Application of the multi-layer silicon carbide etchant material prepared by the method for preparing the multi-layer silicon carbide etchant material according to any one of claims 1 to 6 in plasma etching technology.