Method for directionally and chemically depolymerizing bisphenol A polycarbonate plastic
Through the joint action of acidic catalyst p-toluenesulfonic acid or benzenesulfonic acid and acetic acid aqueous solution, efficient degradation of polycarbonate is achieved, which solves the problem of difficult separation and environmental pollution of alkaline catalysts, ensuring the reuse of the catalyst and efficient degradation effect.
Patent Information
- Application Number
- CN202410882511.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing chemical recycling method of polycarbonate plastic, the alkaline catalyst participates in the reaction and is difficult to separate, and generates salty wastewater that pollutes the environment, making it difficult to recover the catalyst.
An acidic catalyst is used to carry out depolymerization of toluenesulfonic acid or benzenesulfonic acid and acetic acid aqueous solution, and the ester bond is broken through the action of protonic acid to avoid the combination of metal ions under alkaline conditions, so that the product can be easily separated and the catalytic system can be reused.
It achieves efficient degradation of polycarbonate under acidic conditions and avoids the pollution problem of alkaline catalysts. After 10 cycles of the catalyst, the depolymerization rate and yield are stable, and the product recovery rate is more than 95%, which has good application value.
Smart Images

Figure CN118851884A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastic degradation and recycling, in particular to a method for directional chemical depolymerization of bisphenol A type polycarbonate plastic. Background Art
[0002] Polycarbonate plastic (PC) is one of the five major engineering plastics, with an annual output of more than 1.13 million tons, which also means that a huge amount of waste PC plastic is produced. The large amount of organic carbon in its structure is a recyclable carbon resource. If it can be recycled, it can not only reduce the threat to the environment, but also reduce CO2 emissions.
[0003] The degradation and recycling of waste polycarbonate can be divided into physical recycling and chemical recycling. Although the physical method is simple to recycle, it is generally downgraded recycling with low added value of the product. It is often used as the primary processing stage of plastic recycling and is used together with other recycling methods. Chemical recycling is to decompose the waste polycarbonate material into small molecules or single chemical products through pyrolysis or other chemical methods (such as hydrolysis, alcoholysis and hydrogenolysis). The chemical method is favored by researchers because it can degrade waste plastics into high-value chemicals.
[0004] Chemical methods can effectively decompose and recycle PC materials, but no matter which chemical method is used, the synergistic effect of catalysts and solvents is required to achieve efficient PC decomposition. In previous studies, most of the hydroxides such as NaOH and KOH, metal salts, etc. were used to degrade PC. These catalytic systems have mild conditions and good depolymerization rates. However, when hydroxides and metal salts are used as catalysts, metal ions will combine with or be consumed by the reaction components during the reaction, making it difficult to recover the catalyst, and a large amount of salt-containing wastewater will be generated, polluting the environment. Summary of the invention
[0005] The object of the present invention is to provide a method for directional chemical depolymerization of bisphenol A type polycarbonate plastics. The present invention avoids the problem that alkaline catalysts participate in the reaction, are difficult to separate from products, and produce salt-containing wastewater to pollute the environment; the catalytic system used in the present invention is easy to separate the reaction products, and the catalytic system can be reused after separation.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The invention provides a method for directional chemical depolymerization of bisphenol A type polycarbonate plastic, comprising the following steps: mixing bisphenol A type polycarbonate plastic, an acid catalyst, acetic acid and water, and performing a depolymerization reaction to obtain a depolymerization liquid containing bisphenol A, indane bisphenol, spirobiindane and phenol; the temperature of the depolymerization reaction is 130-170°C;
[0008] The acidic catalyst includes p-toluenesulfonic acid and / or benzenesulfonic acid.
[0009] Preferably, the mass of the acidic catalyst does not exceed 45% of the mass of the bisphenol A polycarbonate plastic.
[0010] Preferably, the ratio of the mass of the bisphenol A polycarbonate plastic to the total mass of acetic acid and water is 1:10.
[0011] Preferably, the mass of the acetic acid is 0.1 to 99% of the total mass of acetic acid and water.
[0012] Preferably, the depolymerization reaction time is 2 to 18 hours.
[0013] Preferably, after obtaining the depolymerization liquid, the method further comprises: subjecting the depolymerization liquid to a first solid-liquid separation to obtain a depolymerization liquid; adding water to the depolymerization liquid until solids precipitate, and subjecting the depolymerization liquid to a second solid-liquid separation to obtain a solid product and an aqueous phase, respectively; the solid product comprises bisphenol A, indane bisphenol and spirobisindane; the aqueous phase comprises phenol, acetic acid, water and an acidic catalyst; and subjecting the aqueous phase to rotary evaporation to remove acetic acid, water and phenol to obtain an acidic catalyst.
[0014] Preferably, the temperature of the rotary evaporation is 50-70°C.
[0015] Preferably, the depolymerization reaction is carried out in a reactor lined with polytetrafluoroethylene.
[0016] Preferably, before the mixing, the bisphenol A polycarbonate plastic is crushed.
[0017] Preferably, the mass content of bisphenol A, indane bisphenol and spirobisindan in the solid product is greater than 50%.
[0018] The invention provides a method for directional chemical depolymerization of bisphenol A type polycarbonate plastic, comprising the following steps: mixing bisphenol A type polycarbonate plastic, an acid catalyst, acetic acid and water, carrying out a depolymerization reaction, and obtaining a depolymerization liquid containing bisphenol A, indane bisphenol, spirobiindane and phenol; the temperature of the depolymerization reaction is 130-170 DEG C; and the acid catalyst comprises p-toluenesulfonic acid and / or benzenesulfonic acid.
[0019] The present invention adopts amphiphilic substances p-toluenesulfonic acid or benzenesulfonic acid as a catalyst, and acetic acid aqueous solution as a reaction solvent. Under the joint action of acetic acid, water and p-toluenesulfonic acid (or benzenesulfonic acid), polycarbonate can be effectively broken and degraded. Under the swelling action of acetic acid, p-toluenesulfonic acid (or benzenesulfonic acid) provides proton hydrogen as a protonic acid, selectively attacks the ester bond in the polycarbonate, and causes the CO bond in the ester bond to break. The O end after the break combines with H in water to generate bisphenol A (BPA for short), and the carbonyl formed after the break combines with OH in water to generate H2CO3. Under acidic conditions, H2CO3 decomposes into CO2 and H2O. Under the strong acid conditions of p-toluenesulfonic acid (or benzenesulfonic acid) and acetic acid, the CC bond on the benzene ring of bisphenol A breaks to generate phenol and part of carbon ions. Under the action of p-toluenesulfonic acid (or benzenesulfonic acid), these carbon ions attack and rearrange the generated BPA, and combine to generate indane bisphenol (BPI for short) and spirobisindane (TSD for short).
[0020] The present invention degrades PC under acidic conditions, and while the degradation rate is guaranteed, the problem of alkaline catalyst participating in the reaction, being difficult to separate from the product and polluting the environment is avoided; and the acidic catalyst of the present invention does not participate in the degradation reaction, is easy to separate from the reaction product, and the catalytic system can be reused after separation.
[0021] The results of the embodiment show that after the acid catalyst is cycled 10 times, the PC depolymerization rate and product yield do not decrease significantly, and the system has good stability. The catalytic system can effectively degrade polycarbonate products by expanding the real system (such as CDs, drinking water bucket fragments, etc.), and the total product yield after 8 hours of reaction is more than 95% (see Table 3 and Table 4), which has good application value and prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a technical roadmap for the polycarbonate degradation reaction catalyzed by the p-toluenesulfonic acid / acetic acid system of the present invention;
[0023] Figure 2 The GC-MC spectrum (a) of the solid product of Example 1 and the HPLC spectrum (b) of the aqueous solution, wherein 1-bisphenol A, 2-indanebisphenol, 3-spirobisindane, 4-acetic acid, 5-p-toluenesulfonic acid, 6-phenol;
[0024] Figure 3 It is the recycling performance of the catalyst when the depolymerization rate is 100%. DETAILED DESCRIPTION
[0025] The invention provides a method for directional chemical depolymerization of bisphenol A type polycarbonate plastic, comprising the following steps: mixing bisphenol A type polycarbonate plastic, an acid catalyst, acetic acid and water, carrying out a depolymerization reaction, and obtaining a depolymerization liquid containing bisphenol A, indane bisphenol, spirobiindane and phenol; the temperature of the depolymerization reaction is 130-170°C.
[0026] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0027] In the present invention, the bisphenol A type polycarbonate plastic is preferably discarded bisphenol A type polycarbonate plastic, and the specific source thereof may be discarded compact discs and drinking water buckets, and the present invention does not make any special requirements therefor.
[0028] In the present invention, when the bisphenol A polycarbonate plastic is waste bisphenol A polycarbonate plastic, before the mixing, the present invention preferably further comprises pre-treating the waste bisphenol A polycarbonate plastic. The present invention has no special requirements for the pre-treatment operation, and a pre-treatment method well known in the art can be selected according to the source of the plastic.
[0029] In an embodiment of the present invention, when the bisphenol A type polycarbonate plastic is a discarded optical disc, the pretreatment is: cutting the waste optical disc into 1×1 cm fragments, washing the fragments with distilled water, and then chemically eluting the waste optical disc fragments with a NaClO / NaOH mixed solution to remove the printed layer on the surface of the optical disc, and then washing with distilled water and drying at 80°C for 12 hours.
[0030] When the bisphenol A type polycarbonate plastic is a waste drinking water bucket, the pretreatment is: cutting the waste drinking water bucket into pieces of 1×1 cm, washing the pieces with distilled water, and drying at 80° C. for 12 hours.
[0031] In the present invention, the acidic catalyst includes p-toluenesulfonic acid and / or benzenesulfonic acid. In the present invention, p-toluenesulfonic acid (P-TSA) and benzenesulfonic acid are amphiphilic, have good solubility in an acetic acid-water system, and are easy to interact with PC polymers, can promote the material transfer between the solvent and the resin, and accelerate the degradation rate of PC.
[0032] In the present invention, the mass of the acidic catalyst does not exceed 45% of the mass of the bisphenol A polycarbonate plastic, preferably 5-45%, more preferably 10-40%, and further preferably 20-30%; the ratio of the mass of the bisphenol A polycarbonate plastic to the total mass of acetic acid and water is preferably 1:10; the mass of the acetic acid is preferably 0.1-99% of the total mass of acetic acid and water, specifically 5%, 10%, 15%, 20%, 25%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 95%, which are not listed here. In an embodiment of the present invention, acetic acid and water are used in the form of 94wt% acetic acid aqueous solution. The present invention uses acetic acid and water as solvents, which can effectively swell bisphenol A polycarbonate plastic and promote mass transfer.
[0033] The present invention has no special requirements for the mixing process, and any mixing method known in the art can be used.
[0034] In the present invention, the temperature of the depolymerization reaction is 130-170°C, preferably 135-165°C, more preferably 140-160°C, and further preferably 145-155°C; the time of the depolymerization reaction is preferably 2-18h, more preferably 5-15h, and further preferably 6-12h. In the present invention, the depolymerization reaction is preferably carried out in a reactor lined with polytetrafluoroethylene.
[0035] The present invention adopts amphiphilic substances p-toluenesulfonic acid or benzenesulfonic acid as a catalyst, and acetic acid aqueous solution as a reaction solvent. Under the joint action of acetic acid, water and p-toluenesulfonic acid (or benzenesulfonic acid), polycarbonate can be effectively broken and degraded. Under the swelling action of acetic acid, p-toluenesulfonic acid (or benzenesulfonic acid) provides proton hydrogen as a protonic acid, selectively attacks the ester bond in the polycarbonate, and causes the CO bond in the ester bond to break. The O end after the break combines with H in water to generate bisphenol A (BPA for short), and the carbonyl formed after the break combines with OH in water to generate H2CO3. Under acidic conditions, H2CO3 decomposes into CO2 and H2O. Under the strong acid conditions of p-toluenesulfonic acid (or benzenesulfonic acid) and acetic acid, the CC bond on the benzene ring of bisphenol A breaks to generate phenol and part of carbon ions. Under the action of p-toluenesulfonic acid (or benzenesulfonic acid), these carbon ions attack and rearrange the generated BPA, and combine to generate indane bisphenol (BPI for short) and spirobisindane (TSD for short).
[0036] Therefore, after the depolymerization reaction, the present invention obtains a depolymerization liquid containing bisphenol A, indane bisphenol, spirobisindane and phenol.
[0037] In the present invention, the depolymerization liquid is preferably placed in an ice bath for cooling and then post-treated.
[0038] In the present invention, the post-treatment preferably includes: performing a first solid-liquid separation on the depolymerization liquid to obtain a depolymerization liquid; adding water to the depolymerization liquid until solids are precipitated, and performing a second solid-liquid separation to obtain a solid product and an aqueous phase, respectively; the solid product includes bisphenol A, indane bisphenol and spirobisindane; the aqueous phase includes phenol, acetic acid, water and an acidic catalyst; and rotary evaporating the aqueous phase to remove acetic acid, water and phenol to obtain an acidic catalyst.
[0039] The present invention does not make any special requirements on the first solid-liquid separation and the second solid-liquid separation methods, and any solid-liquid separation method known in the art, such as centrifugation, can be used.
[0040] The present invention obtains the remaining solid (that is, the depolymerized substrate, recorded as solid 1) and the depolymerization liquid through the first solid-liquid separation. The solid 1 is washed, dried, and weighed for calculating the depolymerization rate of polycarbonate.
[0041] The present invention has no special requirements for the amount of water added to the depolymerization liquid, and the solid can be added until no solid is precipitated. BPA, BPI and TSD are insoluble in water. The present invention promotes the precipitation of the three by adding water, and the obtained solid products are mainly bisphenol A, indane bisphenol and spirobiindane, while the phenol produced by the depolymerization reaction remains in the water phase.
[0042] In the present invention, the temperature of the rotary evaporation is preferably 50-70°C, more preferably 65°C.
[0043] The invention removes acetic acid, water and phenol by rotary evaporation to achieve the recovery of the acidic catalyst.
[0044] When phenol needs to be recovered, the present invention preferably extracts the rotary evaporation liquid obtained by rotary evaporation with a dichloromethane solution.
[0045] The method for directional chemical depolymerization of bisphenol A type polycarbonate plastic provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0046] Example 1
[0047] like Figure 1As shown, 0.4g polycarbonate (Shanghai McLean Biochemical Technology Co., Ltd., Mn = 26000), 0.1g p-toluenesulfonic acid, 4.0g acetic acid aqueous solution (94wt%) were placed in a reactor lined with polytetrafluoroethylene, reacted at 170°C for 8h, cooled in an ice bath, centrifuged, and the undepolymerized substrate (solid 1) was washed three times with water and ethanol respectively, dried at 100°C for 10h, weighed, and used for the calculation of the depolymerization rate of polycarbonate. 25mL of water was added to the depolymerization liquid (liquid phase 1), and a solid product precipitated from the water. The solid was separated by centrifugation at a speed of 9800r / min for 10min to obtain a solid product (solid 2) and an aqueous phase (liquid phase 2).
[0048] The solid product (solid 2) was dissolved in methanol and subjected to GC-MS detection. The results were as follows: Figure 2 As shown in a, the mass spectrum of the polycarbonate depolymerization product was analyzed and compared with the mass spectrum of standard chemicals, and it was determined that the solid products were mainly BPA, BPI and TSD. The aqueous solution (liquid phase 2) was extracted with an equal amount of dichloromethane solution, and water-soluble organic matter was obtained after separation. The dichloromethane extraction solution was detected by GC-MS, and the main water-soluble product was determined to be phenol. At the same time, NaOH was used to adjust the pH of liquid phase 2 to 5-8, and then the aqueous solution (liquid phase 2) was analyzed by HPLC. The peak time of substances such as P-TSA and acetic acid was determined by comparison with the standard, as shown in FIG. Figure 2 After analysis, the content of each depolymerization product component is obtained, as shown in Table 1.
[0049] Since the depolymerization product contains bisphenol A (BPA), indane bisphenol (BPI), spirobiindane (TSD), phenol (Ph) and other substances, the product solution may contain the catalyst p-toluenesulfonic acid (P-TSA). In order to quantify the above substances, standard solutions of different concentrations were prepared respectively, and standard curves of different substances were established. The PC depolymerization rate was calculated according to Formula 1, and the product yield was calculated according to Formula 2:
[0050]
[0051]
[0052] In formula 1, m0 is the initial amount of PC added (g); m1 is the remaining amount of PC after the reaction (g);
[0053] In formula 2, Cmol i —The total amount of C in each product (mol); Cmol0—The total amount of aromatic C in the substrate (mol).
[0054] Table 1 Composition analysis of polycarbonate depolymerization products
[0055] Peak number Peak time / min substance Yield / % 1 37.0 Bisphenol A 7.5 2 39.9 Indan bisphenol 21.7 3 43.1 Spirobiindane 16.4 6 27.4 phenol 28.5
[0056] After adding distilled water to the depolymerization liquid (liquid phase 1), a solid-liquid mixed solution is obtained, and the solid is separated by centrifugation to obtain a clear solution (liquid phase 2). Liquid phase 2 is heated at 65°C by a rotary evaporator to evaporate and remove the acetic acid aqueous solution. Most of the phenol in the water is also evaporated away by rotary evaporation to obtain the catalyst in the reaction system. After adding the same acetic acid aqueous solution as in the previous reaction, 0.4g PC and 4.0g acetic acid aqueous solution (94wt%) are added to the catalyst, and a new cycle reaction is carried out under the same reaction conditions.
[0057] like Figure 3 As shown in Table 2, the catalyst of the above technical route can be used continuously for 10 times, the depolymerization rate does not decrease significantly, and the yield of each product changes, indicating that the above technical route can achieve the degradation of bisphenol A type polycarbonate into products such as phenol, indane bisphenol, and spirobiindane.
[0058] Table 2 Product distribution after 10 catalyst cycles
[0059]
[0060]
[0061] Embodiment 2-3
[0062] Degradation of CD fragments catalyzed by p-toluenesulfonic acid / acetic acid system:
[0063] Optical discs are the most common polycarbonate products in daily life. In order to verify the applicability of the catalytic system to the real system of polycarbonate, the technical solution of the present invention is applied to the degradation of waste optical disc fragments. Pretreatment conditions before depolymerization: First, the waste optical discs are cut into 1×1 cm fragments and the fragments are washed with distilled water. Then, the waste optical disc fragments are chemically eluted with a NaClO / NaOH mixed solution to remove the printed layer on the surface of the optical disc, and then washed with distilled water and dried at 80°C for 12 hours.
[0064] Depolymerization reaction conditions: PC is 0.4 g, acetic acid aqueous solution concentration is 94 wt%, 4.0 g, p-toluenesulfonic acid is 0.1 g, depolymerization temperature is 170° C., and depolymerization time is 8 h or 6 h.
[0065] After the depolymerization reaction is completed, the catalyst is separated therefrom, the depolymerization product is analyzed, and the depolymerization rate and yield are calculated.
[0066] The results show that the p-toluenesulfonic acid / acetic acid system can achieve 100% degradation of CD fragments at 170°C. The product distribution and yield are shown in Table 3.
[0067] Table 3 Effect of p-toluenesulfonic acid / acetic acid system on the degradation of CD fragments
[0068] Reaction time (h) phenol Bisphenol A Indan bisphenol Spirobiindane Depolymerization rate 6 25% 4.6% 8.9% 19.4% 100% 8 32% 9.4% 17.8% 40% 100%
[0069] Embodiment 4-5
[0070] The technical solution of the present invention is applied to catalyze the degradation of drinking water bucket fragments.
[0071] The waste drinking water barrels were cut into 1×1 cm fragments, washed with distilled water, dried at 80°C for 12 h, and then depolymerized using a p-toluenesulfonic acid / acetic acid system.
[0072] Depolymerization reaction conditions: PC is 0.4 g, acetic acid aqueous solution concentration is 94 wt%, 4.0 g, p-toluenesulfonic acid is 0.1 g, depolymerization temperature is 170° C., and depolymerization time is 8 h or 6 h.
[0073] After the depolymerization reaction is completed, the catalyst is separated therefrom, the depolymerization product is analyzed, and the depolymerization rate and yield are calculated.
[0074] The results show that the p-toluenesulfonic acid / acetic acid system can achieve 100% degradation of CD fragments at 170°C. The product distribution and yield are shown in Table 4.
[0075] Table 4 Degradation effect of drinking water bucket fragments catalyzed by p-toluenesulfonic acid / acetic acid system
[0076]
[0077]
[0078] Example 6
[0079] The difference from Example 1 is that the catalyst is replaced by benzenesulfonic acid. The depolymerization results are shown in Table 5.
[0080] Table 5 Product distribution of PC depolymerization catalyzed by benzenesulfonic acid
[0081]
[0082] Example 7
[0083] The only difference from Example 1 is the molecular weight of the polycarbonate, Mn = 45000. The depolymerization results are shown in Table 6.
[0084] Table 6 Degradation of polycarbonate with a molecular weight of 45000 by acetic acid / p-toluenesulfonic acid
[0085] Reaction time (h) phenol Bisphenol A Indan bisphenol Spirobiindane Depolymerization rate 6 29.6% 9.6% 8.9% 11.4% 100% 8 31.85% 2.4% 9.3% 25.2% 100%
[0086] It can be seen from the above examples that the present invention provides a method for directional chemical depolymerization of bisphenol A type polycarbonate plastics. The catalyst system used in the present invention is easy to separate the reaction products, and the catalyst system can be reused after separation.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for directional chemical depolymerization of bisphenol A type polycarbonate plastic, characterized in that: The following steps are involved: Mixing bisphenol A type polycarbonate plastic, an acid catalyst, acetic acid and water to carry out a depolymerization reaction to obtain a depolymerization liquid containing bisphenol A, indane bisphenol, spirobiindane and phenol; the temperature of the depolymerization reaction is 130-170°C; The acidic catalyst includes p-toluenesulfonic acid and / or benzenesulfonic acid.
2. The method according to claim 1, characterized in that The mass of the acid catalyst does not exceed 45% of the mass of the bisphenol A polycarbonate plastic.
3. The method according to claim 1, characterized in that The ratio of the mass of the bisphenol A type polycarbonate plastic to the total mass of acetic acid and water is 1:
10.
4. The method according to claim 1, characterized in that: The mass of the acetic acid is 0.1 to 99% of the total mass of the acetic acid and water.
5. The method according to any one of claims 1 to 4, characterized in that: The depolymerization reaction time is 2 to 18 hours.
6. The method according to claim 1, characterized in that After obtaining the depolymerization liquid, the method further includes: performing a first solid-liquid separation on the depolymerization liquid to obtain a depolymerization liquid; adding water to the depolymerization liquid until solids are precipitated, and performing a second solid-liquid separation to obtain a solid product and an aqueous phase respectively; the solid product includes bisphenol A, indane bisphenol and spirobisindane; the aqueous phase includes phenol, acetic acid, water and an acidic catalyst; and rotary evaporating the aqueous phase to remove acetic acid, water and phenol to obtain an acidic catalyst.
7. The method according to claim 6, characterized in that The temperature of the rotary evaporation is 50-70°C.
8. The method according to claim 1, characterized in that The depolymerization reaction is carried out in a reactor lined with polytetrafluoroethylene.
9. The method according to claim 1, characterized in that: Before the mixing, the bisphenol A polycarbonate plastic is crushed.
10. The method according to claim 6, characterized in that The mass content of bisphenol A, indane bisphenol and spirobiindan in the solid product is greater than 50%.
Citation Information
Cited By
Method for appreciation conversion of polycarbonate into phenol