High-stability full-spectrum perovskite nanocrystal and preparation method and device thereof

By modifying lead halide on the surface of nano-titanium dioxide and reacting with cesium precursor to generate perovskite nanocrystals, the preparation and stability problems of perovskite nanocrystals are solved, high stability and full spectrum control are achieved, and its performance in Application potential in the field of optoelectronic materials.

CN118853162AActive Publication Date: 2024-10-29SHANGHAI INST OF TECH

Patent Information

Application Number
CN202410864033.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-30
Publication Date
2024-10-29
Estimated Expiration
2044-06-30

AI Technical Summary

Technical Problem

Existing technology is difficult to achieve large-scale preparation of perovskite nanocrystals and has environmental stability issues. Traditional methods are difficult to control reaction parameters, resulting in uneven distribution and poor stability of perovskite nanocrystals. Existing composite methods reduce luminescence intensity.

Method used

By modifying the surface of titanium dioxide nanoparticles with lead halide and reacting with the cesium precursor, the perovskite nanocrystals generated by the reaction are combined with the titanium dioxide nanoparticles in situ, and the microfluidic chip is used to achieve the continuous and controllable preparation of highly stable full-spectrum perovskite nanocrystals. Enhance its luminous intensity and stability.

Benefits of technology

It achieves high stability, repeatability and uniformity of perovskite nanocrystals, enhances luminous intensity and hot water stability, and can achieve full spectrum control, promoting its application in the field of optoelectronic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118853162A_ABST
    Figure CN118853162A_ABST
Patent Text Reader

Abstract

The invention relates to a high-stability full-spectrum perovskite nanocrystal and a preparation method and device thereof. The surface of nano titanium dioxide is modified by lead halide, the perovskite nanocrystal generated by reacting the lead halide with a cesium precursor is combined with the nano titanium dioxide in situ in the synthesis process, and the perovskite nanocrystal is coated with the nano titanium dioxide; the lead halide is selected from one or more of lead chloride, lead bromide and lead iodide, the molar ratio of the lead halide to the nano titanium dioxide is 1: (1-4), and the molar ratio of cesium to lead in the cesium precursor and the lead halide is 1: (2-7). Compared with the prior art, the luminescent intensity, the water stability and the thermal stability of the perovskite nanocrystal are enhanced, and full-spectrum regulation and continuous controllable preparation can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fluorescent material preparation, and relates to a high-stability full-spectrum perovskite nanocrystal and a preparation method and device thereof. Background Art

[0002] All-inorganic lead halide perovskite nanocrystals (CsPbX3 NCs, X=Cl, Br, I) are widely used in display, solar cell, light-emitting diode (LED) and other fields due to their unique luminescence properties such as narrow half-width, high photoluminescence quantum yield, adjustable band gap, and high carrier mobility. However, the large-scale preparation and environmental stability of perovskite nanocrystals have greatly hindered their practical application in the optoelectronic field. The traditional preparation method of perovskite nanocrystals is an intermittent method based on manual flasks and beakers. This method is not only difficult to achieve rapid regulation of parameters such as reaction temperature and reaction time, but also has uncontrollable and unreproducible heat and mass transfer rates, and has limitations in reproducibility, homogeneous mixing, large-scale and high-throughput preparation, which may lead to uneven distribution and poor reproducibility of the synthesized perovskite nanocrystal particles.

[0003] The environmental stability of all-inorganic lead halide perovskite nanocrystals is extremely poor, especially purple CsPbCl3 nanocrystals and red CsPbI3 nanocrystals are very sensitive to environmental factors such as moisture, oxygen, radiation and high temperature, and are prone to phase change, degradation and agglomeration, resulting in fluorescence quenching. In order to improve the environmental stability of perovskite nanocrystals, compounding with inorganic materials is one of the common methods. Common inorganic materials in existing research include aluminum oxide (Al2O3), silicon dioxide (SiO2) and calcium fluoride (CaF2), etc. They all have high transparency, strong thermal stability and chemical stability. After coating perovskite nanocrystals, they can isolate the influence of environmental factors to a certain extent, but will reduce the luminescence intensity of perovskite nanocrystals. Therefore, it is necessary to find a method that can both continuously and controllably prepare perovskite nanocrystals and enhance their stability.

[0004] Patent CN116590011A discloses a method for preparing perovskite quantum dots based on microfluidics. The microfluidic reactor used includes: a syringe pump, a syringe, a polytetrafluoroethylene tube with an inner diameter of 0.5 mm, a four-way connector used in conjunction with it, and a heated aluminum plate; the square dotted line is the polytetrafluoroethylene tube, A, B and C are the polytetrafluoroethylene tubes connected to the fluid phase A, the fluid phase B and the fluid phase C respectively, and the heated aluminum plate is separated by the dotted line, wherein the left side of the dotted line is the precursor preheating zone, and the right side of the dotted line is the quantum dot preparation zone; the heated aluminum plate has a groove for placing the polytetrafluoroethylene tube, the length of the polytetrafluoroethylene tube placed in the quantum dot preparation zone can be adjusted, and the preparation time is controlled by adjusting the length of the polytetrafluoroethylene tube placed in the quantum dot preparation zone.

[0005] However, the patent combines an injection pump, a polytetrafluoroethylene tube, a four-way joint, and a heated aluminum plate to construct a fluid reaction device, which makes the equipment assembly complicated, and it is difficult to closely fit and fix the polytetrafluoroethylene tube and the heated aluminum plate, and the reaction zone is not completely enclosed in a high-temperature environment;

[0006] The inner diameter of the PTFE tube is 0.5 mm, that is, the cross-sectional area of ​​the reaction tube is 0.19625 mm 2 , the cross-sectional area of ​​the flow channel is large, and the mixing rate of the reaction substances is slow, which is not conducive to the reaction;

[0007] The reaction device is a three-phase flow, where flow phase A is a cesium precursor, flow phase B is a lead halide precursor, and flow direction C is fluorine oil. Fluorine oil is used as a carrier to divide the reaction phase into multiple small droplets. It is a discontinuous flow, and the reaction zone is interrupted;

[0008] The result of preparation using this device is perovskite quantum dots, rather than perovskite nanocrystals.

[0009] Patent CN110607172A discloses a method for preparing perovskite / titanium dioxide composite nanocrystals, comprising: mixing cesium carbonate, octadecene solution and oleic acid to obtain a cesium oleate precursor solution after reaction; mixing lead halide, octadecene solution, oleic acid and oleylamine, and reacting the obtained mixed solution with the cesium oleate precursor solution to obtain a perovskite quantum dot solution; purifying the perovskite quantum dot solution with toluene to obtain a perovskite toluene solution; mixing the perovskite toluene solution with titanium dioxide nanotubes to obtain perovskite / titanium dioxide composite nanocrystals. However, the titanium dioxide morphology used in this patent is titanium dioxide nanotubes. The composite method of perovskite quantum dots and titanium dioxide nanotubes is to first synthesize the perovskite quantum dots and purify them with toluene, and then directly mix the reacted perovskite quantum dots with titanium dioxide nanotubes. The combination method is that the perovskite quantum dots are inside the titanium dioxide nanotubes. After the perovskite quantum dots and titanium dioxide nanotubes are composited, since the perovskite quantum dots are synthesized first, their luminescence performance will not be enhanced due to direct mixing with titanium dioxide nanotubes. The stability changes before and after the combination of the perovskite quantum dots and titanium dioxide nanotubes have not been studied. Summary of the invention

[0010] The purpose of the present invention is to overcome at least one defect of the above-mentioned prior art and to provide a highly stable full-spectrum perovskite nanocrystal and a method and device for preparing the same. The present invention enhances the luminescence intensity, water stability and thermal stability of the perovskite nanocrystal, and can achieve full-spectrum regulation and continuous and controllable preparation.

[0011] The purpose of the present invention can be achieved by the following technical solutions:

[0012] One of the technical solutions of the present invention is to provide a highly stable full-spectrum perovskite nanocrystal, wherein the surface of nano-titanium dioxide (TiO2) is fully modified by lead halide (PbX2), and the perovskite (CsPbX3) nanocrystal generated by the reaction of the lead halide with a cesium precursor is in situ combined with the nano-titanium dioxide during the synthesis process, and the nano-titanium dioxide coats the perovskite nanocrystal to modify the surface defects of the perovskite nanocrystal;

[0013] The lead halide is selected from one or more of lead chloride (PbCl2), lead bromide (PbBr2), and lead iodide (PbI2). The molar ratio of the lead halide to nano-titanium dioxide is 1:(1-4), and the molar ratio of cesium to lead in the cesium precursor and the lead halide is 1:(2-7).

[0014] As a preferred technical solution, the molar ratio between the two halogens is (0-3):(0-3), but not 0 at the same time.

[0015] Furthermore, the cesium source of the cesium precursor includes cesium carbonate (Cs2CO3) or cesium acetate (CsOAc).

[0016] One of the technical solutions of the present invention is to provide a method for preparing the highly stable full-spectrum perovskite nanocrystals, the method comprising the following steps:

[0017] S1. Preparing a precursor solution: mixing a cesium source, oleic acid (OA) and octadecene (ODE) under an inert gas atmosphere, and then heating and mixing. The cesium source and oleic acid react completely to obtain a cesium oleate (Cs-Oleate) solution. Octadecene is added to the cesium oleate solution to dilute it, and the mixture is mixed under an inert gas atmosphere until the solution becomes clear to obtain a first precursor solution.

[0018] S2, mixing lead halide, nano-titanium dioxide, oleic acid, oleylamine (OAm) and octadecene under an inert gas atmosphere, the surface of the nano-titanium dioxide is fully modified by the lead halide to form lead halide / nano-titanium dioxide (PbX2 / TiO2), and the lead halide / nano-titanium dioxide reacts completely with oleic acid and oleylamine to obtain a lead halide / nano-titanium dioxide solution as a second precursor solution;

[0019] S3. Transfer the first precursor solution and the second precursor solution to the first syringe and the second syringe respectively; place the microfluidic chip on a heating platform, and use a syringe pump to drive the precursor solutions in the first syringe and the second syringe to flow evenly and mix and react in the microfluidic channel to obtain highly stable full-spectrum perovskite (CsPbX3 / TiO2) nanocrystals.

[0020] As a preferred technical solution, the inert gas in steps S1 and S2 includes nitrogen or argon.

[0021] Furthermore, in step S1, the molar / volume ratio of cesium, oleic acid and octadecene in the cesium source is 1 mol:(0.4-0.6L):(6-9L).

[0022] Furthermore, in step S2, the molar / volume ratio of lead halide, nano-titanium dioxide, oleic acid, oleylamine and octadecene is 1 mol:(1-4 mol):(1-3 L):(1-3 L):(20-40 L).

[0023] Further, the mixing temperature in step S1 is 110-130°C and the mixing time is 1-1.5h;

[0024] The heating mixing temperature is 140-160°C and the time is 0.5-1h;

[0025] The dilution multiple is 15-25 times, the mixing temperature during dilution is 110-130°C, and the time is 10-15 minutes.

[0026] Furthermore, the mixing temperature in step S2 is 110-130° C. and the mixing time is 0.5-1 h.

[0027] Furthermore, the reaction time in step S3 is determined by the flow rate of the mixed precursors in the reaction zone and the width, depth and length of the microfluidic channel section in the reaction zone. The reaction time is 3-8s, the reaction temperature is 140-180°C, and the flow rate is 300-800μL / min.

[0028] As a preferred technical solution, after step S3, the product solution is centrifuged and the supernatant is discarded to obtain a highly stable full-spectrum perovskite nanocrystal precipitate. After centrifugal washing with a solvent, the highly stable full-spectrum perovskite nanocrystal precipitate is dispersed in a solvent for storage.

[0029] As a preferred technical solution, the centrifugal speed is 8000-12000r / min and the time is 5-10min.

[0030] As a preferred technical solution, the solvent includes n-hexane, cyclohexane or toluene.

[0031] One of the technical solutions of the present invention is to provide a preparation device for highly stable full-spectrum perovskite nanocrystals, through which the perovskite nanocrystals are continuously and controllably prepared using the method described, the device comprising a syringe pump, a first syringe, a second syringe, a microfluidic chip, a heating platform and a collecting device, the microfluidic chip comprising an upper plate, a gasket, a lower plate, a first microfluidic channel, a second microfluidic channel and a third microfluidic channel;

[0032] The lower plate is provided with a first microfluidic channel, a second microfluidic channel and a third microfluidic channel, the first microfluidic channel, the second microfluidic channel and the third microfluidic channel are connected in a T-shaped channel, the first syringe is connected to the first microfluidic channel, the second syringe is connected to the second microfluidic channel, and the third microfluidic channel is connected to the collecting device;

[0033] The first syringe and the second syringe are connected to an injection pump, which is used to push the first syringe and the second syringe. An upper plate is arranged on the lower plate, and the upper plate is sealed with the lower plate through a gasket. A heating platform is arranged under the lower plate, and the heating platform is used to heat the lower plate.

[0034] As a preferred technical solution, the first syringe is connected to the first microfluidic channel through a transparent polytetrafluoroethylene (PTFE) tube and a high-temperature resistant polypropylene (PP) inverted cone joint, the second syringe is connected to the second microfluidic channel through a transparent polytetrafluoroethylene tube and a high-temperature resistant polypropylene inverted cone joint, and the third microfluidic channel is connected to the collection device through a transparent polytetrafluoroethylene tube and a high-temperature resistant polypropylene inverted cone joint.

[0035] As a preferred technical solution, the collection device uses a 50mL spigot centrifuge tube or a 100mL conical flask to receive the material synthesized in the third microfluidic channel.

[0036] As a preferred technical solution, the first syringe and the second syringe are both syringes matched with the injection pump, with a specification of 10-50mL.

[0037] As an optimal technical solution, the upper plate and the lower plate are both made of metal aluminum or copper plates, the length and width of the upper plate and the lower plate are both (90-110)×(60-80) mm, and the thickness is 5-10 mm. The gasket is made of fluororubber or nitrile rubber gasket, and the thickness of the gasket is 1-4 mm.

[0038] Furthermore, the width of the microfluidic channel is 0.4-0.6mm, the depth is 0.2-0.4mm, the flow channel length of the first microfluidic channel and the second microfluidic channel is 150-250mm, the third microfluidic channel is the precursor mixing reaction zone, and the flow channel length of the third microfluidic channel is 500-600mm.

[0039] As a preferred technical solution, the microfluidic pipelines are all etched with a square cross-section flow channel using a photolithography machine.

[0040] As a preferred technical solution, the microfluidic chip can withstand a temperature range of 25-200°C.

[0041] As a preferred technical solution, the flow rate range adjusted by the injection pump is 50-1000 μL / min.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The present invention provides a continuous and controllable preparation and application of high-stability full-spectrum perovskite nanocrystals. The preparation method realizes the synthesis of high-stability full-spectrum perovskite nanocrystals based on a microfluidic chip; microfluidics refers to the science and technology involved in the system of using microfluidic pipes to accurately process and manipulate tiny fluids, and has the characteristics of miniaturization and integration; the common design of the existing microfluidic reaction method is to combine a polytetrafluoroethylene tube with a heating table, but the pipe and the heating table cannot be tightly combined to form a completely closed high-temperature reaction space, and it is difficult to fix the polytetrafluoroethylene tube to the heating table; the microfluidic chip device of the present invention is simple, the heat transfer rate of the aluminum chip is fast, and the reaction area is completely sealed in the high-temperature space;

[0044] (2) The microfluidic chip in the present invention uses a photolithography machine to directly etch a pipeline on an aluminum plate and seal the pipeline with a fluororubber gasket, which makes up for the complex design defects of the existing microfluidic reaction device; the microfluidic chip reaction method can enhance the heat and mass transfer rates of the reaction reagents, and can achieve uniform mixing of the reaction reagents within a few seconds. The rapid and efficient mixing can reduce the difference in the residence time between the reaction reagents. At the same time, the present invention can quickly, continuously and controllably synthesize perovskite nanocrystal particles with good repeatability, good dispersibility and uniform particle size by accurately controlling the preheating and reaction temperature of the reaction reagents in the microfluidic channel, as well as the flow rate in the flow channel and other parameters, and can achieve large-scale preparation of perovskite nanocrystals; and the flow channel has a small cross-sectional area, and the mixing rate of the reaction substances is faster, which is more conducive to the reaction; the first fluid phase is a cesium precursor, and the second fluid phase is a lead precursor. The reaction phase is not divided into small droplets by fluoro oil, but flows continuously, and the reaction zone is uninterrupted;

[0045] (3) In the existing research on compounding perovskite nanocrystals with inorganic material titanium dioxide, the luminescence intensity of perovskite nanocrystals is generally reduced. However, the present invention uses nano-titanium dioxide to coat perovskite nanocrystals, which not only enhances the luminescence intensity of perovskite nanocrystals, promotes carrier migration, and enhances the water stability and thermal stability of perovskite nanocrystals, but also realizes full spectrum regulation of highly stable perovskite nanocrystals according to the composition and proportion of lead halide, thereby promoting the widespread application of perovskite nanocrystals in the field of optoelectronic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is a schematic diagram of the external structure of a device for preparing highly stable full-spectrum perovskite nanocrystals in an embodiment of the present invention;

[0047] Figure 2Schematic diagram of the internal structure of a device for preparing highly stable full-spectrum perovskite nanocrystals in an embodiment of the present invention;

[0048] Figure 3 The photoemission spectra of the perovskite nanocrystals in Example 9 and Comparative Example 2 of the present invention;

[0049] Figure 4 This is a field emission scanning electron microscope image of nano titanium dioxide in Comparative Example 1 of the present invention;

[0050] Figure 5 This is a field emission scanning electron microscope image of the perovskite nanocrystal in Comparative Example 2 of the present invention;

[0051] Figure 6 This is a field emission scanning electron microscope image of the highly stable full-spectrum perovskite nanocrystal in Example 9 of the present invention;

[0052] Figure 7 It is a line graph of the thermal stability luminescence intensity of the perovskite nanocrystals in Example 9 of the present invention and Comparative Example 2;

[0053] Figure 8 It is a line graph of the water stability luminescence intensity of the perovskite nanocrystals in Example 9 of the present invention and Comparative Example 2;

[0054] Fig. 9 This is a photoemission spectrum of the highly stable full-spectrum perovskite nanocrystals in an embodiment of the present invention.

[0055] Description of the markings in the figure:

[0056] 1—syringe pump, 2—first syringe, 3—second syringe, 4—upper plate, 5—gasket, 6—lower plate, 7—first microfluidic channel, 8—second microfluidic channel, 9—third microfluidic channel, 10—heating stage, 11—collecting device. DETAILED DESCRIPTION

[0057] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0058] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.

[0059] Embodiments 1 to 9:

[0060] A preparation device for highly stable full-spectrum perovskite nanocrystals, such as Figure 1 and Figure 2 As shown, it includes a syringe pump 1, a first syringe 2, a second syringe 3, a microfluidic chip, a heating platform 10 and a collecting device 11, and the microfluidic chip includes an upper plate 4, a gasket 5, a lower plate 6, a first microfluidic channel 7, a second microfluidic channel 8 and a third microfluidic channel 9;

[0061] The lower plate 6 is provided with a first microfluidic pipeline 7, a second microfluidic pipeline 8 and a third microfluidic pipeline 9, which are connected in a T-shaped channel manner, the first syringe 2 is connected to the first microfluidic pipeline 7 through a transparent polytetrafluoroethylene (PTFE) tube and a high-temperature resistant polypropylene (PP) inverted cone joint, the second syringe 3 is connected to the second microfluidic pipeline 8 through a transparent PTFE tube and a high-temperature resistant PP inverted cone joint, and the third microfluidic pipeline 9 is connected to the collecting device 11 through a transparent PTFE tube and a high-temperature resistant PP inverted cone joint;

[0062] The first syringe 2 and the second syringe 3 are connected to the syringe pump 1, and the syringe pump 1 is used to push the first syringe 2 and the second syringe 3. The upper plate 4 is arranged on the lower plate 6, and the upper plate 4 is sealed and connected to the lower plate 6 through the gasket 5. A heating platform 10 is arranged under the lower plate 6, and the heating platform 10 is used to heat the lower plate 6;

[0063] The collecting device 11 is a 50 mL spigot centrifuge tube commonly used in laboratories, and is used to receive the material synthesized in the third microfluidic channel 9;

[0064] The first syringe 2 and the second syringe 3 are syringes matched with the syringe pump 1, and the specification is 10-50mL, and preferably 10mL in this embodiment;

[0065] The upper plate 4 and the lower plate 6 are both made of metal aluminum plates, the length and width of the upper plate 4 and the lower plate 6 are both 100×70 mm, the thickness is both 8 mm, the gasket 5 is a fluororubber gasket, and the thickness of the gasket 5 is 2 mm;

[0066] The microfluidic channels are etched with a photolithography machine with a width of 0.5 mm, a depth of 0.3 mm, and a depth of 0.15 mm. 2 The square cross-sectional flow channel has a cross-sectional area, the flow channel lengths of the first microfluidic channel 7 and the second microfluidic channel 8 are both 200 mm, and the third microfluidic channel 9 is a precursor mixing reaction zone, and the flow channel length is 530 mm;

[0067] The temperature range that the microfluidic chip can withstand is 25-200°C;

[0068] The flow rate range of the syringe pump 1 is 50-1000 μL / min.

[0069] A highly stable full-spectrum perovskite nanocrystal, wherein the surface of nano-titanium dioxide (TiO2) is fully modified by lead halide (PbX2), and the perovskite (CsPbX3) nanocrystal generated by the reaction of PbX2 with a cesium precursor is in situ combined with nano-TiO2 during the synthesis process, and the nano-TiO2 covers the CsPbX3 nanocrystal to modify the surface defects of the CsPbX3 nanocrystal;

[0070] In Examples 1 to 9, different PbX2 compositions and ratios are used, namely Cl:Br=3:0, Cl:Br=2:1, Cl:Br=1.5:1.5, Cl:Br=1:2, Cl:Br=0:3, Br:I=2:1, Br:I=1.5:1.5, Br:I=1:2 and Br:I=0:3.

[0071] The above-mentioned method for preparing highly stable full-spectrum perovskite nanocrystals, which continuously and controllably prepares perovskite nanocrystals through the above-mentioned device, has the following specific steps:

[0072] S1. Prepare the precursor solution: weigh 0.814 g of cesium carbonate (Cs2CO3), 2.5 mL of oleic acid (OA) and 40 mL of octadecene (ODE) and put them into a 100 mL three-necked flask, stir them magnetically at 120°C for 1 h under a nitrogen atmosphere, then heat to 150°C and stir them magnetically for 0.5 h. Cs2CO3 and OA react completely to obtain cesium oleate (Cs-Oleate) solution. Take 0.5 mL of Cs-Oleate solution in a 25 mL three-necked flask, add 9.5 mL of ODE to dilute it, and stir it magnetically at 120°C for 10 min under a nitrogen atmosphere until the solution becomes clear, which is used as the first precursor solution.

[0073] S2. PbX2 was weighed at different halogen molar ratios, the total molar amount of different halogens weighed was 0.376 mmol, and the molar ratios were Cl:Br=3:0, Cl:Br=2:1, Cl:Br=1.5:1.5, Cl:Br=1:2, Cl:Br=0:3, Br:I=2:1, Br:I=1.5:1.5, Br:I=1:2 and Br:I=0:3, and 0.1 g of nano-TiO2, 1 mL of OA, 1 mL of oleylamine (OAm) and 10 mL of ODE were added into a 50 mL three-necked flask, and the mixture was stirred magnetically at 120 ° C for 0.5 h under a nitrogen atmosphere. The surface of nano-TiO2 was fully modified by PbX2 to form lead halide / nano-titanium dioxide (PbX2 / TiO2), and PbX2 / TiO2 completely reacted with OA and OAm to obtain a PbX2 / TiO2 solution as a second precursor solution;

[0074] S3, transfer 10 mL of the first precursor solution and the second precursor solution to the first syringe 2 and the second syringe 3 respectively, wherein the ion molar ratio is Cs:Pb=1:6; connect the first syringe 2 and the second syringe 3 to the microfluidic chip and the collection device 11 through a transparent PTFE tube and a high-temperature resistant PP inverted cone joint; place the aluminum microfluidic chip on the heating table 10, adjust the temperature of the heating table 10 to 160°C, adjust the flow rate of the injection pump 1 to 500 μL / min, drive the precursor solutions in the first syringe 2 and the second syringe 3 to The mixture flows evenly in the microfluidic channel; the reaction time is determined by the flow rate of the mixed precursor in the reaction zone and the width, depth and flow channel length of the cross-section of the microfluidic channel in the reaction zone, and the reaction time is 5s; the liquid in the collecting device 11 is centrifuged at a speed of 10000r / min for 5min, and the supernatant is discarded to obtain a highly stable full-spectrum perovskite (CsPbX3 / TiO2) nanocrystal precipitate, which is washed twice with an appropriate amount of n-hexane by centrifugation at a speed of 10000r / min for 5min, and the CsPbX3 / TiO2 nanocrystal precipitate is dispersed in n-hexane for characterization.

[0075] In order to smoothly synthesize CsPbX3 / TiO2 nanocrystals, the experimental temperature needs to be controlled at 140-180°C, preferably 160°C in this embodiment; the experimental flow rate needs to be controlled at 300-800 μL / min, preferably 500 μL / min in this embodiment.

[0076] The raw material composition and process parameters for preparing the first precursor solution and the second precursor solution in the embodiment are shown in Table 1.

[0077] Table 1 Preparation raw material composition and process parameters of the embodiment

[0078]

[0079] Comparative Example 1:

[0080] Nano titanium dioxide.

[0081] Comparative Example 2:

[0082] A device for preparing perovskite nanocrystals is the same as that in the embodiment.

[0083] A perovskite nanocrystal is substantially the same as Example 9, except that PbI2 directly reacts with a cesium precursor to generate CsPbI3 nanocrystals.

[0084] The method for preparing the above perovskite nanocrystals is basically the same as that of Example 9, except that in step S2, nano-TiO2 is not added to the second precursor solution to obtain CsPbI3 nanocrystals.

[0085] The emission spectra of the high-stability full-spectrum perovskite nanocrystals in Example 9 and the perovskite nanocrystals in Comparative Example 2 were tested using a fluorescence spectrometer (HITACHI F-7500).

[0086] like Figure 3 As shown, under 577nm excitation, the luminescence intensity of the CsPbX3 nanocrystals compounded with nano-TiO2 in Example 9 is significantly higher than the luminescence intensity of the CsPbX3 nanocrystals in Comparative Example 2.

[0087] Field emission scanning electron microscope images of the high-stability full-spectrum perovskite nanocrystals in Example 9, the nano-titanium dioxide in Comparative Example 1, and the perovskite nanocrystals in Comparative Example 2 were taken.

[0088] like Figure 4 As shown, the shape of the nano-TiO2 in Comparative Example 1 is mainly spherical particles agglomerated together.

[0089] like Figure 5 As shown, the morphology of the CsPbX3 nanocrystals in Comparative Example 2 is rod-shaped and the surface is relatively smooth, and the surface of the CsPbX3 nanocrystals is completely exposed.

[0090] like Figure 6 As shown, the morphology of the CsPbX3 / TiO2 nanocrystals in Example 9 is rod-shaped and the surface is covered with a large amount of nano-TiO2, and the surface exposure area is reduced.

[0091] The high-stable full-spectrum perovskite nanocrystals dispersed in n-hexane in Example 9 and the nanocrystals dispersed in n-hexane in Comparative Example 2 were centrifuged at 10000 r / min to obtain CsPbI3 / TiO2 nanocrystals and CsPbI3 nanocrystals precipitates, which were placed in a vacuum drying oven and stored at room temperature for 4 hours. The CsPbI3 / TiO2 nanocrystals and CsPbI3 nanocrystals were ground for 10 minutes and then tested for thermal stability at 30-110°C.

[0092] like Figure 7 As shown, although the luminescence intensity of the nanocrystals in Example 9 and Comparative Example 2 decreases with the increase of temperature, the luminescence intensity decrease trend of the CsPbX3 nanocrystals compounded with nano-TiO2 in Example 9 is significantly weaker than that of the CsPbX3 nanocrystals in Comparative Example 2. The fluorescence of the CsPbI3 nanocrystals in Comparative Example 2 is quenched at 110°C, while the luminescence intensity of the CsPbI3 nanocrystals compounded with nano-TiO2 in Example 9 is maintained at 52% of the initial value at 110°C, indicating that the compounding with nano-TiO2 enhances the thermal stability of the CsPbX3 nanocrystals.

[0093] The highly stable full-spectrum perovskite nanocrystals dispersed in n-hexane in Example 9 and the nanocrystals dispersed in n-hexane in Comparative Example 2 were mixed with deionized water in a volume ratio of 1:1, and the spectral changes of CsPbI3 / TiO2 nanocrystals and CsPbI3 nanocrystals were recorded every 5 minutes.

[0094] like Figure 8 As shown, although the luminescence intensity of the nanocrystals in Example 9 and Comparative Example 2 decreases with time, the luminescence intensity decrease trend of the CsPbX3 nanocrystals composited with nano-TiO2 in Example 9 is significantly weaker than that of the CsPbX3 nanocrystals in Comparative Example 2. The fluorescence of the CsPbI3 nanocrystals in Comparative Example 2 is quenched after 0.5 h, while the luminescence intensity of the CsPbI3 nanocrystals composited with nano-TiO2 in Example 9 is maintained at 38% of the initial value after 0.5 h, indicating that the composite with nano-TiO2 enhances the water stability of the CsPbX3 nanocrystals.

[0095] The emission spectra of the highly stable full-spectrum perovskite nanocrystals in Examples 1 to 9 at their respective optimal excitation wavelengths were tested using a fluorescence spectrometer.

[0096] like Fig. 9 As shown, the emission wavelength can be adjusted in the 408-702nm band, and the half-peak width can be adjusted in the 13.2-34.4nm range, indicating that full-spectrum regulation of highly stable perovskite nanocrystals can be achieved according to the composition and proportion of lead halide, which promotes the widespread application of perovskite nanocrystals in the field of optoelectronic materials.

[0097] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A highly stable full-spectrum perovskite nanocrystal, characterized in that: The surface of nano-titanium dioxide is modified by lead halide, and the lead halide reacts with a cesium precursor to generate perovskite nanocrystals that are in situ combined with nano-titanium dioxide during the synthesis process, and the nano-titanium dioxide covers the perovskite nanocrystals; The lead halide is selected from one or more of lead chloride, lead bromide, and lead iodide. The molar ratio of the lead halide to nano-titanium dioxide is 1:(1-4). The molar ratio of cesium to lead in the cesium precursor and the lead halide is 1:(2-7).

2. The highly stable full-spectrum perovskite nanocrystal according to claim 1, characterized in that: The cesium source of the cesium precursor includes cesium carbonate or cesium acetate.

3. A method for preparing highly stable full-spectrum perovskite nanocrystals as claimed in claim 1 or 2, characterized in that: The method comprises the following steps: S1. Preparing a precursor solution: mixing a cesium source, oleic acid and octadecene under an inert gas atmosphere, and then heating and mixing to obtain a cesium oleate solution, adding octadecene to the cesium oleate solution to dilute it, and mixing them under an inert gas atmosphere to obtain a first precursor solution; S2, mixing lead halide, nano-titanium dioxide, oleic acid, oleylamine and octadecene under an inert gas atmosphere to obtain a lead halide / nano-titanium dioxide solution as a second precursor solution; S3. The first precursor solution and the second precursor solution are transferred to the first syringe (2) and the second syringe (3) respectively; the microfluidic chip is placed on a heating platform (10), and the injection pump (1) drives the precursor solutions in the first syringe (2) and the second syringe (3) to flow evenly and mix and react in the microfluidic channel to obtain highly stable full-spectrum perovskite nanocrystals.

4. The method for preparing a highly stable full-spectrum perovskite nanocrystal according to claim 3, characterized in that: In step S1, the molar / volume ratio of cesium, oleic acid and octadecene in the cesium source is 1 mol:(0.4-0.6L):(6-9L).

5. The method for preparing a highly stable full-spectrum perovskite nanocrystal according to claim 3, characterized in that: In step S2, the molar / volume ratio of lead halide, nano-titanium dioxide, oleic acid, oleylamine and octadecene is 1 mol:(1-4 mol):(1-3 L):(1-3 L):(20-40 L).

6. The method for preparing a highly stable full-spectrum perovskite nanocrystal according to claim 3, characterized in that: The mixing temperature in step S1 is 110-130°C and the mixing time is 1-1.5h; The heating mixing temperature is 140-160°C and the time is 0.5-1h; The dilution multiple is 15-25 times, the mixing temperature during dilution is 110-130°C, and the time is 10-15 minutes.

7. The method for preparing a highly stable full-spectrum perovskite nanocrystal according to claim 3, characterized in that: The mixing temperature in step S2 is 110-130° C. and the mixing time is 0.5-1 h.

8. The method for preparing a highly stable full-spectrum perovskite nanocrystal according to claim 3, characterized in that: In step S3, the reaction time is 3-8 s, the reaction temperature is 140-180° C., and the flow rate is 300-800 μL / min.

9. A device for preparing highly stable full-spectrum perovskite nanocrystals, wherein the device is used to continuously and controllably prepare perovskite nanocrystals using the method according to claim 3, characterized in that: The device comprises a syringe pump (1), a first syringe (2), a second syringe (3), a microfluidic chip, a heating platform (10) and a collecting device (11); the microfluidic chip comprises an upper plate (4), a gasket (5), a lower plate (6), a first microfluidic channel (7), a second microfluidic channel (8) and a third microfluidic channel (9); The lower plate (6) is provided with a first microfluidic channel (7), a second microfluidic channel (8) and a third microfluidic channel (9); the first microfluidic channel (7), the second microfluidic channel (8) and the third microfluidic channel (9) are connected in a T-shaped channel manner; the first syringe (2) is connected to the first microfluidic channel (7); the second syringe (3) is connected to the second microfluidic channel (8); and the third microfluidic channel (9) is connected to a collecting device (11); The first syringe (2) and the second syringe (3) are connected to a syringe pump (1); an upper plate (4) is arranged on the lower plate (6); the upper plate (4) is sealed and connected to the lower plate (6) via a gasket (5); and a heating platform (10) is arranged under the lower plate (6).

10. The device for preparing highly stable full-spectrum perovskite nanocrystals according to claim 9, characterized in that: The width of the microfluidic channel is 0.4-0.6 mm, and the depth is 0.2-0.4 mm. The flow channel lengths of the first microfluidic channel (7) and the second microfluidic channel (8) are 150-250 mm. The third microfluidic channel (9) is a precursor mixing reaction zone, and the flow channel length of the third microfluidic channel (9) is 500-600 mm.

Citation Information

Patent Citations

  • Perovskite / titanium dioxide composite nanocrystal preparation method

    CN110607172A

  • Microfluidics-based perovskite quantum dot preparation method

    CN116590011A

  • Preparation method of perovskite quantum dot based on micro-fluidics

    CN109456764A

  • Device and method for continuous and controllable synthesis of uniform nanocrystalline at normal temperature

    CN110902715A

  • Perovskite quantum dot and mesoporous silica composite luminescent material and preparation thereof

    CN114058367A

Cited By

  • Halogen mixed quantum dot as well as high-flux continuous preparation method and application thereof

    CN122302874A