Phenanthroline bottom-buried modified inversion inorganic perovskite solar cell and preparation method thereof

By using phenanthroline and its derivatives as buried interface modification materials to regulate the crystallization process of the perovskite layer, the film stability and defect problems of all-inorganic perovskite solar cells are solved, and efficient energy conversion and humidity stability are achieved. Improved battery performance.

CN118866992APending Publication Date: 2024-10-29XIDIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410803372.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

All-inorganic perovskite solar cell films are prone to halide phase separation, have poor stability, and have high defect density, which affects carrier transmission and battery stability.

Method used

Phenanthroline and its derivatives are used as buried interface modification materials. Through coordination with Pb2+ in the perovskite layer, the crystallization process is regulated, defects and phase separation are reduced, the quality and light absorption performance of the perovskite layer are improved, and through rotation Coating technology to prepare perovskite light-absorbing layer and electron transport layer.

Benefits of technology

It improves the high energy conversion efficiency and humidity stability of inverse all-inorganic perovskite solar cells, reduces the probability of carrier recombination at the interface, and enhances the thermal stability and life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118866992A_ABST
    Figure CN118866992A_ABST
Patent Text Reader

Abstract

The invention relates to a phenanthroline bottom-buried modified inversion inorganic perovskite solar cell and a preparation method thereof, and the inversion inorganic perovskite solar cell comprises a substrate, an anode, a hole transport layer, a bottom-buried interface modification layer, a perovskite light absorption layer, an electron transport layer and a cathode which are sequentially stacked, the buried bottom interface modification layer is made of one or more of phenanthroline and phenanthroline derivatives; the perovskite light absorption layer is made of an inorganic lead-containing perovskite material. The perovskite solar cell is prepared by taking phenanthroline and the derivative thereof as a buried interface modification material, the growth process of perovskite can be regulated and controlled to a certain extent, phase separation of all-inorganic perovskite is inhibited, interface energy level matching is optimized, and the humidity and thermal stability of the inverted all-inorganic perovskite cell are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new energy technology, and specifically relates to a phenanthroline-buried modified inverse inorganic perovskite solar cell and a preparation method thereof. Background Art

[0002] All-inorganic perovskite battery CsPbI 3-x Br x (0≤x≤3) has attracted much attention in the field of tandem cells due to its good thermal stability, high absorption coefficient and ideal band gap. Mixed halide anions are often used to optimize the band gap and stability of all-inorganic perovskite materials, but they also cause the following problems: (1) Mixed halogen all-inorganic perovskite films are prone to halide phase separation, and the perovskite film phase stability is poor; (2) The defect density is large. The positively charged metal cations and negatively charged halide anion defects can not only act as non-radiative recombination centers to affect carrier transport, but also provide a path for the penetration of water or oxygen molecules, resulting in serious non-radiative recombination at the perovskite / transport layer interface, which has a serious impact on the photoelectric conversion efficiency and stability of the battery.

[0003] In response to the above problems, many literatures at this stage use strategies such as precursor doping, defect passivation, and transport layer interface modification to regulate the microstructure of perovskite films and the interface electrical properties of perovskite / transport layer, which has improved the quality, phase stability, or interface carrier transport characteristics of all-inorganic perovskite films to a certain extent. However, precursor doping may introduce defects in the perovskite lattice, forming scattering or capture centers, and damaging the interface carrier transport efficiency. Interface modification usually involves depositing interface modification molecules on the surface of the perovskite layer to regulate the interface energy level or passivate the perovskite surface / grain boundary defects. It has a single function and generally does not form specific interface interactions or has a certain damage to the interface carrier mobility. Therefore, the stability of the interface modification strategy is poor and is easily affected by the environment.

[0004] Therefore, improving the quality and phase stability of all-inorganic perovskite films has become an urgent problem to be solved. Summary of the invention

[0005] In order to solve the above problems existing in the prior art, the present invention provides a phenanthroline-buried modified inverse inorganic perovskite solar cell and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:

[0006] The embodiment of the present invention provides a phenanthroline-buried inverted inorganic perovskite solar cell, comprising: a substrate, an anode, a hole transport layer, a buried interface modification layer, a perovskite light absorption layer, an electron transport layer and a cathode stacked in sequence, wherein:

[0007] The material of the buried interface modification layer includes one or more of phenanthroline and phenanthroline derivatives;

[0008] The material of the perovskite light-absorbing layer is an inorganic lead-containing perovskite material.

[0009] In one embodiment of the present invention, the thickness of the buried bottom interface modification layer is 50 - 300 nm;

[0010] The phenanthroline derivative includes one or more of phenanthroline compound Phen 1 and phenanthroline compound Phen 2;

[0011] The molecular structural formula of the phenanthroline is:

[0012] The molecular structural formula of the phenanthroline compound Phen 1 is:

[0013]

[0014] The molecular structural formula of the phenanthroline compound Phen 2 is:

[0015]

[0016] In one embodiment of the present invention, the thickness of the perovskite light-absorbing layer is 100 - 300 nm;

[0017] The inorganic lead-containing perovskite material includes one or more of CsPbCl3, CsPbI3, CsPbBr3, CsPbI 3-x Br x (0 < x < 3);

[0018] In one embodiment of the present invention, the material of the substrate includes one or more of silicon wafers, glass, flexible metal foils, and flexible plastics;

[0019] The material of the hole transport layer includes one or more of MeO-2PACz, Me-4PACz, Spiro-MeOTAD, PMMA, and NiO x ;

[0020] The material of the electron transport layer includes PC 61 BM, TiO2, and ZnO;

[0021] The material of the cathode includes one or more of Ag and Cu.

[0022] In one embodiment of the present invention, a cathode buffer layer is further included, and the cathode buffer layer is located between the transport layer and the cathode.

[0023] In one embodiment of the present invention, the number of the cathode buffer layers is 2;

[0024] The material of the cathode buffer layer includes C 60 , or one or more of BCP.

[0025] Another embodiment of the present invention provides a method for preparing a phenanthroline-buried modified inverse inorganic perovskite solar cell, comprising the steps of:

[0026] S1. Pre-treating a substrate substrate, wherein the substrate substrate comprises a substrate and an anode located on a surface of the substrate;

[0027] S2, preparing a hole transport layer on the surface of the substrate having the anode;

[0028] S3, preparing a buried interface modification layer on the surface of the hole transport layer, wherein the material of the buried interface modification layer includes one or more of phenanthroline and phenanthroline derivatives;

[0029] S4, preparing a perovskite light-absorbing layer on the surface of the buried interface modification layer, wherein the material of the perovskite light-absorbing layer is an inorganic lead-containing perovskite material;

[0030] S5, preparing an electron transport layer on the surface of the perovskite light absorbing layer;

[0031] S6. Preparing a cathode on the surface of the electron transport layer.

[0032] In one embodiment of the present invention, step S3 includes:

[0033] S31, dissolving the buried interface modification material in an isopropanol or ethanol solution to obtain a precursor solution of the buried interface modification material;

[0034] S32, spin coating the precursor solution of the buried interface modification material on the hole transport layer at a spin coating speed of 2000-6000 r / min and a spin coating time of 30-50 s to form a buried interface modification layer.

[0035] In one embodiment of the present invention, step S4 includes:

[0036] S41, using a one-step spin coating method to spin-coat a perovskite precursor solution on the surface of the buried interface modification layer, wherein the spin coating conditions are: firstly spin coating at a speed of 500 to 2000 r / min for 3 to 10 seconds, and then increasing the speed to 2000 to 6000 r / min for 20 to 40 seconds;

[0037] S42, annealing the spin-coated substrate in an air environment at a temperature of 100 to 200° C. for 5 to 30 minutes to form a perovskite light-absorbing layer.

[0038] In one embodiment of the present invention, before step S6, the method further includes:

[0039] A cathode buffer layer is prepared on the surface of the electron transport layer.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1. In the perovskite solar cell of the present invention, the material of the buried interface modification layer is one or more of phenanthroline and phenanthroline derivatives, and the material of the perovskite light absorption layer is an inorganic lead-containing perovskite material. Since the two N atoms in the o-phenanthroline skeleton of phenanthroline and its derivatives have chelating ability, they can act as a Lewis base and react with Pb in the top perovskite. 2+ A coordination effect occurs, thereby regulating the crystallization process of the perovskite layer, promoting crystal orientation, reducing defect formation and phase separation, and improving the perovskite crystal quality and light absorption performance. At the same time, phenanthroline and its derivatives also have the advantage of matching the HOMO energy level or valence band of the hole transport layer and the perovskite light absorption layer, ultimately achieving high energy conversion efficiency and high humidity stability of inverted all-inorganic perovskite solar cells.

[0042] 2. In the perovskite solar cell of the present invention, the steric hindrance of the triphenylethylene group in the phenanthroline derivative can reduce the π-π interaction between it and the hole transport layer, reduce the close stacking between it and the perovskite layer, and greatly reduce the probability of carrier recombination at the interface. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 A schematic diagram of the structure of a perovskite solar cell modified with a phenanthroline derivative provided in an embodiment of the present invention;

[0044] Figure 2 A schematic diagram of the structure of a perovskite solar cell modified with a phenanthroline derivative provided in an embodiment of the present invention;

[0045] Figure 3 A schematic flow chart of a method for preparing an inverse inorganic perovskite solar cell modified with phenanthroline buried in an embodiment of the present invention;

[0046] Figure 4a-4g A schematic diagram of the process of preparing a phenanthroline-buried modified inverse inorganic perovskite solar cell provided in an embodiment of the present invention;

[0047] Figure 5 JV curve measurement of the perovskite solar cell provided in the embodiment of the present invention;

[0048] Figure 6 A stability test of the perovskite solar cell provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0049] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.

[0050] Embodiment 1

[0051] See also Figure 1 , Figure 1 A schematic diagram of the structure of a phenanthroline derivative-buried bottom-modified perovskite solar cell provided in an embodiment of the present invention. The perovskite solar cell comprises: a substrate, an anode, a hole transport layer, a buried bottom interface modification layer, a perovskite light absorption layer, an electron transport layer and a cathode stacked sequentially from bottom to top.

[0052] The substrate is a transparent conductive substrate, and its material can be one or more of a large-area silicon wafer, glass, flexible metal foil and flexible plastic. The flexible metal foil includes one or more of stainless steel, molybdenum, titanium, aluminum, copper, etc., and the flexible plastic includes one or more of polyimide (PI), polyethylene terephthalate (PET) or polyethylene naphthalate (PEN). The substrate 1 is used to allow incident light to enter the device from one side of the substrate.

[0053] The surface of the substrate is provided with an anode to form a substrate substrate. Exemplarily, the substrate substrate adopts FTO.

[0054] The materials of the hole transport layer include [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-MeOTAD), polymethyl methacrylate (PMMA), nickel oxide (NiO x The hole transport layer can help the charge transfer in the solar cell and improve the conversion efficiency of the cell.

[0055] The thickness of the buried interface modification layer is 50 to 300 nm, and the material includes one or more of phenanthroline and phenanthroline derivatives. Among them, the molecular structure of phenanthroline is: The phenanthroline derivatives include one or more of the phenanthroline compound Phen1 and the phenanthroline compound Phen 2. The molecular structure of the phenanthroline compound Phen1 is:

[0056]

[0057] The molecular structure of the phenanthroline compound Phen 2 is:

[0058]

[0059] The thickness of the perovskite light-absorbing layer is 100 - 300 nm; the material of the perovskite light-absorbing layer is an inorganic lead-containing perovskite material. The inorganic lead-containing perovskite material includes but is not limited to CsPbCl3, CsPbI3, CsPbBr3, CsPbI 3-x Br x (0 < x < 3), or one or more of them. Exemplarily, the material of the perovskite light-absorbing layer is any one of CsPbCl3, CsPbI3, CsPbBr3, CsPbI2Br, CsPbIBr2. The perovskite light-absorbing layer 5 is the core layer of the perovskite solar cell, and its main function is to absorb sunlight and convert light energy into electrical energy.

[0060] In this embodiment, the two N atoms in the o-phenanthroline skeleton of phenanthroline, phenanthroline compound Phen 1, and phenanthroline compound Phen 2 have chelating ability. As a Lewis base, it can coordinate with Pb in the top perovskite 2+ to regulate the crystallization process of the perovskite layer, promote the crystallization orientation, reduce the formation of defects and phase separation, and improve the perovskite crystallization quality and light absorption performance; the phenanthroline derivative also has the advantage of matching the HOMO energy level or valence band of the hole transport layer and the perovskite light-absorbing layer; at the same time, for phenanthroline compound Phen 1 and phenanthroline compound Phen 2, the steric hindrance of the triphenylethylene group therein can reduce the π-π interaction between it and the hole transport layer, reduce the tight stacking between it and the perovskite layer, and greatly reduce the occurrence probability of carrier recombination at the interface. Therefore, the embodiment of the present invention can achieve high energy conversion efficiency and high humidity stability of the inverted all-inorganic perovskite solar cell.

[0061] The materials of the electron transport layer include PC 61 BM, TiO2, ZnO, or one or more of them. The electron transport layer can enhance the separation effect of electrons and holes, thereby effectively improving the conversion efficiency of the solar cell.

[0062] The materials of the cathode include Ag, Cu, or one or more of them.

[0063] Please refer to Figure 2 , Figure 2 which is a schematic structural diagram of a perovskite solar cell modified by burying a phenanthroline derivative provided by an embodiment of the present invention. The perovskite solar cell includes: a substrate, an anode, a hole transport layer, a buried interface modification layer, a perovskite light-absorbing layer, an electron transport layer, a cathode buffer layer, and a cathode, which are stacked in sequence from bottom to top.

[0064] For the related materials and thicknesses of the substrate, anode, hole transport layer, buried interface modification layer, perovskite light-absorbing layer, electron transport layer, and cathode, please refer to the above embodiments, and will not be elaborated here.

[0065] The cathode buffer layer is arranged between the electron transport layer and the cathode to improve the conversion efficiency of the battery. It can adopt a one-layer structure or a two-layer structure. The specific number of layers is selected according to the battery performance. The materials of the cathode buffer layer include C 60 , or one or more of BCP.

[0066] In a specific embodiment, the cathode buffer layer has two layers, namely a first buffer layer and a second buffer layer. The first buffer layer and the second buffer layer are stacked from bottom to top between the electron transport layer and the cathode.

[0067] The material of the first buffer layer is C 60 , the material of the second buffer layer is BCP.

[0068] This embodiment can inhibit the phase separation of the all-inorganic perovskite, while optimizing the interface energy level matching, and improving the humidity and thermal stability of the inverted all-inorganic perovskite battery.

[0069] Embodiment 2

[0070] Based on Example 1, see Figure 3 and Figure 4a-4g , Figure 3 Schematic diagram of the process for preparing the inverse inorganic perovskite solar cell modified by phenanthroline buried in the embodiment of the present invention, Figure 4a-4g A schematic diagram of the process of preparing a phenanthroline-embedded modified inverse inorganic perovskite solar cell provided in an embodiment of the present invention. The preparation method comprises the steps of:

[0071] S1. Pre-treating the substrate substrate, wherein the substrate substrate comprises a substrate and an anode located on the surface of the substrate, such as Figure 4a Step S1 specifically includes:

[0072] S11, select a substrate with a transparent conductive oxide thin film electrode. Exemplarily, a transparent conductive glass substrate with fluorine-doped tin oxide FTO is selected as the substrate.

[0073] S12. Ultrasonic cleaning is performed on the substrate with a cleaning agent, deionized water and anhydrous ethanol in sequence, and finally the substrate is blown dry with a nitrogen gun.

[0074] S13, placing the substrate wafer in an ultraviolet ozone environment for pretreatment.

[0075] S2, preparing a hole transport layer on the surface of the substrate having the anode, such as Figure 4b Step S2 specifically includes:

[0076] S21, spin coating the prepared hole transport material precursor solution on the substrate; wherein the spin coating speed is 2000-4000 r / min, and the spin coating time is 20-50 s.

[0077] S22, placing the entire substrate on a hot stage for annealing to form a hole transport layer.

[0078] S23, using a poor solvent for hole transport materials to clean the surface of the substrate to reduce the anchored hole transport materials and obtain a hole transport layer.

[0079] S3, preparing a buried interface modification layer on the surface of the hole transport layer, such as Figure 4c As shown, the material of the buried interface modification layer includes one or more of phenanthroline and phenanthroline derivatives. Step S3 specifically includes:

[0080] S31, dissolving the buried bottom interface modification material in an isopropanol or ethanol solution to obtain a precursor solution of the buried bottom interface modification material.

[0081] Specifically, firstly, phenanthroline or a phenanthroline derivative is dissolved in an isopropanol or ethanol solution to obtain a mixed solution; then the mixed solution is stirred at room temperature to obtain a clear phenanthroline precursor solution or a phenanthroline derivative precursor solution.

[0082] S32, spin coating the precursor solution of the buried interface modification material on the hole transport layer at a spin coating speed of 2000-6000 r / min and a spin coating time of 30-50 s to form a buried interface modification layer.

[0083] S4, preparing a perovskite light absorbing layer on the surface of the buried interface modification layer, such as Figure 4d As shown, the material of the perovskite light absorbing layer is an inorganic lead-containing perovskite material. Step S4 specifically includes the following steps:

[0084] S41. Use a one-step spin coating method to spin coat the perovskite precursor solution on the surface of the buried interface modification layer, wherein the spin coating conditions are: first spin coating at a speed of 500-2000 r / min for 3-10 s, and then increase the speed to 2000-6000 r / min for 20-40 s.

[0085] S42, annealing the spin-coated substrate in an air environment at a temperature of 100 to 200° C. for 5 to 30 minutes to form a perovskite light-absorbing layer.

[0086] S5. Prepare an electron transport layer on the surface of the perovskite light absorbing layer, such as Figure 4e Step S5 specifically includes:

[0087] S51, spin coating the prepared electron transport material precursor solution on the perovskite light absorbing layer; wherein the spin coating speed is 1000-3000 r / min, and the spin coating time is 20-40 s.

[0088] S52, placing the entire substrate on a hot stage for annealing in a nitrogen atmosphere to form an electron transport layer, wherein the annealing temperature is 50-200° C. and the annealing time is 3-10 minutes.

[0089] S6. Prepare a cathode buffer layer on the surface of the electron transport layer, such as Figure 4f shown.

[0090] The number of cathode buffer layers is 2, and the material of the first buffer layer is C 60 , taking the material of the first buffer layer as BCP as an example, step S6 specifically includes:

[0091] S61, deposit 10-40nm C on the electron transport layer 60 Cathode buffer layer.

[0092] S62, in C 60 The cathode buffer layer is prepared by depositing 5-10 nm BCP.

[0093] S7, preparing a cathode on the surface of the cathode buffer layer, such as Figure 4g shown.

[0094] Specifically, a 50-200 nm metal electrode is evaporated on the surface of the cathode buffer layer to complete the preparation of the inverted all-inorganic perovskite solar cell.

[0095] It should be noted that the cathode buffer layer is used to improve the conversion efficiency of the battery. This layer can be prepared, and the battery structure formed at this time is: substrate substrate / hole transport layer / phenanthroline and its derivatives buried interface modification layer / perovskite light absorption layer / electron transport layer / first buffer layer / second buffer layer / cathode; it can also not be prepared, and the battery structure formed at this time is: substrate substrate / hole transport layer / phenanthroline and its derivatives buried interface modification layer / perovskite light absorption layer / electron transport layer / cathode. When the cathode buffer layer is not prepared, the cathode is directly prepared on the surface of the electron transport layer.

[0096] This embodiment regulates the perovskite growth process to a certain extent, inhibits the phase separation of the all-inorganic perovskite, optimizes the interface energy level matching, and improves the humidity and thermal stability of the inverted all-inorganic perovskite battery.

[0097] Embodiment 3

[0098] On the basis of Example 1 and Example 2, this example further illustrates a phenanthroline-buried modified inverse inorganic perovskite solar cell and a preparation method thereof.

[0099] Example 1

[0100] The prepared substrate is a glass substrate with fluorine-doped tin oxide FTO, MeO-2PACz is a hole transport layer, Phen 1 phenanthroline derivative is a buried interface modification layer, CsPbI 2.85 Br 0.15 For the perovskite light absorption layer, PC 61 BM is the electron transport layer, C 60 Taking an inverse perovskite solar cell with BCP as the cathode buffer layer and Ag as the cathode as an example, the preparation method of an inverse inorganic perovskite solar cell modified by phenanthroline buried bottom comprises the steps of:

[0101] S1. Pre-treat the substrate, such as Figure 4a Specifically including:

[0102] S11. Select a transparent conductive glass substrate with fluorine-doped tin oxide FTO as the base substrate.

[0103] S12. Ultrasonic clean the substrate with a cleaning agent, deionized water and anhydrous ethanol for 15 minutes in sequence, and finally blow dry with a nitrogen gun.

[0104] S13, placing the substrate in a UV ozone environment for pretreatment for 15 minutes.

[0105] S2, preparing a hole transport layer on the surface of the substrate having the anode, such as Figure 4b As shown. Specifically including the steps:

[0106] S21. First, 1 mg of MeO-2PACz was dissolved in 1 L of ethanol and stirred at room temperature for 6 hours until dissolved to obtain a MeO-2PACz precursor solution. Then, the MeO-2PACz precursor solution was spin-coated on the substrate; wherein the spin-coating speed was 3000 r / min and the spin-coating time was 30 s.

[0107] S22. Place the entire substrate on a hot stage for annealing to obtain a 20 nm MeO-2PACz hole transport layer; wherein the hot stage temperature is 100° C. and the annealing time is 10 min.

[0108] S23, take 200 μL of poor solvent isopropyl alcohol (IPA) and dynamically spin-coat to clean the substrate; wherein the spin-coating speed is 3000 r / min, and the spin-coating time is 30 s.

[0109] S3, depositing a phenanthroline derivative Phen 1 on the surface of the hole transport layer to form a buried interface modification layer, such as Figure 4c Specifically including:

[0110] S31, dissolving 10 mg of Phen 1 in 1 mL of isopropanol solution to obtain a mixed solution, stirring at room temperature for 12 hours until it is completely dissolved, to obtain a 10 mg / mL Phen 1 precursor solution.

[0111] S32, taking 200 μL of Phen 1 precursor solution and dynamically spin-coating it on the hole transport layer, wherein the spin-coating speed is 4000 r / min and the spin-coating time is 40 s, to form a Phen 1 buried interface modification layer.

[0112] S4, preparing a perovskite light absorbing layer on the surface of the buried interface modification layer, such as Figure 4d Specifically including:

[0113] S41. First, prepare a precursor solution of the perovskite light-absorbing layer: take 312 mg CsI, 560 mg PbI2, 33.6 mg PbBr2 and 240 mg DMAI and dissolve them in 1 L of a mixed solution, wherein the mixed solution is composed of DMF and DMSO in a volume ratio of 9:1; then, stir at room temperature for 3 hours to fully dissolve the perovskite light-absorbing material to obtain a light yellow perovskite precursor solution.

[0114] Next, the perovskite precursor solution was spin-coated using a one-step spin coating method, first at a speed of 1000 r / min for 5 s, and then the speed was increased to 4000 r / min for 30 s.

[0115] S42, annealing the spin-coated substrate in an air environment to form a perovskite light-absorbing layer, wherein the annealing temperature is 200° C. and the annealing time is 5 minutes.

[0116] S5. Prepare an electron transport layer on the surface of the perovskite light absorbing layer, such as Figure 4e Specifically including:

[0117] S51. First configure the PC 61 BM precursor solution: take 10 mg PC 61 BM was dissolved in 1 L of chlorobenzene and stirred at room temperature for 6 hours to fully dissolve it to obtain a black precursor solution.

[0118] Then, the configured PC 61 The BM precursor solution is spin-coated on the perovskite light-absorbing layer, wherein the spin-coating speed is 3000 r / min and the spin-coating time is 30 s.

[0119] S52, placing the entire substrate in a glove box and annealing on a hot plate at 60°C for 5 minutes to form a 20nm electron transport layer thin film.

[0120] S6. Prepare a cathode buffer layer on the surface of the electron transport layer, such as Figure 4fSpecifically including:

[0121] S61, use a vacuum evaporator to evaporate 30nm C on the electron transport layer 60 As the first buffer layer, the growth pressure is 1E-4Pa, the power is 100W, and the growth rate is

[0122] S62, use vacuum evaporation machine in C 60 6nm BCP was evaporated as the second buffer layer, the growth pressure was 1E-4Pa, the power was 100W, and the growth rate was

[0123] S7, preparing a cathode on the surface of the cathode buffer layer, such as Figure 4g shown.

[0124] Specifically, a vacuum evaporator was used to evaporate 100 nm Ag on the cathode buffer layer as the cathode, the growth pressure was 1E-4 Pa, the power was 100 W, and the growth rate was

[0125] The batteries prepared by the above method are as follows from bottom to top: FTO / MeO-2PACz / Phen1 / CsPbI 2.85 Br 0.15 / PC 61 BM / C 60 / BCP / Ag.

[0126] Example 2

[0127] The prepared substrate is a glass substrate with fluorine-doped tin oxide FTO, MeO-2PACz is a hole transport layer, Phen 2 phenanthroline derivative is a buried interface modification layer, CsPbI 2.85 Br 0.15 For the perovskite light absorption layer, PC 61 BM is the electron transport layer, C 60 Taking an inverse perovskite solar cell with BCP as the cathode buffer layer and Cu as the cathode as an example, the preparation method of an inverse inorganic perovskite solar cell modified by phenanthroline buried bottom comprises the steps of:

[0128] S1. Pre-treat the substrate, such as Figure 4a Specifically including:

[0129] S11. Select a transparent conductive glass substrate with fluorine-doped tin oxide FTO as the base substrate.

[0130] S12. Ultrasonic clean the substrate with a cleaning agent, deionized water and anhydrous ethanol for 15 minutes in sequence, and finally blow dry with a nitrogen gun.

[0131] S13, placing the substrate in a UV ozone environment for pretreatment for 15 minutes.

[0132] S2, preparing a hole transport layer on the surface of the substrate having the anode, such as Figure 4b Specifically including:

[0133] S21. First, 1 mg of MeO-2PACz was dissolved in 1 L of ethanol and stirred at room temperature for 6 hours until dissolved to obtain a MeO-2PACz precursor solution. Then, the MeO-2PACz precursor solution was spin-coated on the substrate; wherein the spin-coating speed was 3000 r / min and the spin-coating time was 30 s.

[0134] S22. Place the entire substrate on a hot stage for annealing to obtain a 20 nm MeO-2PACz hole transport layer; wherein the hot stage temperature is 100° C. and the annealing time is 10 min.

[0135] S23, take 200 μL of poor solvent isopropyl alcohol (IPA) and dynamically spin-coat to clean the substrate; wherein the spin-coating speed is 3000 r / min, and the spin-coating time is 30 s.

[0136] S3, depositing a phenanthroline derivative Phen 2 on the surface of the hole transport layer to form a buried interface modification layer, such as Figure 4c Specifically including:

[0137] S31. Prepare a precursor solution of a phenanthroline derivative Phen 2: dissolve 15 mg of Phen 2 in 1 mL of ethanol solution to obtain a mixed solution, stir at room temperature for 12 hours until the solution is completely dissolved, and obtain a 15 mg / mL precursor solution of Phen 2.

[0138] S32, spin coating the Phen 2 precursor solution on the hole transport layer; wherein the spin coating speed is 3000 r / min, and the spin coating time is 30 s, to form a Phen 2 buried interface modification layer.

[0139] S4, preparing a perovskite light absorbing layer on the surface of the buried interface modification layer, such as Figure 4d Specifically including:

[0140] S41. First, prepare a precursor solution of the perovskite light-absorbing layer: take 312 mg CsI, 560 mg PbI2, 33.6 mg PbBr2 and 240 mg DMAI and dissolve them in 1 L of a mixed solution, wherein the mixed solution is composed of DMF and DMSO in a volume ratio of 9:1; then, stir at room temperature for 3 hours to fully dissolve the perovskite light-absorbing material to obtain a light yellow perovskite precursor solution.

[0141] Next, the perovskite precursor solution was spin-coated using a one-step spin coating method, first at a speed of 1000 r / min for 5 s, and then the speed was increased to 4000 r / min for 30 s.

[0142] S42, annealing the spin-coated substrate in an air environment to form a perovskite light-absorbing layer, wherein the annealing temperature is 200° C. and the annealing time is 5 minutes.

[0143] S5. Prepare an electron transport layer on the surface of the perovskite light absorbing layer, such as Figure 4e Specifically including:

[0144] S51. First configure the PC 61 BM precursor solution: take 10 mg PC 61 BM was dissolved in 1 L of chlorobenzene and stirred at room temperature for 6 hours to fully dissolve it to obtain a black precursor solution.

[0145] Then, the configured PC 61 The BM precursor solution is spin-coated on the perovskite light-absorbing layer, wherein the spin-coating speed is 3000 r / min and the spin-coating time is 30 s.

[0146] S52, placing the entire substrate in a glove box and annealing on a hot plate at 60°C for 5 minutes to form a 20nm electron transport layer thin film.

[0147] S6. Prepare a cathode buffer layer on the surface of the electron transport layer, such as Figure 4f Specifically including:

[0148] S61, use a vacuum evaporator to evaporate 30nm C on the electron transport layer 60 As the first buffer layer, the growth pressure is 1E-4Pa, the power is 100W, and the growth rate is

[0149] S62, use vacuum evaporation machine in C 60 6nm BCP was evaporated as the second buffer layer, the growth pressure was 1E-4Pa, the power was 100W, and the growth rate was

[0150] S7, preparing a cathode on the surface of the cathode buffer layer, such as Figure 4g shown.

[0151] Specifically, a vacuum evaporator was used to evaporate 100nm Cu as the cathode on the cathode buffer layer, the growth pressure was 1E-4Pa, the power was 100W, and the growth rate was

[0152] The batteries prepared by the above method are as follows from bottom to top: FTO / MeO-2PACz / Phen2 / CsPbI 2.85 Br 0.15 / PC 61 BM / C 60 / BCP / Cu.

[0153] Example 3

[0154] The prepared substrate is a glass substrate with fluorine-doped tin oxide FTO, Me-4PACz is a hole transport layer, Phen 2 phenanthroline derivative is a buried interface modification layer, CsPbI 2.85 Br 0.15 For the perovskite light absorption layer, PC 61 BM is the electron transport layer, C 60 Taking an inverse perovskite solar cell with BCP as the cathode buffer layer and Cu as the cathode as an example, the preparation method of an inverse inorganic perovskite solar cell modified by phenanthroline buried bottom comprises the steps of:

[0155] S1. Pre-treat the substrate, such as Figure 4a Specifically including:

[0156] S11. Select a transparent conductive glass substrate with fluorine-doped tin oxide FTO as the base substrate.

[0157] S12. Ultrasonic clean the substrate with a cleaning agent, deionized water and anhydrous ethanol for 15 minutes in sequence, and finally blow dry with a nitrogen gun.

[0158] S13, placing the substrate in a UV ozone environment for pretreatment for 15 minutes.

[0159] S2, preparing a hole transport layer on the surface of the substrate having the anode, such as Figure 4b Specifically including:

[0160] S21. First, 1 mg of Me-4PACz was dissolved in 1 L of ethanol and stirred at room temperature for 6 hours until dissolved to obtain a Me-4PACz precursor solution. Then, the Me-4PACz precursor solution was spin-coated on the substrate; wherein the spin-coating speed was 3000 r / min and the spin-coating time was 30 s.

[0161] S22. Place the entire substrate on a hot stage for annealing to obtain a 20 nm Me-4PACz hole transport layer; wherein the hot stage temperature is 100° C. and the annealing time is 10 min.

[0162] S23, take 200 μL of poor solvent isopropyl alcohol (IPA) and dynamically spin-coat to clean the substrate; wherein the spin-coating speed is 3000 r / min, and the spin-coating time is 30 s.

[0163] S3, depositing a phenanthroline derivative Phen 2 on the surface of the hole transport layer to form a buried interface modification layer, such as Figure 4c Specifically including:

[0164] S31. Prepare a precursor solution of a phenanthroline derivative Phen 2: dissolve 20 mg of Phen 2 in 1 mL of ethanol solution to obtain a mixed solution, stir at room temperature for 12 hours until the solution is completely dissolved, and obtain a 20 mg / mL precursor solution of Phen 2.

[0165] S32, spin coating the Phen 2 precursor solution on the hole transport layer; wherein the spin coating speed is 3000 r / min, and the spin coating time is 30 s, to form a Phen 2 buried interface modification layer.

[0166] S4, preparing a perovskite light absorbing layer on the surface of the buried interface modification layer, such as Figure 4d Specifically including:

[0167] S41, first prepare a precursor solution of a perovskite light absorbing layer: 182 mg CsI, 392 mg HPbI3 and 11.01 mg PbBr2 are dissolved in 1 L of a mixed solution, wherein the mixed solution is composed of DMF and DMSO in a volume ratio of 9:1. Then, stir at room temperature for 3 hours to fully dissolve the perovskite light absorbing material to obtain a light yellow perovskite precursor solution.

[0168] Next, the perovskite precursor solution was spin-coated using a one-step spin coating method, first at a speed of 1000 r / min for 5 s, and then the speed was increased to 4000 r / min for 30 s.

[0169] S42, annealing the spin-coated substrate in an air environment to form a perovskite light-absorbing layer, wherein the annealing temperature is 200° C. and the annealing time is 5 minutes.

[0170] S5. Prepare an electron transport layer on the surface of the perovskite light absorbing layer, such as Figure 4e Specifically including:

[0171] S51. First configure the PC 61 BM precursor solution: take 10 mg PC 61 BM was dissolved in 1 L of chlorobenzene and stirred at room temperature for 6 hours to fully dissolve it to obtain a black precursor solution.

[0172] Then, the configured PC 61 The BM precursor solution is spin-coated on the perovskite light-absorbing layer, wherein the spin-coating speed is 3000 r / min and the spin-coating time is 30 s.

[0173] S52, placing the entire substrate in a glove box and annealing on a hot plate at 60°C for 5 minutes to form a 20nm electron transport layer thin film.

[0174] S6. Prepare a cathode buffer layer on the surface of the electron transport layer, such as Figure 4f Specifically including:

[0175] S61, use a vacuum evaporator to evaporate 30nm C on the electron transport layer 60 As the first buffer layer, the growth pressure is 1E-4Pa, the power is 100W, and the growth rate is

[0176] S62, use vacuum evaporation machine in C 60 6nm BCP was evaporated as the second buffer layer, the growth pressure was 1E-4Pa, the power was 100W, and the growth rate was

[0177] S7, preparing a cathode on the surface of the cathode buffer layer, such as Figure 4g shown.

[0178] Specifically, a vacuum evaporator was used to evaporate 100nm Cu as the cathode on the cathode buffer layer, the growth pressure was 1E-4Pa, the power was 100W, and the growth rate was

[0179] The batteries prepared by the above method are as follows from bottom to top: FTO / Me-4PACz / Phen2 / CsPbI 2.85 Br 0.15 / PC 61 BM / C 60 / BCP / Cu.

[0180] Furthermore, the all-inorganic perovskite solar cells prepared in Examples 1, 2, and 3 were subjected to optical and electrical tests, and compared with the performance of conventional MeO-2PACz type perovskite solar cells, wherein the conventional MeO-2PACz type perovskite solar cells are, from bottom to top, FTO / MeO-2PACz / CsPbI 2.85 Br 0.15 / PC 61 BM / C 60 / BCP / Cu.

[0181] The effective area of ​​the Phen 1 and Phen 2 perovskite solar cells prepared in Examples 1, 2, and 3 is 7 mm 2 The electrical performance and defect state density of the perovskite solar cells prepared in Examples 1, 2, and 3 were tested under the AM 1.5G solar spectrum. Figure 5 and Figure 6 , Figure 5 The JV curve of the perovskite solar cell provided in the embodiment of the present invention is measured. Figure 6 A stability test of the perovskite solar cell provided in an embodiment of the present invention.

[0182] like Figure 5 As shown, the open circuit voltage (V OC )=1.05V,fill factor (FF)=63.95%,short circuit current density (J SC )=19.82mA / cm 2 , the device photoelectric conversion efficiency (PCE) is 13.31%; Example 1 prepared based on Phen 1 buried interface modification of the solar cell, device V OC =1.05V, fill factor (FF) = 77.30%, short circuit current density (J SC )=20.31mA / cm 2 , the device photoelectric conversion efficiency (PCE) is 16.48%; Example 2 prepared based on Phen 2 buried interface modification of the solar cell, device V OC =1.09V, fill factor (FF) = 76.65%, short circuit current density (J SC )=19.6mA / cm 2 , the device photoelectric conversion efficiency (PCE) is 16.39%; Example 3 prepared based on Phen2 buried interface modification of the solar cell, device V OC =1.05V, fill factor (FF) = 72.54%, short circuit current density (J SC )=21.05mA / cm 2 , the device photoelectric conversion efficiency (PCE) is 16.03%. It can be seen that the addition of phenanthroline derivatives as bottom-buried interface modification materials in the perovskite solar cell in this embodiment improves the open circuit voltage and fill factor of the perovskite solar cell, and finally obtains an inverted all-inorganic perovskite solar cell with excellent performance.

[0183] from Figure 6 It can be seen that the all-inorganic perovskite solar cells prepared using the phenanthroline derivative interface modification materials Phen1 and Phen2 provided in this embodiment still maintain 85% and 80% of the original efficiency after 500 hours, respectively, while the PCE of the reference device not modified with a phenanthroline derivative rapidly decreases to 60% of the initial efficiency.

[0184] All-inorganic perovskite battery CsPbI 3-x Br x(0≤x≤3) has attracted much attention in the field of tandem cells due to its good thermal stability, high absorption coefficient and ideal band gap. Improving the quality of all-inorganic perovskite films, especially accurately controlling the composition and microstructure of perovskite films, and effectively passivating grain boundaries or surface defects, is conducive to the inversion of all-inorganic perovskite solar cells to achieve higher photoelectric conversion efficiency and excellent stability. This application uses phenanthroline and its derivatives as buried interface modification materials to prepare perovskite solar cells, which not only accurately controls the crystallization process of the perovskite layer, promotes crystallization orientation, reduces defect formation and phase separation, but also greatly improves the stability and life of the battery; in addition, flexible all-inorganic perovskite solar cells can also be prepared on flexible substrates, which is conducive to the commercial large-scale preparation and production of perovskite cells. The all-inorganic films and solar cells prepared based on this application have great potential in crystalline silicon-perovskite and perovskite-perovskite tandem cells.

[0185] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A phenanthroline-buried inverse inorganic perovskite solar cell, characterized in that: include: A substrate, an anode, a hole transport layer, a buried interface modification layer, a perovskite light absorption layer, an electron transport layer and a cathode are stacked in sequence, wherein: The material of the buried interface modification layer includes one or more of phenanthroline and phenanthroline derivatives; The material of the perovskite light absorbing layer is an inorganic lead-containing perovskite material.

2. The phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 1, characterized in that: The thickness of the buried interface modification layer is 50 to 300 nm; The phenanthroline derivatives include one or more of phenanthroline compounds Phen 1 and Phen 2; The molecular structural formula of the phenanthroline is: The molecular structural formula of the phenanthroline compound Phen 1 is: The molecular structural formula of the phenanthroline compound Phen 2 is:

3. The phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 1, characterized in that: The thickness of the perovskite light absorbing layer is 100 to 300 nm; The inorganic lead-containing perovskite materials include one or more of CsPbCl3, CsPbI3, CsPbBr3, CsPbI 3-x Br x (0 < x < 3).

4. The phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 1, characterized in that: The material of the substrate includes one or more of silicon wafer, glass, flexible metal foil, and flexible plastic; The materials of the hole transport layer include MeO-2PACz, Me-4PACz, Spiro-MeOTAD, PMMA, NiO x One or more of; The material of the electron transport layer includes PC 61 One or more of BM, TiO2, ZnO; The material of the cathode includes one or more of Ag and Cu.

5. The phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 1, characterized in that: A cathode buffer layer is also included, and the cathode buffer layer is located between the transport layer and the cathode.

6. The phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 5, characterized in that: The number of the cathode buffer layers is 2; The material of the cathode buffer layer includes C 60 , or one or more of BCP.

7. A method for preparing a phenanthroline-buried modified inverse inorganic perovskite solar cell, characterized in that: Includes steps: S1. Pre-treating a substrate substrate, wherein the substrate substrate comprises a substrate and an anode located on a surface of the substrate; S2, preparing a hole transport layer on the surface of the substrate having the anode; S3, preparing a buried interface modification layer on the surface of the hole transport layer, wherein the material of the buried interface modification layer includes one or more of phenanthroline and phenanthroline derivatives; S4, preparing a perovskite light-absorbing layer on the surface of the buried interface modification layer, wherein the material of the perovskite light-absorbing layer is an inorganic lead-containing perovskite material; S5, preparing an electron transport layer on the surface of the perovskite light absorbing layer; S6. Preparing a cathode on the surface of the electron transport layer.

8. The method for preparing a phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 7, characterized in that: Step S3 includes: S31, dissolving the buried interface modification material in an isopropanol or ethanol solution to obtain a precursor solution of the buried interface modification material; S32, spin coating the precursor solution of the buried interface modification material on the hole transport layer at a spin coating speed of 2000-6000 r / min and a spin coating time of 30-50 s to form a buried interface modification layer.

9. The method for preparing a phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 7, characterized in that: Step S4 includes: S41, using a one-step spin coating method to spin-coat a perovskite precursor solution on the surface of the buried interface modification layer, wherein the spin coating conditions are: firstly spin coating at a speed of 500 to 2000 r / min for 3 to 10 seconds, and then increasing the speed to 2000 to 6000 r / min for 20 to 40 seconds; S42, annealing the spin-coated substrate in an air environment at a temperature of 100 to 200° C. for 5 to 30 minutes to form a perovskite light-absorbing layer.

10. The method for preparing a phenanthroline-buried modified inverse inorganic perovskite solar cell according to claim 7, characterized in that: Before step S6, the method further includes: A cathode buffer layer is prepared on the surface of the electron transport layer.