InGaAs material structure based on large overshoot rapid gradient and preparation method thereof

By introducing specific hierarchical structures and a transfer buffer layer into the indium gallium arsenic material, the problems of mismatch stress and dislocation defects during wavelength expansion are solved, and the performance and signal-to-noise ratio of the short-wave infrared detector are improved.

CN118957749APending Publication Date: 2024-11-15SHANGHAI INSTITUTE OF TECHNICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411016947.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing indium gallium arsenic materials have insufficient performance due to mismatch stress and dislocation defects during wavelength expansion, which limits the development of short-wave infrared focal plane detectors.

Method used

Using the indium gallium arsenic material structure based on large overshoot and fast-transfer, the InwAl1-wAs fixed component contact layer, InxGa1-xAs absorbing layer, InwAl1-wAs buffer layer, and InyAl1-yAs relaxation layer are introduced into the indium gallium arsenic material. hierarchical structures such as InzAl1-zAs large overshoot fast-transmitting linear buffer layer and In0.52Al0.48As lattice matching buffer layer are grown in combination with molecular beam epitaxial technology to adjust the material's transmission rate and overshoot degree to reduce mismatch dislocation and relaxation.

Benefits of technology

The crystal quality and minority life of the indium gallium arsenic absorber layer are significantly improved, the performance of the short-wave infrared detector is enhanced, the photolithography efficiency and yield rate are improved, and the signal-to-noise ratio is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957749A_ABST
    Figure CN118957749A_ABST
Patent Text Reader

Abstract

The invention discloses an indium gallium arsenic material structure based on large overshoot rapid gradient and a preparation method thereof. The material structure comprises an InwAl < 1-w > As fixed component contact layer, an In < x > Ga < 1-x > As fixed component absorption layer, an InwAl < 1-w > As fixed component buffer layer, an In < y > Al < 1-y > As fixed component relaxation layer, an In < z > Al < 1-z > As large-overshoot rapid gradient linear buffer layer, an In < 0.52 > Al < 0.48 > As lattice matching buffer layer and an InP homogeneous buffer layer from top to bottom. The InwAl1-wAs fixed component contact layer, the InxGa1-xAs fixed component absorption layer and the InwAl1-wAs fixed component buffer layer are in lattice matching, w is larger than 0.52 and smaller than or equal to 0.85, and x is larger than 0.53 and smaller than or equal to 0.85. The component of the InyAl1-yAs fixed component relaxation layer is w + 0.05 < = y < = 1, the components of the InzAl1-zAs large-overshoot rapid gradient linear buffer layer are linearly and progressively increased from 0.52 to y from bottom to top, the gradient rate is v, and v is larger than or equal to 0.4 / h and smaller than or equal to 0.6 / h. According to the material structure design, the indium gallium arsenic absorption layer can be promoted to grow in a complete relaxation state, wafer warping is greatly reduced, the service life of indium gallium arsenic minority carriers is prolonged, and when a focal plane detector is prepared through the material structure, the high signal-to-noise ratio can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor thin film materials, and in particular relates to an InGaAs material structure based on large overshoot rapid gradient and a preparation method thereof. Background Art

[0002] Indium gallium arsenide (InGaAs) material has good optical and electrical properties and is an excellent short-wave infrared photoelectric detection material. The focal plane detector based on InGaAs material is one of the ideal choices in the field of short-wave infrared detection. The common InGaAs material on the market is InGaAs material that is lattice-matched with the indium phosphide substrate, with a cutoff wavelength of 1.7 microns, which is mainly prepared by molecular beam epitaxy or metal organic chemical vapor deposition technology. However, taking the country's major demand for accurate monitoring of greenhouse gases as an example, CO2 is one of the most important greenhouse gases, and its two main transmittance spectra are located at 1.6 microns (weak absorption band) and 2.06 microns (strong absorption band). These two bands cooperate to complete high-precision inversion, and can perform high-precision quantitative top-down carbon monitoring. The detector based on InGaAs material with a cutoff wavelength of 1.7 microns is not enough to detect the characteristic peak of the strong absorption band of CO2, so it is necessary to increase the indium component in the InGaAs material to achieve wavelength expansion.

[0003] As the indium content in the InGaAs material increases, the mismatch with the InP substrate gradually increases, resulting in mismatch stress inside the material. As the epitaxial growth process proceeds, these mismatch stresses will be released in the form of wafer warping or dislocation defects, which will lead to increased difficulty in lithography alignment, reduced yield of reverse solder interconnection, increased device dark current, increased blind pixel rate and other adverse effects, limiting the development of InGaAs short-wave infrared focal plane detectors towards larger scale and higher performance. At present, stress regulation and defect suppression are mainly achieved by inserting a buffer layer between the InP substrate and the wavelength-extended InGaAs epitaxial material, thereby obtaining epitaxial growth of high-quality wavelength-extended InGaAs materials. This patent provides a high-quality wavelength-extended InGaAs material structure based on a large overshoot fast-gradient buffer layer and a preparation method thereof. Summary of the invention

[0004] The purpose of the present invention is to provide an InGaAs material structure based on large overshoot rapid transition and a preparation method thereof in order to address the problem that the performance of extended wavelength InGaAs detector materials needs to be improved due to mismatch stress and dislocation defects.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A structure of InGaAs material based on large overshoot rapid transition, including In w Al 1-wAs fixed component contact layer, In x Ga 1-x As fixed component absorption layer, In w Al 1-w As fixed component buffer layer, In y Al 1-y As fixed component relaxation layer, In z Al 1-z As large overshoot fast gradient linear buffer layer, In 0.52 Al 0.48 As lattice matching buffer layer, InP homogeneous buffer layer.

[0007] In the above technical solution, w Al 1-w The composition of the As fixed component contact layer is 0.52<w≤0.85, and the thickness ranges from 600-1000nm. For the planar detector structure, In w Al 1-w The As fixed component contact layer is doped with N-type light doping, with a doping concentration of 5×10 15 -5×10 16 cm -3 , for the table-top detector structure, In w Al 1-w The As fixed component contact layer is doped with P-type heavy doping, with a doping concentration of 1×10 18 -5×10 18 cm -3 .

[0008] In the above technical solution, x Ga 1-x The composition of the As fixed component absorption layer is 0.53<x≤0.85, the thickness ranges from 1600-2500nm, and the doping is N-type light doping with a doping concentration of 1×10 15 -5×10 16 cm -3 The invention discloses a structure of InGaAs material based on large overshoot and rapid transition. x Ga 1-x The improvement effect of the As fixed component absorption layer decreases as x increases.

[0009] In the above technical solution, w Al 1-w The composition of the As fixed component buffer layer is 0.52<w≤0.85, the thickness ranges from 200-1000nm, and the doping is N-type heavy doping with a doping concentration of 5×10 17 -5×10 18 cm -3 , and In wAl 1-w As fixed component contact layer, In x Ga 1-x As fixed component absorption layer and In w Al 1-w As fixed component buffer layer three lattice matching to avoid interface mismatch leading to In x Ga 1-x New misfit dislocation defects are introduced into the As fixed component absorption layer, thereby obtaining the epitaxial growth of high-quality extended wavelength InGaAs detector materials.

[0010] In the above technical solution, y Al 1-y The composition of the As fixed component relaxation layer is w+0.05≤y≤1, the thickness range is 0-110nm, the doping is N-type light doping, and the doping concentration is 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 , the difference between y and w, that is, the effect is not obvious when the component is large and the overshoot is too small, In x Ga 1-x As fixed component absorption layer cannot be completely relaxed, at this time In y Al 1-y As fixed component relaxation layer thickness needs to be increased, when the component is large and the overshoot is too large, new defects will be introduced, resulting in increased surface roughness. y Al 1-y The thickness of the As fixed component relaxation layer needs to be reduced.

[0011] In the above technical solution, z Al 1-z As large overshoot rapid gradient linear buffer layer from bottom to top component linearly increases from 0.52 to y, and In z Al 1-z The composition gradient rate of the As large overshoot fast gradient linear buffer layer is v, 0.4 / h≤v≤0.6 / h, the thickness range is 300-1000nm, the doping is N-type light doping, and the doping concentration is 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 Rapid composition gradient is beneficial to limit the climb of misfit dislocations, but the composition gradient rate is limited by the PID temperature control of the source furnace of the molecular beam epitaxy equipment.

[0012] In the above technical solution, 0.52 Al 0.48The As lattice matching buffer layer has a thickness range of 200-400 nm and is doped with light N-type doping at a doping concentration of 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 .

[0013] In the above technical solution, the thickness of the InP homogeneous buffer layer is 40-200nm, and the doping is N-type light doping with a doping concentration of 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 .

[0014] The present invention also discloses a method for preparing an InGaAs material structure based on large overshoot and rapid gradient, which is used to prepare the InGaAs material structure based on large overshoot and rapid gradient as described above, comprising the following steps:

[0015] The InGaAs material structure based on large overshoot rapid gradient is grown by molecular beam epitaxy technology, and the InP substrate is placed on the heater of the pretreatment chamber for pretreatment. The pretreatment conditions are: heating to 300-400°C and placing for 20-40 minutes after reaching the set maximum temperature.

[0016] The pretreated InP substrate was transferred to the sample holder of the growth chamber for deoxidation treatment. The deoxidation conditions were as follows: the sample holder holding the InP substrate was heated to 300°C. When the temperature reached 300°C, the As beam or P beam was immediately turned on to protect the InP substrate to prevent the V group from desorbing in large quantities on the surface of the substrate at higher temperatures. At this time, the vacuum in the growth chamber should be 8×10 -8 -3×10 - 7 Torr, and then heat it to 600-650°C in the protection environment of As beam or P beam. When the temperature reaches the set maximum temperature, clear and bright 4×2 structure stripes can be observed in the imaging on the fluorescent screen through reflection high-energy electron beam diffraction. Let it stand for 5-10 minutes, and then grow the above-mentioned InP homogeneous buffer layer after sufficient deoxidation.

[0017] The InP homogeneous buffer layer is grown on the InP homogeneous buffer layer. 0.52 Al 0.48 As lattice matching buffer layer, in the above In 0.52 Al 0.48 The above-mentioned In is grown on the As lattice matching buffer layer z Al 1-z As large overshoot fast gradient linear buffer layer, for Inz Al 1-z The material growth of the linear buffer layer with large As overshoot and rapid gradient is achieved by increasing the temperature of the In furnace and reducing the temperature of the Al furnace by twice. The composition gradient rate is determined by the temperature change rate of the In furnace and the Al furnace. z Al 1-z As large overshoot fast gradient linear buffer layer is grown on the above In y Al 1-y As fixed component relaxation layer, in the above In y Al 1-y The above-mentioned In is grown on the As fixed composition relaxation layer w Al 1-w As fixed component buffer layer, in the above In w Al 1-w The above-mentioned In x Ga 1-x As fixed component absorption layer, in the above In x Ga 1-x The above-mentioned In w Al 1-w As fixed component contact layer.

[0018] Wait for the above In w Al 1-w After the growth of the As fixed component contact layer is completed, the sample holder is cooled to 300°C under the protection of As atmosphere, the As protection is turned off, and the sample holder is taken out after cooling to room temperature to complete the growth.

[0019] Furthermore, during the growth of the InP homogeneous buffer layer, the sample holder temperature is 530-550°C.

[0020] Furthermore, the In 0.52 Al 0.48 During the growth of the As lattice-matched buffer layer, the sample holder temperature was 570-610 °C.

[0021] Furthermore, the In z Al 1-z As large overshoot fast gradient linear buffer layer and the In y Al 1-y During the growth of the As fixed component relaxation layer, the sample holder temperature was 560-600 °C.

[0022] Furthermore, the In w Al 1-w During the growth of the As fixed component buffer layer, the sample holder temperature was 550-580°C.

[0023] Furthermore, the In x Ga1-x As fixed component absorption layer and the In w Al 1-w During the growth of the As fixed component contact layer, the sample holder temperature was 540-570°C.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention is based on the joint regulation of the gradient rate and overshoot degree of the linear gradient buffer layer. The buffer layer with a faster linear gradient rate suppresses the mismatch dislocation climb caused by mismatch stress. At the same time, the large overshoot regulates the relaxation degree between the InGaAs absorption layer and the InP substrate, promotes the growth of the InGaAs absorption layer in a completely relaxed state, improves the crystallization quality of the InGaAs absorption layer, and increases the minority carrier lifetime of the InGaAs absorption layer, thereby improving the performance of the extended wavelength short-wave infrared InGaAs focal plane detector.

[0026] 2. For the back-illuminated extended-wavelength short-wave infrared InGaAs focal plane detector, increasing the gradient rate of the linear gradient buffer layer is beneficial to obtaining a thinner buffer layer structure, thereby reducing the absorption of the light source by the buffer layer and promoting more light sources to reach the InGaAs layer, which is beneficial to improving the signal-to-noise ratio of the extended-wavelength short-wave infrared InGaAs focal plane detector.

[0027] 3. For the extended wavelength short-wave infrared InGaAs focal plane detector, the InGaAs material structure based on large overshoot and rapid transition of the present invention greatly improves the wafer warpage of the extended wavelength InGaAs material, which is beneficial to improving the lithography efficiency and the yield rate of flip-flop interconnection. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic structural diagram of a preferred embodiment of the present invention.

[0029] The vertical height of each layer in the figure is a schematic representation of the layer thickness, and the horizontal width is a schematic representation of the change in lattice constant corresponding to the change in composition.

[0030] In the figure:

[0031] 1—In w Al 1-w As fixed component contact layer;

[0032] 2—In x Ga 1-x As fixed component absorption layer;

[0033] 3—In w Al 1-w As fixed component buffer layer;

[0034] 4—In y Al 1-y As fixed component relaxation layer;

[0035] 5—In z Al 1-z As large overshoot fast gradient linear buffer layer

[0036] 6—In 0.52 Al 0.48 As lattice matching buffer layer;

[0037] 7—InP homogeneous buffer layer.

[0038] Figure 2 The minority carrier lifetime test and fitting results of the extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown using existing technology.

[0039] Figure 3 The minority carrier lifetime test and fitting results of an extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown based on a large overshoot fast-gradient InGaAs material structure of the present invention are presented.

[0040] Figure 4 Wafer warpage test and pseudo 3D mapping results of extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown using existing technology.

[0041] Figure 5 The present invention discloses wafer warpage test and pseudo 3D mapping results of an extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown based on a large overshoot fast-gradient InGaAs material structure. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. It should be noted that, after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the present application.

[0043] Example 1

[0044] The purpose of this embodiment is to achieve a high quality extended wavelength In with a cut-off wavelength of about 1800nm. 0.57 Ga 0.43 The effective preparation of As focal plane detector material. The InGaAs material structure including the large overshoot fast gradient of the present invention shown in this embodiment is a common back-illuminated mesa PIN structure, which includes the following materials from top to bottom:

[0045] 1.P-type In 0.57 Al 0.43As fixed component contact layer, doped with Be, with a thickness of 1000nm and a doping concentration of 5×10 18 cm -3 ;

[0046] 2.N-type In 0.57 Ga 0.43 As fixed component absorption layer, doped with Si, thickness 1600nm, doping concentration 5×10 16 cm -3 ;

[0047] 3.N-type In 0.57 Al 0.43 As fixed component buffer layer, doped with Si, thickness 1000nm, doping concentration 5×10 18 cm -3 ;

[0048] 4.N-type In 0.64 Al 0.36 As fixed component relaxation layer, doped with Si, thickness 110nm, doping concentration 5×10 16 cm -3 ;

[0049] 5.N-type In z Al 1-z As large overshoot fast gradient linear buffer layer, the composition z linearly changes from 0.52 to 0.64, the composition gradient rate is 0.4 / h, Si is doped, the thickness is 500nm, and the doping concentration is 5×10 16 cm -3 ;

[0050] 6.N-type In 0.52 Al 0.48 As lattice matching buffer layer, doped with Si, thickness 200nm, doping concentration 5×10 16 cm -3 ;

[0051] 7. N-type InP homogeneous buffer layer, doped with Si, thickness 40nm, doping concentration 5×10 16 cm -3 .

[0052] This embodiment adopts molecular beam epitaxy technology for growth, and the growth process is as follows:

[0053] Preliminary experiments have determined that InP and InP can be grown on Fe-doped semi-insulating InP (001) at a growth rate of about 1 μm / h. 0.52 Al 0.48 As、In z Al 1-z As component z changes linearly from 0.52 to 0.64, In 0.64Al 0.36 As、In 0.57 Al 0.43 As and In 0.57 Ga 0.43 As, calibrate the temperature of each beam source furnace, and at the same time calibrate the growth temperature of each layer, V / III ratio and other conditions to determine In z Al 1-z The temperature and heating and cooling rates of the In furnace and Al furnace with the As component z linearly changing from 0.52 to 0.64 determine the N-type doping concentration of 5×10 16 cm -3 and 5×10 18 cm -3 The Si beam source furnace temperature is determined to be 5×10 18 cm -3 Be beam source furnace temperature;

[0054] A piece of Fe-doped semi-insulating InP (001) substrate was placed on the heater of the pretreatment chamber of the molecular beam epitaxy equipment, and the heating temperature was set to 300°C. After reaching the set temperature, it was maintained for 40 minutes to perform substrate pretreatment;

[0055] The pretreated semi-insulating InP (001) substrate was introduced into the growth chamber, and the sample holder temperature was set to 300 °C. When the set temperature was reached, the As beam was immediately turned on. At this time, the growth vacuum was 3×10 -7 Torr, continue to heat up to 650℃, and clear and bright 4×2 structure stripes can be seen. After standing for 10 minutes and fully deoxidizing, the above materials 7 to 1 are grown in sequence, and the type, thickness and concentration of each layer of materials are as described above;

[0056] The growth temperature of the InP homogeneous buffer layer is 530℃. 0.52 Al 0.48 The growth temperature of the As lattice matching buffer layer is 570℃, and the In z Al 1-z As large overshoot fast transition linear buffer layer and In 0.64 Al 0.36 The growth temperature of the As fixed composition relaxation layer is 560℃, and the In 0.57 Al 0.43 The growth temperature of the As fixed composition buffer layer is 550℃, and the In 0.57 Ga 0.43 As fixed component absorption layer and In 0.57 Al 0.43 The growth temperature of the As fixed component contact layer is 540°C;

[0057] After the epitaxial growth is completed, the sample holder is cooled to 300°C under the protection of As atmosphere. After the temperature reaches 300°C, the As beam is turned off and the temperature is continued to cool to room temperature. When the vacuum in the growth chamber is less than 1×10 -9 After 0.040 ...

[0058] Example 2

[0059] The purpose of this embodiment is to achieve a high quality extended wavelength In with a cut-off wavelength of about 2300nm. 0.77 Ga 0.23 The effective preparation of As focal plane detector material. The InGaAs material structure with large overshoot and fast gradient shown in this embodiment is a common back-illuminated planar NIN structure, which includes the following materials from top to bottom:

[0060] 1.N-type In 0.77 Al 0.23 As fixed component contact layer, doped with Si, with a thickness of 600nm and a doping concentration of 1×10 16 cm -3 ;

[0061] 2.N-type In 0.77 Ga 0.23 As fixed component absorption layer, doped with Si, thickness 2500nm, doping concentration 1×10 15 cm -3 ;

[0062] 3.N-type In 0.77 Al 0.23 As fixed component buffer layer, doped with Si, thickness 200nm, doping concentration 5×10 17 cm -3 ;

[0063] 4. Unintentional doping with In z Al 1-z As large overshoot fast gradient linear buffer layer, the component z linearly changes from 0.52 to 0.85, the component gradient rate is 0.5 / h, the thickness is 1000nm, the concentration is 8×10 14 cm -3 ;

[0064] 5. Unintentional doping with In 0.52 Al 0.48 As lattice matching buffer layer, thickness 400nm, concentration 8×10 14 cm -3 ;

[0065] 6. Unintentionally doped InP homogeneous buffer layer, thickness 200nm, concentration 8×10 14 cm -3 .

[0066] This embodiment adopts molecular beam epitaxy technology for growth, and the growth process is as follows:

[0067] Preliminary experiments have determined that InP and InP can be grown on Fe-doped semi-insulating InP (001) at a growth rate of about 1 μm / h. 0.52 Al 0.48 As、In z Al 1-z As component z changes linearly from 0.52 to 0.85, In 0.77 Al 0.23 As and In 0.77 Ga 0.23 As, calibrate the temperature of each beam source furnace, and at the same time calibrate the growth temperature of each layer, V / III ratio and other conditions to determine In z Al 1-z The temperature and heating and cooling rates of the In furnace and Al furnace with the As component z linearly changing from 0.52 to 0.85 determine the N-type doping concentration of 1×10 15 cm -3 and 3×10 16 cm -3 The Si beam source furnace temperature;

[0068] A piece of Fe-doped semi-insulating InP (001) substrate was placed on the heater of the pretreatment chamber of the molecular beam epitaxy equipment, and the heating temperature was set to 400°C. After reaching the set temperature, it was maintained for 20 minutes to perform substrate pretreatment;

[0069] The pretreated semi-insulating InP (001) substrate was introduced into the growth chamber, and the sample holder temperature was set to 300 °C. When the set temperature was reached, the P beam was immediately turned on. At this time, the growth vacuum was 8×10 -8 Torr, continue to heat up to 600℃, and clear and bright 4×2 structure stripes can be seen. After standing for 5 minutes and fully deoxidizing, the above materials 6 to 1 are grown in sequence, and the material type, thickness and concentration of each layer are as described above;

[0070] The growth temperature of the InP homogeneous buffer layer is 550℃. 0.52 Al 0.48 The growth temperature of the As lattice matching buffer layer is 610℃, and the In z Al 1-z The growth temperature of the As large overshoot fast gradient linear buffer layer is 600℃, and the In 0.77 Al 0.23 The growth temperature of the As fixed composition buffer layer is 580℃, and the In 0.77 Ga 0.23 As fixed component absorption layer and In 0.77 Al 0.23The growth temperature of the As fixed component contact layer is 570°C;

[0071] After the epitaxial growth is completed, the sample holder is cooled to 300°C under the protection of As atmosphere. After the temperature reaches 300°C, the As beam is turned off and the temperature is continued to cool to room temperature. When the vacuum in the growth chamber is less than 1×10 -9 After 0.040 ...

[0072] Figure 2 The minority carrier lifetime test and fitting results of the extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown using existing technology.

[0073] The red line in the figure is the exponential fitting result, and the inset table is the corresponding fitting parameters. The minority carrier lifetime obtained by fitting is 85.04ns.

[0074] Figure 3 The minority carrier lifetime test and fitting results of an extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown based on a large overshoot fast-gradient InGaAs material structure of the present invention are presented.

[0075] The red line in the figure is the exponential fitting result, and the inset table is the corresponding fitting parameters. The minority carrier lifetime obtained by fitting is 329.9ns.

[0076] contrast Figure 2 and Figure 3 It can be seen from the fitting results of the minority carrier lifetime test that the InGaAs material structure based on large overshoot rapid gradient of the present invention can significantly improve the minority carrier lifetime of the extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm, which is conducive to obtaining higher device quantum efficiency.

[0077] Figure 4 Wafer warpage test and pseudo 3D mapping results of extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown using existing technology.

[0078] Figure 5 The present invention discloses wafer warpage test and pseudo 3D mapping results of an extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm grown based on a large overshoot fast-gradient InGaAs material structure.

[0079] The PV value in the figure is the difference between the calculated peak height and valley height, which can reflect the warpage of the wafer. Figure 4 and Figure 5It can be seen from the PV value results in that the InGaAs material structure based on large overshoot and rapid gradient of the present invention can significantly optimize the wafer warpage of the extended wavelength InGaAs focal plane detector material with a cutoff wavelength of 2300nm, which is conducive to obtaining a larger scale of extended wavelength InGaAs focal plane detector preparation.

[0080] Example 3

[0081] The purpose of this embodiment is to achieve a high quality extended wavelength In with a cut-off wavelength of about 2600nm. 0.85 Ga 0.15 The effective preparation of As focal plane detector material. The InGaAs material structure with large overshoot and fast gradient shown in this embodiment is a common back-illuminated planar NIN structure, which includes the following materials from top to bottom:

[0082] 1.N-type In 0.85 Al 0.15 As fixed component contact layer, doped with Si, with a thickness of 600nm and a doping concentration of 5×10 16 cm -3 ;

[0083] 2.N-type In 0.85 Ga 0.15 As fixed component absorption layer, doped with Si, thickness 2000nm, doping concentration 5×10 15 cm -3 ;

[0084] 3.N-type In 0.85 Al 0.15 As fixed component buffer layer, doped with Si, thickness 500nm, doping concentration 8×10 17 cm -3 ;

[0085] 4. N-type InAs fixed component relaxation layer, doped with Si, thickness 50nm, doping concentration 1×10 15 cm -3 ;

[0086] 5.N-type In z Al 1-z As large overshoot fast gradient linear buffer layer, the composition z linearly changes from 0.52 to 1, the composition gradient rate is 0.6 / h, Si is doped, the thickness is 300nm, and the concentration is 1×10 15 cm -3 ;

[0087] 6.N-type In 0.52 Al 0.48 As lattice matching buffer layer, doped with Si, 300 nm thick, with a concentration of 1×10 15 cm-3 ;

[0088] 7. N-type InP homogeneous buffer layer, doped with Si, thickness 100nm, concentration 1×10 15 cm -3 .

[0089] This embodiment adopts molecular beam epitaxy technology for growth, and the growth process is as follows:

[0090] Preliminary experiments have determined that InP and InP can be grown on Fe-doped semi-insulating InP (001) at a growth rate of about 1 μm / h. 0.52 Al 0.48 As、InAs、In 0.85 Al 0.15 As and In 0.85 Ga 0.15 As, calibrate the temperature of each beam source furnace, and at the same time calibrate the growth temperature of each layer, V / III ratio and other conditions to determine In z Al 1-z The temperature and heating and cooling rates of the In furnace and Al furnace where the As component z changes linearly from 0.52 to 1 determine the N-type doping concentration of 1×10 15 cm -3 , 5×10 15 cm -3 , 5×10 16 cm -3 and 8×10 17 cm -3 The Si beam source furnace temperature;

[0091] A piece of Fe-doped semi-insulating InP (001) substrate was placed on the heater of the pretreatment chamber of the molecular beam epitaxy equipment, and the heating temperature was set to 400°C. After reaching the set temperature, it was maintained for 20 minutes to perform substrate pretreatment;

[0092] The pretreated semi-insulating InP (001) substrate was introduced into the growth chamber, and the sample holder temperature was set to 300 °C. When the set temperature was reached, the P beam was immediately turned on. At this time, the growth vacuum was 8×10 -8 Torr, continue to heat up to 600℃, and clear and bright 4×2 structure stripes can be seen. After standing for 5 minutes and fully deoxidizing, the above materials 6 to 1 are grown in sequence, and the material type, thickness and concentration of each layer are as described above;

[0093] The growth temperature of the InP homogeneous buffer layer is 540℃. 0.52 Al 0.48 The growth temperature of the As lattice matching buffer layer is 600℃, and the In z Al 1-zThe growth temperature of the As large overshoot fast gradient linear buffer layer and the InAs fixed composition relaxation layer is 580℃. 0.85 Al 0.23 The growth temperature of the As fixed composition buffer layer is 560℃, and the In 0.77 Ga 0.23 As fixed component absorption layer and In 0.77 Al 0.23 The growth temperature of the As fixed component contact layer is 550°C;

[0094] After the epitaxial growth is completed, the sample holder is cooled to 300°C under the protection of As atmosphere. After the temperature reaches 300°C, the As beam is turned off and the temperature is continued to cool to room temperature. When the vacuum in the growth chamber is less than 1×10 -9 After 0.040 ...

Claims

1. A structure of InGaAs material based on large overshoot rapid gradient, the structure of which includes In w Al 1-w As fixed component contact layer (1), In x Ga 1-x As fixed component absorption layer (2), In w Al 1-w As fixed component buffer layer (3), In y Al 1- y As fixed component relaxation layer (4), In z Al 1-z As large overshoot fast gradient linear buffer layer (5), In 0.52 Al 0.48 As lattice matching buffer layer (6), InP homogeneous buffer layer (7), characterized by: In w Al 1-w The composition of the As fixed composition contact layer (1) is 0.52<w≤0.85, and the In x Ga 1-x The composition of the As fixed composition absorption layer (2) is 0.53<x≤0.85, and the In w Al 1-w The composition of the As fixed composition buffer layer (3) is 0.52<w≤0.85, and the In w Al 1-w As fixed component contact layer (1), In x Ga 1-x As fixed component absorption layer (2) and In w Al 1- w As fixed component buffer layer (3) has lattice matching among the three, the In y Al 1-y The composition of the As fixed composition relaxation layer (4) is w+0.05≤y≤1, and the In z Al 1-z As large overshoot rapid gradient linear buffer layer (5) from bottom to top composition linearly increases from 0.52 to y, the In z Al 1-z As is the composition change rate of the large overshoot fast-changing linear buffer layer (5), that is, In per hour z Al 1-z The amount of linear variation of component z in As is v, 0.4 / h≤v≤0.6 / h.

2. The InGaAs material structure based on large overshoot and rapid gradient according to claim 1, characterized in that: In w Al 1-w The thickness of the As fixed component contact layer (1) is 600-1000 nm, and the doping is N-type light doping with a doping concentration of 5×10 15 -5×10 16 cm -3 ; or doped with P-type heavy doping, with a doping concentration of 1×10 18 -5×10 18 cm -3 .

3. The InGaAs material structure based on large overshoot and rapid gradient according to claim 1, characterized in that: In x Ga 1-x The As fixed component absorption layer (2) has a thickness of 1600-2500 nm and is doped with N-type light doping at a doping concentration of 1×10 15 -5×10 16 cm -3 .

4. The InGaAs material structure based on large overshoot and rapid gradient according to claim 1, characterized in that: In w Al 1-w The As fixed component buffer layer (3) has a thickness of 200-1000 nm and is heavily doped with N-type doping at a doping concentration of 5×10 17 -5×10 18 cm -3 .

5. The InGaAs material structure based on large overshoot and rapid gradient according to claim 1, characterized in that: In y Al 1-y The As fixed component relaxation layer (4) has a thickness of 0-110 nm and is doped with N-type light doping at a doping concentration of 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 .

6. The InGaAs material structure based on large overshoot and fast gradient according to claim 1, characterized in that: In z Al 1-z The As large overshoot fast gradient linear buffer layer (5) has a thickness of 300-1000 nm and is doped with N-type light doping at a doping concentration of 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 .

7. The InGaAs material structure based on large overshoot and fast gradient according to claim 1, characterized in that: In 0.52 Al 0.48 The As lattice matching buffer layer (6) has a thickness of 200-400 nm and is doped with N-type light doping at a doping concentration of 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 .

8. The InGaAs material structure based on large overshoot and fast gradient according to claim 1, characterized in that: The thickness of the InP homogeneous buffer layer (7) is 40-200 nm, and the doping is N-type light doping with a doping concentration of 1×10 15 -5×10 16 cm -3 ; or unintentional doping, concentration <1×10 15 cm -3 .

9. A method for preparing an InGaAs material structure based on large overshoot and rapid gradient, characterized in that The following steps are involved: 1) using molecular beam epitaxy technology to grow the indium gallium arsenide material structure based on large overshoot rapid gradient, and placing the InP substrate in a pretreatment chamber for pretreatment; 2) The pre-treated InP substrate is introduced into the sample rack of the growth chamber for deoxidation treatment; 3) growing the InP homogeneous buffer layer (7) on the fully deoxidized InP substrate; 4) Growing the InP homogeneous buffer layer (7) 0.52 Al 0.48 As lattice matching buffer layer (6); 5) In the 0.52 Al 0.48 The In is grown on the As lattice matching buffer layer (6) z Al 1-z As large overshoot fast gradient linear buffer layer (5), by increasing the In furnace temperature by the same amount and reducing the Al furnace temperature by twice the amount to achieve a fast linear gradient of composition; 6) In the z Al 1-z As large overshoot fast gradient linear buffer layer (5) grows the In y Al 1-y As fixed component relaxation layer (4); 7) In the y Al 1-y The In is grown on the As fixed component relaxation layer (4). w Al 1-w As fixed component buffer layer (3); 8) In the w Al 1-w The In is grown on the As fixed component buffer layer (3) x Ga 1-x As fixed component absorption layer (2); 9) In the x Ga 1-x The In is grown on the As fixed component absorption layer (2) w Al 1-w As fixed component contact layer (1); 10) In the w Al 1-w After the growth of the As fixed component contact layer (1) is completed, the sample holder is cooled to 300° C. under the protection of As atmosphere, the As protection is turned off, and the sample holder is taken out after cooling to room temperature to complete the growth.

Citation Information

Cited By

  • Molecular beam epitaxy variable component epitaxy process optimization method

    CN122649083A