End welding method for copper rotating target material

Through two-pass friction stir welding and mechanical processing, the problem of insufficient welding reliability and hardness of copper rotary target ends is solved, and the welding bonding performance and sealing performance are significantly improved, and the welding process in the prior art is solved. Cracking and tearing defects and insufficient hardness.

CN118875459APending Publication Date: 2024-11-01KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411221996.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing end welding methods of copper rotary targets have problems such as low welding reliability, insufficient hardness, easy tilt and eccentricity, and reduced welding bonding effect of electric glue layers. In addition, high-purity copper rotary targets need to maintain concentricity during welding, resulting in Rewelding and utilization reduction.

Method used

Using two-pass friction stir welding treatment, select high-purity copper flanges and tube caps, and gradually increase welding depth and rotation speed through the first and second welding, combining mechanical processing and cooling to ensure the stability of the welding joint and Sealing performance.

Benefits of technology

Effectively remove welding cracks and tear defects, improve the welding bonding and sealing performance of copper rotary targets, meet industrial requirements, and ensure flange hardness and welding reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875459A_ABST
    Figure CN118875459A_ABST
Patent Text Reader

Abstract

The invention provides an end welding method for a copper rotating target material, which comprises the following steps: (1) respectively assembling two ends of a copper target material pipe body with a flange and a pipe cap to obtain a copper target material pipe with a welding joint part; and (2) the welding joint part in the step (1) is subjected to friction stir welding, then cooling and machining are sequentially conducted, and the copper rotating target material is obtained. The friction stir welding comprises first welding and second welding which are sequentially carried out. According to the end welding method for the copper rotating target material, through two-pass friction stir welding, the welding defects such as cracks and tearing in the welding process can be effectively removed, the welding combination performance and the welding reliability of the welding combination parts of the copper target material pipe body and the flanges and the pipe caps at the two ends in the obtained copper rotating target material are excellent, and the welding quality is improved. And the sealing performance is obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of target material welding, and in particular relates to an end welding method of a copper rotating target material. Background Art

[0002] With the development and progress of thin film products or component preparation technology used in TFT display technology, in order to meet the market demand for large-size panels above 8.5 generation lines, new manufacturing technology for copper metal targets for wiring layers has emerged. The copper targets required for large-size panels are divided into two categories: planar targets and rotary targets. In contrast, rotary targets are in a leading position in terms of corresponding panel size and effective utilization rate, so the development of rotary targets is of great significance to panel size and metal resource utilization rate.

[0003] Although there are related products on the market for copper rotating targets, this type of product is generally an integrated rotating target, that is, the flange (installation position) is machined from the tube blank material. However, due to the need to ensure the grain and cutting performance, the hardness of the tube blank material cannot be made too high, about 60 to 90HV. The flange (installation position) machined from this material is relatively soft in hardness and will gradually tilt and eccentric during use, resulting in product scrapping or even machine damage. Selecting a copper alloy with higher hardness as the flange material is an effective solution, but how to reliably and effectively weld the copper alloy and the tube body, which are dissimilar materials, has become a practical problem and difficulty that plagues and restricts the manufacturing of copper rotating target products.

[0004] CN 218203024U discloses an integrated rotating target material that is easy to connect with an end head, wherein the integrated rotating target material that is easy to connect with the end head is provided with a conductive adhesive layer on the end surface connected with the end head, and is used for connecting the integrated rotating target material that is easy to connect with the end head with the end head. The utility model connects the integrated rotating target material with the end head by providing a conductive adhesive layer, which is simple to operate and saves equipment and labor costs, but the conductive adhesive layer will reduce the effect of welding after long-term use.

[0005] CN 109807453A discloses a terminal welding method for a high-purity copper rotary target, wherein the terminal welding method is divided into three steps to weld the terminal welding port or the tail cover welding port, wherein the first step is spot welding, the second step is arc welding, and the third step is circumferential welding. During the welding process of the high-purity copper rotary target, the target material needs to maintain a high concentricity with the terminal and the tail cover. If displacement occurs during the welding process, re-welding is required, resulting in a waste of time. Moreover, the utilization rate of the terminal and the tail cover is reduced by connecting the terminal and the tail cover to the rotary target material by welding.

[0006] Therefore, in view of the shortcomings of the prior art, it is urgently necessary to provide a method for welding the end of a copper rotating target with high welding reliability. Summary of the invention

[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for welding the end of a copper rotating target. The present invention reasonably selects the materials of the flange and the pipe cap and adopts two-pass stir friction welding treatment. The obtained copper rotating target has excellent welding bonding performance, no defects such as cracks and tears, and the flange hardness of the copper rotating target is high, which can meet industrial requirements.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for welding an end of a copper rotating target, the method comprising the following steps:

[0010] (1) Assembling the two ends of the copper target tube body with flanges and tube caps respectively to obtain a copper target tube with a welded joint;

[0011] (2) performing friction stir welding on the welded joint in step (1), followed by cooling and machining in sequence to obtain the copper rotary target;

[0012] The friction stir welding includes a first welding and a second welding which are performed sequentially.

[0013] The end welding method of the copper rotating target provided by the present invention can effectively remove welding defects such as cracks and tears in the welding process through two-pass stir friction welding. The welding joints between the copper target tube body and the flanges and tube caps at both ends in the obtained copper rotating target have excellent welding bonding performance and welding reliability. Compared with one-pass welding, the sealing performance can be significantly improved.

[0014] As a preferred technical solution of the present invention, the copper target tube body is a high-purity copper target tube body;

[0015] Preferably, the tube cap is a high-purity copper tube cap.

[0016] In the present invention, the material of the copper target tube body and the tube cap are both high-purity copper, and the friction stir welding bonding performance of the copper target tube body and the tube cap of the same material is better and the bonding rate is higher.

[0017] As a preferred technical solution of the present invention, the material of the flange includes copper alloy.

[0018] Preferably, the hardness of the copper alloy is ≥100 HV, for example, it may be 100 HV, 110 HV, 120 HV, 130 HV, 140 HV or 150 HV, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the grade of the copper alloy includes any one of C18000, C18200 or C46400.

[0020] As a preferred technical solution of the present invention, the diameter of the welding port of the copper target tube body in step (1) is the same as the diameter of the welding port of the flange.

[0021] It is worth noting that the diameter of the welding port of the copper target tube body described in the present invention is kept the same as the diameter of the welding port of the flange, which is beneficial to maintaining the stability of rotation during the subsequent stir friction welding process.

[0022] As a preferred technical solution of the present invention, the friction stir welding in step (2) includes: performing cutting welding along the circumference of the edge of the assembly process.

[0023] As a preferred technical solution of the present invention, the stirring head depth of the first welding is 0.5-1.5 mm, for example, it can be 0.5 mm, 0.7 mm, 0.9 mm, 1.1 mm, 1.3 mm or 1.5 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] Preferably, the stirring head speed of the first welding is 900-1200 r / min, for example, it can be 900 r / min, 1000 r / min, 1100 r / min or 1200 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, the feed speed of the first welding is 48-52 mm / min, for example, it can be 48 mm / min, 49 mm / min, 50 mm / min, 51 mm / min or 52 mm / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the pressing amount of the stirring head of the first welding is 0.45-0.55 mm, for example, it can be 0.45 mm, 0.47 mm, 0.49 mm, 0.51 mm, 0.53 mm or 0.55 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] As a preferred technical solution of the present invention, the stirring head depth of the second welding is 2.5-4.5 mm, for example, it can be 2.5 mm, 2.7 mm, 2.9 mm, 3.1 mm, 3.3 mm, 3.5 mm, 3.7 mm, 3.9 mm, 4.1 mm, 4.3 mm or 4.5 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the stirring head speed of the second welding is 1000-1400r / min, for example, it can be 1000r / min, 1100r / min, 1200r / min, 1300r / min or 1400r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the feed speed of the second welding is 48-52 mm / min, for example, it can be 48 mm / min, 49 mm / min, 50 mm / min, 51 mm / min or 52 mm / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the pressing amount of the stirring head of the second welding is 0.45-0.55 mm, for example, it can be 0.45 mm, 0.47 mm, 0.49 mm, 0.51 mm, 0.53 mm or 0.55 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] The present invention can increase the welding depth gradually by selecting stirring heads with increasing depths in the first welding and the second welding and limiting the stirring head rotation speed to increase successively, thereby avoiding the bottom tearing defect caused by one-time excessive welding depth or excessive rotation speed.

[0032] As a preferred technical solution of the present invention, the cooling in step (2) includes: air cooling to 20-30°C, for example, it can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the cooling in step (2) is carried out on a welding table.

[0034] Preferably, step (2) further includes a sealing test after cooling.

[0035] Preferably, the sealing detection is: using a helium leakage device to detect the sealing performance of the copper rotary target after welding.

[0036] As a preferred technical solution of the present invention, the mechanical processing in step (2) includes outer cylindrical turning, length turning and polishing in sequence.

[0037] Preferably, the tools used for the external cylindrical turning and length turning include carbide tools or high-speed steel tools.

[0038] Preferably, the polishing process comprises polishing with sandpaper and scouring pad in sequence.

[0039] The present invention does not limit the process parameters of external cylindrical turning and length turning in mechanical processing, as long as the required size can be obtained by processing.

[0040] As a preferred technical solution of the present invention, the end welding method of the copper rotating target provided by the present invention comprises the following steps:

[0041] (1) Assembling the two ends of the high-purity copper target tube body with flanges and high-purity copper tube caps respectively to obtain a copper target tube with a welded joint;

[0042] Wherein, the material of the flange includes a copper alloy with a hardness of ≥100 HV; the diameter of the welding port of the copper target tube body is the same as the diameter of the welding port of the flange;

[0043] (2) performing friction stir welding on the welded joint of step (1), followed by air cooling to 20-30° C., sealing testing and mechanical processing to obtain the copper rotary target;

[0044] Wherein, the friction stir welding includes: performing cutting welding along the circumference of the edge of the assembly process; the friction stir welding includes a first welding and a second welding performed in sequence; the stirring head depth of the first welding is 0.5-1.5mm, the stirring head speed is 900-1200r / min, the feed speed is 48-52mm / min, and the stirring head pressure is 0.45-0.55mm; the stirring head depth of the second welding is 2.5-4.5mm, the stirring head speed is 1000-1400r / min, the feed speed is 48-52mm / min, and the stirring head pressure is 0.45-0.55mm;

[0045] The mechanical processing includes outer circle turning, length turning and polishing with sandpaper and scouring pad in sequence.

[0046] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] (1) The end welding method of the copper rotating target provided by the present invention can effectively remove welding defects such as cracks and tears during the welding process by reasonably selecting the materials of the flange and the pipe cap and using two-pass stir friction welding treatment;

[0049] (2) The copper rotating target material obtained by the end welding method provided by the present invention has excellent welding bonding performance, no defects such as cracks and tears, and excellent sealing performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 It is a schematic diagram of the assembly of the copper target tube body and the flange provided in Example 1 of the present invention;

[0051] Figure 2 Schematic diagram of the assembly of the copper target tube body and the tube cap provided in Example 1 of the present invention

[0052] Figure 3 is a schematic structural diagram of a copper rotary target provided in Example 1 of the present invention;

[0053] Among them, 1 is the copper target tube body, 2 is the flange, 3 is the tube cap, and 4 is the welding joint. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0055] Example 1

[0056] This embodiment provides a method for welding the end of a copper rotating target, and the method comprises the following steps:

[0057] (1) The two ends of the high-purity copper target tube body 1 are assembled with the flange 2 and the high-purity copper tube cap 3 respectively, as shown in FIG. Figure 1 and Figure 2 As shown, a copper target tube having a welding joint 4 is obtained;

[0058] The material of the flange 2 includes a C18000 copper alloy with a hardness of 210 HV; the diameter of the welding port of the copper target tube body 1 is the same as the diameter of the welding port of the flange 2;

[0059] (2) Stir friction welding is performed on the welded joint 4 in step (1), followed by air cooling to 25° C., sealing test and mechanical processing, to obtain the following Figure 3 The copper rotary target shown;

[0060] The friction stir welding includes: performing cutting welding along the circumference of the edge of the assembly process; the friction stir welding includes a first welding and a second welding performed in sequence; the stirring head depth of the first welding is 1.5 mm, the stirring head speed is 1150 r / min, the feed speed is 50 mm / min, and the stirring head pressure is 0.5 mm; the stirring head depth of the second welding is 4.5 mm, the stirring head speed is 1200 r / min, the feed speed is 50 mm / min, and the stirring head pressure is 0.5 mm;

[0061] The mechanical processing includes outer circle turning, length turning and polishing with sandpaper and scouring pad in sequence.

[0062] Example 2

[0063] This embodiment provides a method for welding the end of a copper rotating target, and the method comprises the following steps:

[0064] (1) Assembling the two ends of a high-purity copper target tube body 1 with a flange 2 and a high-purity copper tube cap 3 respectively to obtain a copper target tube having a welded joint 4;

[0065] The material of the flange 2 includes C46400 copper alloy with a hardness of 120 HV; the diameter of the welding port of the copper target tube body 1 is the same as the diameter of the welding port of the flange 2;

[0066] (2) performing friction stir welding on the welded joint of step (1), followed by air cooling to 20° C., sealing testing and mechanical processing to obtain the copper rotary target;

[0067] The friction stir welding comprises: performing cutting welding along the circumference of the edge of the assembly process; the friction stir welding comprises a first welding and a second welding performed in sequence; the stirring head depth of the first welding is 0.5 mm, the stirring head speed is 900 r / min, the feed speed is 48 mm / min, and the stirring head pressure is 0.45 mm; the stirring head depth of the second welding is 2.5 mm, the stirring head speed is 1000 r / min, the feed speed is 48 mm / min, and the stirring head pressure is 0.45 mm;

[0068] The mechanical processing includes outer circle turning, length turning and polishing with sandpaper and scouring pad in sequence.

[0069] Example 3

[0070] This embodiment provides a method for welding the end of a copper rotating target, and the method comprises the following steps:

[0071] (1) Assembling the two ends of a high-purity copper target tube body 1 with a flange 2 and a high-purity copper tube cap 3 respectively to obtain a copper target tube having a welded joint 4;

[0072] The material of the flange 2 includes C18200 copper alloy with a hardness of 160 HV; the diameter of the welding port of the copper target tube body 1 is the same as the diameter of the welding port of the flange 2;

[0073] (2) performing friction stir welding on the welded joint of step (1), followed by air cooling to 20-30° C., sealing testing and mechanical processing to obtain the copper rotary target;

[0074] The friction stir welding comprises: performing cutting welding along the circumference of the edge of the assembly process; the friction stir welding comprises a first welding and a second welding performed in sequence; the stirring head depth of the first welding is 1.5 mm, the stirring head speed is 1200 r / min, the feed speed is 52 mm / min, and the stirring head pressure is 0.55 mm; the stirring head depth of the second welding is 4.5 mm, the stirring head speed is 1400 r / min, the feed speed is 52 mm / min, and the stirring head pressure is 0.55 mm;

[0075] The mechanical processing includes outer circle turning, length turning and polishing with sandpaper and scouring pad in sequence.

[0076] Example 4

[0077] This embodiment provides a method for welding the end of a copper rotating target. The difference between the end welding method and the embodiment 1 is that:

[0078] In this embodiment, the hardness of the flange is adjusted to 80 HV.

[0079] Example 5

[0080] This embodiment provides a method for welding the end of a copper rotating target. The difference between the end welding method and the embodiment 1 is that:

[0081] In this embodiment, the stirring head depth of the first welding and the second welding in step (2) is adjusted to 5 mm.

[0082] Example 6

[0083] This embodiment provides a method for welding the end of a copper rotating target. The difference between the end welding method and the embodiment 1 is that:

[0084] In this embodiment, the rotation speeds of the stirring heads for the first welding and the second welding in step (2) are both adjusted to 1400 r / min.

[0085] Example 7

[0086] This embodiment provides a method for welding the end of a copper rotating target. The difference between the end welding method and the embodiment 1 is that:

[0087] In this embodiment, the feed speeds of the first welding and the second welding are both adjusted to 45 mm / min.

[0088] Example 8

[0089] This embodiment provides a method for welding the end of a copper rotating target. The difference between the end welding method and the embodiment 1 is that:

[0090] In this embodiment, the feed speeds of the first welding and the second welding are both adjusted to 55 mm / min.

[0091] Comparative Example 1

[0092] This comparative example provides a method for welding the end of a copper rotating target. The difference between the end welding method and Example 1 is that:

[0093] The second welding process was omitted in this comparative example.

[0094] Comparative Example 2

[0095] This comparative example provides a method for welding the end of a copper rotating target. The difference between the end welding method and Example 1 is that:

[0096] In this comparative example, a third welding is added after the second welding. The stirring head depth of the third welding is 6 mm, the stirring head rotation speed is 1500 r / min, the feed speed is 50 mm / min, and the downward pressure is 0.5 mm.

[0097] According to the end welding method provided in the above embodiment and comparative example, the sealing performance of the copper rotating target after friction stir welding was tested by using a helium leakage device, and the appearance of the welded joint was visually observed. The results are shown in Table 1.

[0098] Among them, the gas leakage conditions of the sealing performance test are divided into "leakage" and "no leakage"; the visual observation results of the appearance of the welding joint are divided into "no cracks", "shallow cracks", "deep cracks" and "bottom tearing".

[0099] Table 1

[0100]

[0101]

[0102] Table 1 shows the following points:

[0103] (1) Comprehensive analysis of Examples 1-3 shows that when the end welding method provided by the present invention is adopted, the sealing effect of the welded joint is excellent, the welded joint performance is excellent, and there is no crack defect;

[0104] (2) Comprehensive analysis of Example 1 and Example 4 shows that when the flange hardness is too low, its deformation resistance is poor and cracks are easily generated during the welding process, resulting in a decrease in the sealing effect;

[0105] (3) Comprehensive analysis of Example 1 and Examples 5 and 6 shows that using the same stirring head depth or stirring head speed during the friction stir welding process will reduce the welding effect of the welded joint, resulting in cracks and affecting the sealing effect;

[0106] (4) Comprehensive analysis of Example 1 and Examples 7-8 shows that the feed speed of the first welding and the second welding is too high or too low, which will have an adverse effect on the welding performance;

[0107] (5) Comprehensive analysis of Example 1 and Comparative Example 1 shows that only one pass of friction stir welding cannot obtain a welded joint with good sealing performance, and a bottom tearing defect will occur;

[0108] (6) Comprehensive analysis of Example 1 and Comparative Example 2 shows that adding a stir friction welding step will lead to softening of the structure in the welding area, low joint strength, and the risk of deformation and cracks in the welding area during use.

[0109] In summary, the end welding method of the copper rotating target provided by the present invention can effectively remove welding defects such as cracks and tears in the welding process through two passes of stir friction welding. The welding joints between the copper target tube body and the flanges and pipe caps at both ends in the obtained copper rotating target have excellent welding bonding performance and welding reliability, and the sealing performance is significantly improved.

[0110] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for welding the end of a copper rotating target, characterized in that: The end welding method comprises the following steps: (1) Assembling the two ends of the copper target tube body with flanges and tube caps respectively to obtain a copper target tube with a welded joint; (2) performing friction stir welding on the welded joint described in step (1), followed by cooling and machining in sequence to obtain the rotating copper target; The friction stir welding includes a first welding and a second welding which are performed sequentially.

2. The end welding method of the copper rotating target according to claim 1, characterized in that: The copper target material tube body is a high-purity copper target material tube body; Preferably, the tube cap is a high-purity copper tube cap.

3. The end welding method of the copper rotating target according to claim 1 or 2, characterized in that: The material of the flange includes copper alloy; Preferably, the hardness of the copper alloy is ≥100 HV; Preferably, the grade of the copper alloy includes any one of C18000, C18200 or C46400.

4. The end welding method of the copper rotating target according to any one of claims 1 to 3, characterized in that: The diameter of the welding port of the copper target tube body in step (1) is the same as the diameter of the welding port of the flange.

5. The end welding method of the copper rotating target according to any one of claims 1 to 4, characterized in that: The friction stir welding in step (2) includes: performing cutting welding along the circumference of the edge of the assembly process.

6. The end welding method of the copper rotating target according to any one of claims 1 to 5, characterized in that: The stirring head depth of the first welding is 0.5 to 1.5 mm; Preferably, the rotation speed of the stirring head of the first welding is 900-1200 r / min; Preferably, the feed speed of the first welding is 48-52 mm / min; Preferably, the downward pressure of the stirring head of the first welding is 0.45-0.55 mm.

7. The end welding method of the copper rotating target according to any one of claims 1 to 6, characterized in that: The stirring head depth of the second welding is 2.5 to 4.5 mm; Preferably, the rotation speed of the stirring head of the second welding is 1000-1400 r / min; Preferably, the feed speed of the second welding is 48-52 mm / min; Preferably, the pressing amount of the stirring head of the second welding is 0.45-0.55 mm.

8. The end welding method of the copper rotating target according to any one of claims 1 to 7, characterized in that: The cooling in step (2) comprises: air cooling to 20-30° C.; Preferably, step (2) further includes a sealing test after cooling.

9. The end welding method of the copper rotating target according to any one of claims 1 to 8, characterized in that: The mechanical processing in step (2) includes outer cylindrical turning, length turning and polishing in sequence; Preferably, the tools used for the external turning and length turning include carbide tools or high-speed steel tools; Preferably, the polishing process comprises polishing with sandpaper and scouring pad in sequence.

10. The end welding method of a copper rotating target according to any one of claims 1 to 9, characterized in that: The end welding method comprises the following steps: (1) Assembling the two ends of the high-purity copper target tube body with flanges and high-purity copper tube caps respectively to obtain a copper target tube with a welded joint; Wherein, the material of the flange includes a copper alloy with a hardness of ≥100 HV; the diameter of the welding port of the copper target tube body is the same as the diameter of the welding port of the flange; (2) performing friction stir welding on the welded joint of step (1), followed by air cooling to 20-30° C., sealing testing and mechanical processing to obtain the copper rotary target; Wherein, the friction stir welding includes: performing cutting welding along the circumference of the edge of the assembly process; the friction stir welding includes a first welding and a second welding performed in sequence; the stirring head depth of the first welding is 0.5-1.5mm, the stirring head speed is 900-1200r / min, the feed speed is 48-52mm / min, and the stirring head pressure is 0.45-0.55mm; the stirring head depth of the second welding is 2.5-4.5mm, the stirring head speed is 1000-1400r / min, the feed speed is 48-52mm / min, and the stirring head pressure is 0.45-0.55mm; The mechanical processing includes outer circle turning, length turning and polishing with sandpaper and scouring pad in sequence.