Soluble aluminum alloy preparation method and soluble aluminum alloy
Through the ball milling, blanking, extrusion and solution quenching process of aluminum-lithium alloy waste, combined with specific element ratios and process parameters, the problem of difficult to take into account both the mechanical properties and the dissolution rate of soluble aluminum alloys is prepared, and excellent mechanical properties are prepared and soluble aluminum alloys with high dissolution rate meet the high strength and high solubility requirements of downhole tool bridge plugs.
Patent Information
- Application Number
- CN202410998918.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-01
AI Technical Summary
The existing soluble aluminum alloy materials are difficult to balance between mechanical properties and dissolution rate, and the preparation process is complex, which cannot meet the high strength and high solubility requirements of downhole tool bridge plugs.
Aluminum-lithium alloy waste is used as raw material, and is prepared through ball milling, blanking, extrusion and solution quenching processes. The ratios and process parameters of Cu, Li, Mg, Zr, Ag are controlled to form fine discontinuous oxidizing substances that are diffuse lithium particles. , improve mechanical properties and dissolution rate.
The prepared soluble aluminum alloy has tensile strength greater than 580MPa, yield strength greater than 530MPa, elongation greater than 12%, and dissolution rate greater than 4.0g/h. It meets the high strength and high solubility requirements of the bridge plug, and the process is simple and stable. Suitable for large-scale processing.
Smart Images

Figure CN118880089A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of soluble aluminum alloy preparation, and specifically to a soluble aluminum alloy preparation method and the soluble aluminum alloy. Background Art
[0002] Soluble aluminum alloy is the main material of downhole tool bridge plugs at present. Soluble aluminum alloy is mainly used in drilling and completion tools and staged fracturing processes, forming a variety of tools such as soluble fracturing balls, soluble fracturing ball seats, soluble fracturing bridge plugs, and soluble blind plates, which solves the problems of the ball being unable to be discharged, small production diameter, and the need for drilling plugs after fracturing during the current staged fracturing technology application process. Using soluble aluminum alloy to make drilling and completion tools can simplify the drilling and completion construction process, reduce drilling and completion costs, save completion time, and maintain a large casing diameter, which is convenient for the later transformation of oil and gas wells.
[0003] Existing soluble aluminum alloy materials generally add low-melting point elements such as Ga, In, and Sn, which have a good dissolution rate. However, with the increasing complexity of oilfield mining conditions, higher requirements are placed on the mechanical properties of bridge plugs, requiring them to have higher strength and a corresponding dissolution rate. In recent years, studies have been conducted to improve the comprehensive properties of soluble aluminum alloys by adding low-melting point elements and strengthening elements to the alloy. However, low-melting point alloying elements are often enriched or unevenly distributed at the grain boundaries, resulting in a decrease in the mechanical properties of the alloy, such as strength and plasticity. Although the addition of strengthening elements improves the mechanical properties of the alloy, it significantly reduces the solubility of the alloy and even causes passivation. The Chinese patent with application number 201910645705.1 discloses an ultra-high-strength aluminum-lithium alloy and a preparation method thereof, which weighs each component according to the designed aluminum alloy component ratio, and uses atmospheric smelting or vacuum smelting to cast an ingot, and then undergoes multi-stage homogenization treatment, hot extrusion deformation, gradual temperature increase solid solution, cold rolling deformation, and aging treatment. The aluminum-lithium alloy product prepared has the characteristics of high strength, but the product prepared by this preparation method is not soluble. Therefore, after adding low melting point elements and strengthening elements to the alloy, the performance of the alloy is mutually restricted, and it is impossible to take into account both mechanical properties and solubility. In addition, the preparation process is complicated, which is still an urgent problem to be solved for soluble aluminum alloys. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a method for preparing a soluble aluminum alloy and a soluble aluminum alloy, which uses aluminum-lithium alloy waste as raw materials to prepare the aluminum-lithium alloy, so as to solve the problem in the prior art that the mechanical properties and dissolution rate of the soluble aluminum alloy cannot be taken into account at the same time and the preparation process is complicated.
[0005] The technical problem solved by the present invention is achieved by adopting the following technical solutions:
[0006] A method for preparing a soluble aluminum alloy comprises the following steps:
[0007] 1) Material selection: Al-Cu-Li aluminum-lithium alloy waste is selected as raw material;
[0008] 2) Ball milling: The raw materials are ball milled, an inert gas is introduced during the ball milling, the ball milling speed is 180-350r / min, and the ball milling time is 30-90min;
[0009] 3) Pressing treatment: the raw material powder obtained after ball milling is pressed into a green sheet at a pressing pressure of 200-300 MPa and a holding time of 5-20 min;
[0010] 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 440-480°C and kept warm for 4-8 hours, and then extruded with an extrusion ratio of 8-20 and an extrusion rate of 0.2-1 mm / s;
[0011] 5) Solution quenching: The extruded material after the extrusion treatment is subjected to solution quenching, and then aging treatment is performed after the solution quenching is completed.
[0012] Furthermore, in step 1), the Al-Cu-Li aluminum-lithium alloy waste has a Cu content of 3.2-4.2%, a Li content of 0.5-1.2%, a Mg content of 0.4-1.2%, a Zr content of 0.08-0.2%, an Ag content of 0.3-0.8%, and the remainder is impurities. The selection of the raw materials is critical. If the ratio of lithium to other components is not properly controlled, the dissolution rate will be significantly reduced.
[0013] Furthermore, in step 2), the mass ratio of the raw material to the grinding ball is 1:3-8, and the diameter of the grinding ball is 5-12 mm. If the setting is improper, the oxide film formed by the waste material cannot be fully broken, thereby affecting the performance and dissolution rate.
[0014] Furthermore, in step 2), the inert gas is argon or nitrogen. The presence of the inert gas is to prevent oxidation of the newly generated cross section during the ball milling process, and to prevent the resulting elongation difference and reduced dissolution rate.
[0015] Furthermore, in step 3), a cold isostatic press is used for compacting. The cold isostatic press is conducive to forming the powder after ball milling, which is convenient for subsequent extrusion.
[0016] Furthermore, in step 5), after extrusion is completed, the extruded material is subjected to solution quenching, the solution temperature is 500-520° C., and the temperature is kept for 2-4 hours. After the solution is completed, the extruded material is immediately quenched.
[0017] Furthermore, in step 5), the quenching medium is water, the water temperature is controlled at 15-30° C., and the quenching transfer time does not exceed 15 s.
[0018] Furthermore, in step 5), the aging system is 150-170° C. and the temperature is kept at 15-36 hours.
[0019] A soluble aluminum alloy is prepared by any of the above methods.
[0020] Furthermore, the soluble aluminum alloy has a tensile strength greater than 580 MPa, a yield strength greater than 530 MPa, an elongation greater than 12%, and a dissolution rate greater than 4.0 g / h.
[0021] Beneficial effect: Aluminum-lithium alloy debris is severely oxidized due to the activity of lithium, which makes the purification and reuse process complicated. The soluble aluminum alloy preparation method described in the present invention uses aluminum-lithium alloy waste as raw material, fully utilizes the high activity of lithium in the raw material, combines the characteristics of aluminum-lithium alloy waste and soluble aluminum alloy, and combines specific ball milling, billet pressing and extrusion, and solution quenching processes to form fine non-continuous oxidized material points diffused with lithium particles, thereby providing a continuous dissolution channel for soluble aluminum alloys, so that the final product has better mechanical properties and excellent dissolution rate, solving the problem that the currently mainly used soluble aluminum alloy system is difficult to improve strength or it is difficult to balance strength improvement and solubility; thereby better meeting the working conditions of bridge plugs.
[0022] The method for preparing the soluble aluminum alloy of the present invention has simple preparation process, easy control of nodes, stable products and is suitable for large-scale processing applications.
[0023] The soluble aluminum alloy prepared by the present invention has a tensile strength greater than 580 MPa, a yield strength greater than 530 MPa, an elongation greater than 12%, and a dissolution rate greater than 4.0 g / h, and has both good mechanical properties and excellent dissolution properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the microstructure diagram of the aluminum alloy in Example 1.
[0025] Figure 2 This is the microstructure diagram of the aluminum alloy in Example 2.
[0026] Figure 3 This is the microstructure diagram of the aluminum alloy in Control Example 2. DETAILED DESCRIPTION
[0027] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0028] Example 1
[0029] The method for preparing the soluble aluminum alloy described in this embodiment comprises the following steps:
[0030] 1) Material selection: Al-Cu-Li aluminum-lithium alloy waste is selected as the raw material; the raw material composition is 3.9% Cu, 0.9% Li, 0.7% Mg, 0.12% Zr, 0.35% Ag, and the balance is Al and impurities; the raw material type is the debris after sawing and turning;
[0031] 2) Ball milling: The raw materials were placed in a ball mill for ball milling. Argon gas was introduced for protection during ball milling. The mass ratio of raw materials to grinding balls was 1:4. The diameter of the grinding balls was 10 mm. The ball milling speed was 280 r / min and the ball milling time was 60 min.
[0032] 3) Pressing treatment: the raw material powder obtained after ball milling is loaded into a rubber mold and pressed by a cold isostatic press with a pressing pressure of 240 MPa and a holding time of 15 min;
[0033] 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 460°C and kept at this temperature for 6 hours, and then subjected to extrusion treatment, with an extrusion ratio of 12 and an extrusion rate of 0.41 mm / s;
[0034] 5) Solution quenching: The extruded material after extrusion treatment is subjected to solution quenching at a temperature of 510°C and kept at this temperature for 3 hours. After solution quenching, the material is immediately quenched. The quenching medium is water and the water temperature is controlled at 20°C. The quenching transfer time does not exceed 15 seconds. After solution quenching, aging is performed at a temperature of 160°C and kept at this temperature for 26 hours.
[0035] The prepared aluminum alloy material is shown in Figure Figure 1 As shown, it can be seen that the second phase in the aluminum matrix is dispersed and can better meet the performance and solubility requirements.
[0036] Example 2
[0037] The method for preparing the soluble aluminum alloy described in this embodiment comprises the following steps:
[0038] 1) Material selection: Al-Cu-Li aluminum-lithium alloy scrap is selected as the raw material; the raw material composition is 3.5% Cu, 1.1% Li, 0.9% Mg, 0.11% Zr, 0.31% Ag, and the balance is Al and impurities; the raw material type is sawing and turning debris.
[0039] 2) Ball milling: The raw materials were placed in a ball mill for ball milling. Argon gas was introduced for protection during ball milling. The mass ratio of the raw materials to the grinding balls was 1:5. The diameter of the grinding balls was 8 mm. The ball milling speed was 300 r / min and the ball milling time was 80 min.
[0040] 3) Pressing treatment: the raw material powder obtained after ball milling is loaded into a rubber mold and pressed by a cold isostatic press with a pressing pressure of 240 MPa and a holding time of 15 min;
[0041] 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 460°C and kept at this temperature for 6 hours, and then extruded with an extrusion ratio of 12 and an extrusion rate of 0.4 mm / s;
[0042] 5) Solution quenching: The extruded material after extrusion treatment is subjected to solution quenching at 510°C and kept at this temperature for 3 hours. After solution quenching, the material is immediately quenched. The quenching medium is water and the water temperature is controlled at 30°C. The quenching transfer time does not exceed 15s. After solution quenching, aging is carried out at 155°C and kept at this temperature for 32 hours.
[0043] The prepared aluminum alloy material is shown in Figure Figure 2 As shown, it can be seen that the second phase in the aluminum matrix is dispersed and can better meet the performance and solubility requirements.
[0044] Comparative Example 1
[0045] The method for preparing the soluble aluminum alloy in this comparative example has unreasonable configuration of the content of each element in the raw material, and specifically includes the following steps:
[0046] 1) Material selection: Al-Cu-Li aluminum-lithium alloy scrap is selected as the raw material; the raw material composition is 3.9% Cu, 0.3% Li, 0.7% Mg, 0.12% Zr, 0.35% Ag, and the balance is Al and impurities; the raw material type is the debris after sawing and turning;
[0047] 2) Ball milling: The raw materials were placed in a ball mill for ball milling. Argon gas was introduced for protection during ball milling. The mass ratio of raw materials to grinding balls was 1:4. The diameter of the grinding balls was 10 mm. The ball milling speed was 280 r / min and the ball milling time was 60 min.
[0048] 3) Pressing treatment: the raw material powder obtained after ball milling is loaded into a rubber mold and pressed by a cold isostatic press with a pressing pressure of 240 MPa and a holding time of 15 min;
[0049] 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 460°C and kept at this temperature for 6 hours, and then subjected to extrusion treatment, with an extrusion ratio of 12 and an extrusion rate of 0.41 mm / s;
[0050] 5) Solution quenching: The extruded material after extrusion treatment is subjected to solution quenching at a temperature of 510°C and kept at this temperature for 3 hours. After solution quenching, the material is immediately quenched. The quenching medium is water and the water temperature is controlled at 20°C. The quenching transfer time does not exceed 15 seconds. After solution quenching, aging is performed at a temperature of 160°C and kept at this temperature for 26 hours.
[0051] Comparative Example 2
[0052] In this comparative example, the method for preparing the soluble aluminum alloy comprises the following steps:
[0053] 1) Material selection: Al-Cu-Li aluminum-lithium alloy waste is selected as the raw material; the raw material composition is 3.9% Cu, 0.9% Li, 0.7% Mg, 0.12% Zr, 0.35% Ag, and the balance is Al and impurities; the raw material type is the debris after sawing and turning;
[0054] 2) Ball milling: The raw materials were placed in a ball mill for ball milling. Argon gas was introduced for protection during ball milling. The mass ratio of the raw materials to the grinding balls was 1:2. The diameter of the grinding balls was 10 mm. The ball milling speed was 280 r / min and the ball milling time was 60 min.
[0055] 3) Pressing treatment: the raw material powder obtained after ball milling is loaded into a rubber mold and pressed by a cold isostatic press with a pressing pressure of 240 MPa and a holding time of 15 min;
[0056] 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 460°C and kept at this temperature for 6 hours, and then subjected to extrusion treatment, with an extrusion ratio of 12 and an extrusion rate of 0.41 mm / s;
[0057] 5) Solution quenching: The extruded material after extrusion treatment is subjected to solution quenching at a temperature of 510°C and kept at this temperature for 3 hours. After solution quenching, the material is immediately quenched. The quenching medium is water and the water temperature is controlled at 20°C. The quenching transfer time does not exceed 15 seconds. After solution quenching, aging is performed at a temperature of 160°C and kept at this temperature for 26 hours.
[0058] The aluminum alloy material prepared in this comparative example is shown in FIG. Figure 3 As shown, it can be seen that in this control example, due to the unreasonable ball milling process, there are larger compounds, which are poorly bonded to the matrix, forming large pores after falling off, reducing the plasticity and solubility of the alloy.
[0059] Comparative Example 3
[0060] In this comparative example, the method for preparing the soluble aluminum alloy comprises the following steps:
[0061] 1) Material selection: Al-Cu-Li aluminum-lithium alloy waste is selected as the raw material; the raw material composition is 3.9% Cu, 0.9% Li, 0.7% Mg, 0.12% Zr, 0.35% Ag, and the balance is Al and impurities; the raw material type is the debris after sawing and turning;
[0062] 2) Ball milling: The raw materials were placed in a ball mill for ball milling. The mass ratio of the raw materials to the grinding balls was 1:4, the diameter of the grinding balls was 10 mm, the ball milling speed was 280 r / min, and the ball milling time was 60 min.
[0063] 3) Pressing treatment: the raw material powder obtained after ball milling is loaded into a rubber mold and pressed by a cold isostatic press with a pressing pressure of 240 MPa and a holding time of 15 min;
[0064] 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 460°C and kept at this temperature for 6 hours, and then subjected to extrusion treatment, with an extrusion ratio of 12 and an extrusion rate of 0.41 mm / s;
[0065] 5) Solution quenching: The extruded material after extrusion treatment is subjected to solution quenching at a temperature of 510°C and kept at this temperature for 3 hours. After solution quenching, the material is immediately quenched. The quenching medium is water and the water temperature is controlled at 20°C. The quenching transfer time does not exceed 15 seconds. After solution quenching, aging is performed at a temperature of 160°C and kept at this temperature for 26 hours.
[0066] Comparative Example 4
[0067] In this comparative example, the method for preparing the soluble aluminum alloy comprises the following steps:
[0068] 1) Material selection: Al-Cu-Li aluminum-lithium alloy waste is selected as the raw material; the raw material composition is 3.9% Cu, 0.9% Li, 0.7% Mg, 0.12% Zr, 0.35% Ag, and the balance is Al and impurities; the raw material type is the debris after sawing and turning;
[0069] 2) Ball milling: The raw materials were placed in a ball mill for ball milling. Argon gas was introduced for protection during ball milling. The mass ratio of raw materials to grinding balls was 1:4. The diameter of the grinding balls was 10 mm. The ball milling speed was 280 r / min and the ball milling time was 60 min.
[0070] 3) Pressing treatment: The raw material powder obtained after ball milling is loaded into a rubber mold and pressed by a cold isostatic press with a pressing pressure of 160 MPa and a holding time of 15 min.
[0071] 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 460°C and kept at this temperature for 6 hours, and then subjected to extrusion treatment, with an extrusion ratio of 12 and an extrusion rate of 0.41 mm / s;
[0072] 5) Solution quenching: The extruded material after extrusion treatment is subjected to solution quenching at a temperature of 510°C and kept at this temperature for 3 hours. After solution quenching, the material is immediately quenched. The quenching medium is water and the water temperature is controlled at 20°C. The quenching transfer time does not exceed 15 seconds. After solution quenching, aging is performed at a temperature of 160°C and kept at this temperature for 26 hours.
[0073] Comparative Example 5
[0074] In this comparative example, the soluble aluminum alloy is a commercially available conventional soluble aluminum alloy Al-Ga-In-Sn system material provided by a bridge plug manufacturing unit.
[0075] Comparative Example 6
[0076] In this comparative example, the soluble aluminum alloy is a conventional high-strength aluminum alloy Al-Cu-Li system material produced by the company.
[0077] The mechanical properties and dissolution rate of the materials obtained in Example 1 and Example 2 were tested and compared, and the test results are shown in the following table. The mechanical properties test was carried out in accordance with GB / T228 standard, and the dissolution rate test was carried out using a 2 cm 3 The material was placed in a 3 wt% KCl solution at 93°C for measurement. The results are shown in Table 1.
[0078] Table 1
[0079]
[0080]
[0081] As can be seen from Table 1, the soluble aluminum alloy preparation method of the present invention can make full use of aluminum-lithium alloy waste, combine specific ball milling, pressing and extrusion, and solid solution quenching processes, and prepare a soluble aluminum alloy product that takes into account both mechanical properties and solubility without the need for external additives. As can be seen from the comparative example, the technical solution of the present invention, the combination of ball milling, pressing and extrusion, and solid solution quenching processes and parameter control are extremely critical. If the control is improper, a product with excellent performance cannot be obtained.
[0082] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a soluble aluminum alloy, It is characterized in that The steps include: 1) Material selection: Al-Cu-Li aluminum-lithium alloy waste is selected as raw material; 2) Ball milling: The raw materials are ball milled, an inert gas is introduced during the ball milling, the ball milling speed is 180-350r / min, and the ball milling time is 30-90min; 3) Pressing treatment: the raw material powder obtained after ball milling is pressed into a green sheet at a pressing pressure of 200-300 MPa and a holding time of 5-20 min; 4) Extrusion treatment: The blank obtained by the pressing treatment is heated to 440-480°C and kept warm for 4-8 hours, and then extruded with an extrusion ratio of 8-20 and an extrusion rate of 0.2-1 mm / s; 5) Solution quenching: The extruded material after the extrusion treatment is subjected to solution quenching, and then aging treatment is performed after the solution quenching is completed.
2. The method for preparing a soluble aluminum alloy according to claim 1, It is characterized in that In step 1), the Al-Cu-Li aluminum-lithium alloy waste has a Cu content of 3.2-4.2%, a Li content of 0.5-1.2%, a Mg content of 0.4-1.2%, a Zr content of 0.08-0.2%, an Ag content of 0.3-0.8%, and the balance is.
3. The method for preparing a soluble aluminum alloy according to claim 1, It is characterized in that In step 2), the mass ratio of the raw material to the grinding balls is 1:3-8, and the diameter of the grinding balls is 5-12 mm.
4. The method for preparing a soluble aluminum alloy according to claim 1, It is characterized in that In step 2), the inert gas is argon or nitrogen.
5. The method for preparing a soluble aluminum alloy according to claim 1, It is characterized in that In step 3), a cold isostatic press is used to carry out green compaction treatment.
6. The method for preparing a soluble aluminum alloy according to claim 1, It is characterized in that In step 5), after extrusion is completed, the extruded material is solution quenched at a temperature of 500 to 520°C for 2 to 4 hours, and quenched immediately after the solution is completed.
7. The method for preparing a soluble aluminum alloy according to claim 6, It is characterized in that In step 5), the quenching medium is water, the water temperature is controlled at 15-30° C., and the quenching transfer time does not exceed 15 seconds.
8. The method for preparing a soluble aluminum alloy according to claim 6, It is characterized in that In step 5), the aging system is 150-170° C. and the temperature is kept at 15-36 hours.
9. A soluble aluminum alloy, It is characterized in that The method is prepared by any one of claims 1 to 8.
10. The soluble aluminum alloy according to claim 9, It is characterized in that The tensile strength is greater than 580 MPa, the yield strength is greater than 530 MPa, the elongation is greater than 12%, and the dissolution rate is greater than 4.0 g / h.
Citation Information
Patent Citations
Ultrahigh-strength aluminum-lithium alloy and preparation method thereof
CN110423927A