Special-shaped copper strip and preparation method thereof

By optimizing the alloy composition and process flow, combined with electromagnetically assisted casting and annealing treatment, the cracking and insufficient hardness of the special-shaped copper belt during the forging process is solved, and the production of special-shaped copper belt with high conductivity and appropriate hardness is achieved, and the production efficiency is improved. and product quality.

CN118880101APending Publication Date: 2024-11-01CHINALCO DAYE COPPER PLATE & STRIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411104763.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing special-shaped copper belts are prone to cracking during forging and have low hardness, resulting in high production costs and increased customer complaints, limiting the development of the precision copper belt industry and the integrated circuit industry.

Method used

Using optimized alloy composition ratio and horizontal continuous casting combined with electromagnetic assisted casting technology, the ratio of Fe and P is controlled through uniform annealing and multi-pass cold rolling deformation treatment to ensure the work hardening and hardness requirements of copper tape during forging. , while avoiding cracking problems.

Benefits of technology

The high conductivity and appropriate hardness of the special-shaped copper tape are achieved, the production process is simplified, the cost is reduced, the production efficiency and product quality are improved, and the forging and cracking problem is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990414460000151
    Figure BDA0004990414460000151
Patent Text Reader

Abstract

The invention relates to the technical field of copper strip processing, in particular to a special-shaped copper strip and a preparation method thereof.The special-shaped copper strip is composed of 0.05%-0.1% of Fe, 0.02%-0.032% of P, 0.01%-0.04% of Zn and the balance Cu, and the mass ratio of Fe to P is 2.8-3.5. Compared with the prior art, the special-shaped copper strip has the advantages that the alloy composition proportion is optimized; the horizontal continuous casting strip blank with the uniform component structure is prepared in the mode of combining horizontal continuous casting and electromagnetic auxiliary casting, the technological process is shortened, the relatively moderate hardness level can be obtained in the subsequent machining process, the work hardening requirement in the forging and pressing process can be met, the cracking problem in the forging and pressing process can be avoided, and the production efficiency is improved. And through collaborative optimization of the forging process, it is ensured that the special-shaped copper material obtains the requirements for high conductivity and proper hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper strip processing, and in particular to a special-shaped copper strip and a preparation method thereof. Background Art

[0002] With the rapid development of the electronics and electrical industry, the miniaturization and high performance of electronic components have led to an increasing demand for special-shaped copper strips made of high-performance copper alloys. Due to the conductivity and heat dissipation of thick plates and the processability of thin plates, special-shaped copper strips have been used in the lead frames and high-current terminals of high-power ICs.

[0003] At the same time, with the continuous expansion of large-scale integrated circuit and ultra-large-scale integrated circuit production lines, and the continuous improvement of the performance and quality requirements of international high-end electronic equipment manufacturers for integrated circuit lead frames, the demand for copper strips for lead frames is also increasing. As one of the core materials for semiconductor discrete devices and integrated circuit packaging, the lead frame materials used internationally include copper alloy and nickel-iron alloy. Copper alloy lead frame materials are highly favored due to their excellent high conductivity, adaptability to processing, electric brazing, resistance to stress corrosion cracking, necessary strength and adhesion to resin packaging.

[0004] However, the copper strips produced by the semi-continuous casting → ingot heating → hot rolling → milling → cold rolling process for lead frame special-shaped copper strips currently have problems such as forging cracking and low hardness of special-shaped strips, which leads to low production cost rate of downstream customers and many customer complaints of production enterprises, and has become a bottleneck restricting the development of my country's precision copper strip industry and integrated circuit industry. Based on this, the present invention provides a short-process preparation method that solves problems such as forging cracking. The method has the characteristics of short production cycle, simple process, high production efficiency and stable quality. Summary of the invention

[0005] In order to overcome the above defects of the prior art, the present invention provides a special-shaped copper strip and a preparation method thereof, so as to solve the problems of forging cracking and low hardness of the special-shaped strip in the prior art.

[0006] A first aspect of the present invention provides a special-shaped copper strip, which is composed of the following components in mass percentage: Fe: 0.05-0.1%, P: 0.02-0.032%, Zn: 0.01-0.04%, and the remainder is Cu, and in the special-shaped copper strip, the mass ratio of Fe to P is: 2.8-3.5.

[0007] A second aspect of the present invention provides a method for preparing a special-shaped copper strip, the method specifically comprising the following steps:

[0008] S1, smelting the zinc sheet and electrolytic copper, and after they are completely melted, sequentially adding the baked iron sheet and copper-phosphorus master alloy, and obtaining an intermediate melt through heat preservation treatment;

[0009] S2, transferring the intermediate melt obtained in step S1 to a holding furnace, and after the composition is qualified, performing horizontal continuous casting by applying electromagnetic assistance, and obtaining a horizontal continuous casting strip after the casting is completed;

[0010] S3, subjecting the horizontal continuous casting strip obtained in step S2 to homogenization annealing, double-sided milling and 6-pass cold rolling deformation treatments, placing the strip in a bell furnace for annealing, degreasing, pickling and cleaning after the annealing, and then slitting to obtain a fixed-length flat strip;

[0011] S4, subjecting the fixed-length flat strip blank obtained in step S3 to forging treatment on a forging press to obtain a profiled strip blank, placing the profiled strip blank in a continuous annealing furnace for annealing treatment, and then brushing to obtain a profiled strip blank;

[0012] S5. The special-shaped strip obtained in step S4 is subjected to finish rolling, stamping treatment and slitting treatment in sequence to obtain a special-shaped copper strip.

[0013] Furthermore, in the step S1, the smelting process is carried out in a horizontal continuous casting smelting furnace, and the smelting temperature is 1230-1260°C; the insulation temperature is 1200-1220°C.

[0014] Furthermore, in step S2, the temperature of horizontal continuous casting is 1180-1200°C, and the horizontal continuous casting adopts a pull-stop-withdraw casting process with a casting speed of 14-16mm / min; the applied electromagnetic auxiliary parameters are as follows: frequency is 20-30Hz, current is 15-25A, and cooling water temperature of the electromagnetic stirrer is 40-45°C.

[0015] Furthermore, in step S3, the parameters of the homogenization annealing treatment are as follows: temperature is 720-750°C, and the holding time is 6-8h; the parameters of the annealing treatment in the bell furnace are as follows: temperature is 530-560°C, and the holding time is 4-6h.

[0016] Furthermore, in the step S3, in the 6-pass cold rolling deformation treatment, the deformation amount of each pass is: 25%→33%→29%→28%→23%→21%.

[0017] Furthermore, the parameters of the fixed-length flat strip obtained in step S3 are as follows: Vickers hardness is 58-63HV, electrical conductivity is ≥85% IACS, and elongation is ≥36%.

[0018] Furthermore, in the step S4, the forging speed of the forging process is 8-10 m / min, and the annealing temperature in the continuous annealing furnace is 700-750°C.

[0019] Furthermore, in step S5, the reduction amount of the finish rolling is 0.02-0.03 mm.

[0020] Furthermore, in step S5, the Vickers hardness of the special-shaped copper strip is 100-115 HV.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] The present invention adopts a method of optimizing the alloy component ratio and combining horizontal continuous casting with electromagnetic assisted casting to prepare a horizontal continuous casting strip with uniform composition and structure. The process flow is shortened, and a relatively moderate hardness level can be obtained in the subsequent processing process, which can meet the work hardening requirements in the forging process, avoid cracking problems in the forging process, and meet the hardness requirements of subsequent special-shaped finished products. By co-optimizing the forging process, it is ensured that the special-shaped copper material obtains the requirements of high conductivity and appropriate hardness. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.

[0026] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.

[0027] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0028] In the prior art, there are problems such as forging cracking and low hardness of special-shaped copper strips. In order to solve the above technical problems, the present invention provides a special-shaped copper strip. The special-shaped copper strip is composed of the following components in mass percentage: Fe: 0.05-0.1%, P: 0.02-0.032%, Zn: 0.01-0.04%, and the remainder is Cu, and in the special-shaped copper strip, the mass ratio of Fe to P is: 2.8-3.5. In the present invention, the content of Fe element is controlled within the range of 0.05-0.1%, because: the addition of Fe can improve the hardness and strength of copper, but excessive Fe will increase the brittleness of the material and affect the ductility and welding performance, while the technical solution is controlled within the range of 0.05-0.1%, Fe can enhance the wear resistance and corrosion resistance of the material while maintaining good electrical conductivity; phosphorus can be used as a deoxidizer in copper, it reacts with oxygen in copper liquid to form phosphide, which helps to reduce oxidized inclusions in the copper material and improve the purity and uniformity of copper, but the presence of excessive phosphorus element may also increase the brittleness of the material and greatly reduce the electrical conductivity. Therefore, the phosphorus content in the copper strip needs to be strictly controlled; the solid solution effect of zinc in copper can enhance the hardness and strength of copper, because zinc atoms form point defects in the copper lattice, hindering the movement of dislocations, thereby achieving solid solution strengthening, but copper with a high zinc content may show hot brittleness and easily produce self-cracking during the cooling process, which is caused by the precipitation and segregation of zinc during the cooling process; therefore, the technical solution controls the zinc content to 0.01-0.04%.

[0029] Finally, this technical solution controls the ratio of Fe and P elements, mainly taking into account: iron mainly strengthens the material by forming hard spots, while phosphorus strengthens the material through deoxidation and solid solution strengthening. However, excessive iron will make the material brittle and affect ductility; excessive phosphorus may cause the conductivity to decrease and cannot meet the use requirements. By controlling the Fe / P ratio, it is possible to improve strength while avoiding excessive sacrifice of ductility.

[0030] In summary, by adopting the element composition of the technical solution and combining it with the corresponding preparation process, the Vickers hardness of the obtained special-shaped copper strip can reach 100-115HV.

[0031] Another aspect of the present invention provides a method for preparing the above-mentioned special-shaped copper strip, which specifically comprises the following steps:

[0032] S1, smelting the zinc sheet and electrolytic copper, and after they are completely melted, sequentially adding the baked iron sheet and copper-phosphorus master alloy, and obtaining an intermediate melt through heat preservation treatment;

[0033] S2, transferring the intermediate melt obtained in step S1 to a holding furnace, and after the composition is qualified, performing horizontal continuous casting by applying electromagnetic assistance, and obtaining a horizontal continuous casting strip after the casting is completed;

[0034] S3, subjecting the horizontal continuous casting strip obtained in step S2 to homogenization annealing, double-sided milling and 6-pass cold rolling deformation treatments, placing the strip in a bell furnace for annealing, degreasing, pickling and cleaning after the annealing, and then slitting to obtain a fixed-length flat strip;

[0035] S4, subjecting the fixed-length flat strip blank obtained in step S3 to forging treatment on a forging press to obtain a profiled strip blank, placing the profiled strip blank in a continuous annealing furnace for annealing treatment, and then brushing to obtain a profiled strip blank;

[0036] S5. The special-shaped strip obtained in step S4 is subjected to finish rolling, stamping treatment and slitting treatment in sequence to obtain a special-shaped copper strip.

[0037] This technical solution adopts the method of optimizing the alloy composition ratio, combining horizontal continuous casting and electromagnetic assisted casting, to prepare a horizontal continuous casting strip with uniform composition and organization. Not only the process flow is shortened, but also a relatively moderate hardness level can be obtained in the subsequent processing process, which can not only meet the work hardening requirements in the forging process, but also avoid cracking problems in the forging process, and also meet the hardness requirements of the subsequent special-shaped finished products. By co-optimizing the forging process, it ensures that the special-shaped copper material obtains high conductivity and appropriate hardness. Compared with the existing methods, this method has the characteristics of simple operation, no cracking during forging, strong market competitiveness and significant economic benefits.

[0038] Further, in step S1, the smelting treatment is carried out in a horizontal continuous casting smelting furnace, and the smelting temperature is 1230-1260°C; the holding temperature is 1200-1220°C. In this step, first, the iron sheet and the copper-phosphorus master alloy are subjected to a baking treatment, the purpose of which is to remove the moisture in the iron sheet and the copper-phosphorus master alloy, as well as the mixing of chemical substances such as acid remaining in the iron sheet and the copper-phosphorus master alloy, to ensure the purity of the melt added to the horizontal continuous casting smelting furnace, and to reduce the introduction of impurity elements; secondly, the phosphorus element is introduced as a master alloy, the purpose of which is: on the one hand, the role of phosphorus in copper alloy is very subtle, and its content needs to be precisely controlled, and the use of copper-phosphorus master alloy can more accurately adjust the amount of phosphorus added, avoiding the problem of uneven distribution or excessive addition that may be caused by directly adding phosphorus powder; on the other hand, phosphorus is easy to volatilize at high temperature, and directly adding it to molten copper may cause phosphorus loss, affecting the phosphorus content of the final product. The phosphorus in the copper-phosphorus master alloy exists in a more stable form, which can improve the absorption efficiency of phosphorus in copper and reduce volatilization loss.

[0039] In the present technical solution, the above-mentioned smelting temperature is adopted because the above-mentioned temperature is sufficient to completely melt the electrolytic copper, and is also conducive to the full dissolution of the iron sheet and the copper-phosphorus intermediate alloy. In this step, temperature control is very critical. Too high a temperature may cause metal evaporation loss or oxidation, while insufficient temperature cannot ensure complete melting and uniform mixing of the raw materials.

[0040] Furthermore, in step S2, the temperature of horizontal continuous casting is 1180-1200°C, and the horizontal continuous casting adopts a pull-stop-withdraw casting process with a casting speed of 14-16mm / min; in the present technical scheme, compared with the existing process using semi-continuous casting, horizontal continuous casting can realize continuous production of metal materials. Compared with traditional casting methods, it greatly improves production efficiency, reduces production interruption time, and reduces energy consumption and cost per unit product. At the same time, during the horizontal continuous casting process, the molten metal is rapidly cooled and solidified in the mold to form a fine grain structure. This fine grain structure helps to improve the strength, toughness and processing properties of the material. By controlling the casting conditions, defects in the material, such as pores, shrinkage cavities and segregation, can be reduced or eliminated, further optimizing material properties.

[0041] Therefore, the technical solution adopts a casting temperature of 1180-1200° C., a pull-stop-withdraw casting process and a casting speed of 14-16 mm / min, and applies electromagnetic assistance.

[0042] Among them, the technical solution sets the temperature of horizontal continuous casting at 1180-1200℃. This temperature range can ensure that the melt maintains good fluidity while avoiding alloy performance degradation or oxidation caused by overheating. The casting speed of 14-16mm / min is mainly considered to be: the selection of this speed needs to balance the cooling rate and production efficiency of the casting, too fast or too slow may affect the quality of the casting; combined with the pull-stop-withdraw casting process, this casting process combines drawing casting with periodic stopping and retreating actions, which can effectively control the internal stress of the casting, reduce cracks and deformation, and help to achieve a finer microstructure.

[0043] The electromagnetic assistance parameters applied are as follows: frequency is 20-30Hz, current is 15-25A, and cooling water temperature of electromagnetic stirrer is 40-45℃. Based on the horizontal continuous casting method adopted in this technical solution, horizontal continuous casting is an efficient metal forming technology, especially suitable for the production of long strip materials, such as strips. In this process, the application of electromagnetic assistance can improve the fluidity and crystallization process of the melt, and help to form a more uniform and defect-free casting structure. The application of electromagnetic field can reduce segregation, inhibit the formation of pores and inclusions, and improve the density and flatness of the casting. This technical solution adopts electromagnetic assistance with the above parameters, which needs to be coordinated and optimized with other process parameters such as casting speed and cooling conditions to achieve the best casting effect. For example, an appropriate casting speed can cooperate with electromagnetic stirring to optimize the solidification process and improve the microstructural quality of the casting.

[0044] Further, in step S3, the parameters of the homogenization annealing treatment are as follows: the temperature is 720-750°C, and the holding time is 6-8h; the annealing treatment parameters in the bell furnace are as follows: the temperature is 530-560°C, and the holding time is 4-6h. In the present technical scheme, the purpose of the homogenization annealing treatment with the above parameters is to ensure that the alloy elements have enough time and energy to complete the diffusion process, while avoiding excessive growth of grains and affecting subsequent processing performance; the purpose of using the above annealing treatment parameters in the bell furnace is that the annealing temperature here is lower than that of the homogenization annealing, mainly to avoid the grains from growing again, while ensuring the stability and optimization of the material properties. After the annealing treatment is completed, further surface treatment is carried out to remove grease and contaminants, surface oxide scale and residual impurities on the surface of the material, and finally thoroughly clean the residual substances after pickling, so as to ensure a clean surface.

[0045] Furthermore, in step S3, in the 6-pass cold rolling deformation treatment, the deformation amount of each pass is: 25% → 33% → 29% → 28% → 23% → 21%. In this technical solution, the deformation amount of each pass is limited. This decreasing deformation amount arrangement can effectively control the work hardening of the material and avoid the risk of cracks or fractures in later processing.

[0046] The parameters of the fixed-length flat strip obtained in step S3 are as follows: Vickers hardness is 58-63HV, electrical conductivity is ≥85% IACS, and elongation is ≥36%.

[0047] Furthermore, in step S4, the forging speed of the forging process is 8-10 m / min, and the annealing temperature in the continuous annealing furnace is 700-750°C. In the present technical solution, in the process of processing the fixed-length flat strip into the final special-shaped strip, forging and annealing are two key steps, which are responsible for giving the material the desired shape and optimizing its performance, respectively. The present technical solution adopts a relatively high forging speed, which can help to increase the output. At the same time, the above-mentioned high annealing temperature can effectively promote the recrystallization process inside the material, eliminate work hardening, and restore the material to a relatively soft state, which is convenient for subsequent processing or use.

[0048] Further, in step S5, the reduction of the finishing rolling is 0.02-0.03mm. Step S5 is sequentially subjected to finishing rolling treatment, stamping treatment and slitting treatment, wherein the finishing rolling is to further reduce the thickness of the profiled strip by fine-tuning the reduction, while ensuring the dimensional accuracy and surface finish. This is the last thickness adjustment before the finished product, which is crucial for controlling the final thickness tolerance of the strip. Therefore, the present invention adopts a reduction of 0.02-0.03, which is a very fine value, meaning that the finishing rolling process pursues extremely high dimensional accuracy. Such a small reduction can ensure that the required thickness adjustment is achieved without introducing too much work hardening, while maintaining good surface quality. The entire S5 step is a highly precise process, from subtle thickness adjustment to complex shape forming to precise length segmentation, each link requires strict quality control to ensure that the dimensional accuracy, surface quality and mechanical properties of the final product meet high standards.

[0049] Based on the above element composition and process, the Vickers hardness of the special-shaped copper strip finally produced by this technical solution is 100-115HV.

[0050] The technical effects of the present invention are described below in conjunction with specific embodiments.

[0051] Example 1

[0052] The present embodiment provides a special-shaped copper strip, which is composed of the following components by mass percentage: Fe: 0.056%, P: 0.02%, Zn: 0.02%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 2.8. The special-shaped copper strip in the present embodiment is prepared by the following preparation method:

[0053] S1, placing zinc flakes and electrolytic copper in a horizontal continuous casting smelting furnace for smelting treatment at a smelting temperature of 1240°C, and after being completely melted, successively adding the baked iron flakes and copper-phosphorus master alloy, and obtaining an intermediate melt after heat preservation treatment at 1210°C;

[0054] S2, the intermediate melt obtained in step S1 is transferred to a holding furnace, and after the composition is qualified, horizontal continuous casting is carried out by applying electromagnetic assistance, and a horizontal continuous casting strip is obtained after the casting is completed; wherein, the temperature of the horizontal continuous casting is 1190°C, and the horizontal continuous casting adopts a pull-stop-withdraw casting process, and the casting speed is 14mm / min; the electromagnetic assistance parameters applied are as follows: the frequency is 20Hz, the current is 25A, and the cooling water temperature of the electromagnetic stirrer is 40°C;

[0055] S3, the horizontal continuous casting strip obtained in step S2 is subjected to homogenization annealing, double-sided milling and 6-pass cold rolling deformation treatment in sequence, and then placed in a bell furnace for annealing. After the annealing treatment, it is degreased, pickled and cleaned in sequence and then cut to obtain a fixed-length flat strip; wherein the parameters of the homogenization annealing treatment are as follows: the temperature is 730°C and the holding time is 7h; the annealing treatment parameters in the bell furnace are as follows: the temperature is 530°C and the holding time is 6h; in the 6-pass cold rolling deformation treatment, the deformation amount of each pass is as follows: 25%→33%→29%→28%→23%→21%; the parameters of the fixed-length flat strip finally obtained in this step are as follows: Vickers hardness is 60HV, conductivity is 87%IACS, and elongation is 39%;

[0056] S4, forging the fixed-length flat strip blank obtained in step S3 on a forging press to obtain a profiled strip blank, placing the profiled strip blank in a continuous annealing furnace for annealing and then brushing to obtain a profiled strip blank; wherein the forging speed of the forging treatment is 10 m / min, and the annealing temperature in the continuous annealing furnace is 750° C.;

[0057] S5. The special-shaped strip obtained in step S4 is subjected to finish rolling, stamping treatment and slitting treatment in sequence to obtain a special-shaped copper strip, wherein the reduction amount of the finish rolling is 0.024 mm.

[0058] Example 2

[0059] The present embodiment provides a special-shaped copper strip, which is composed of the following components by mass percentage: Fe: 0.1%, P: 0.0286%, Zn: 0.03%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 3.5. The special-shaped copper strip in the present embodiment is prepared by the following preparation method:

[0060] S1, placing zinc flakes and electrolytic copper in a horizontal continuous casting smelting furnace for smelting treatment at a smelting temperature of 1260°C, and after being completely melted, successively adding the baked iron flakes and copper-phosphorus master alloy, and obtaining an intermediate melt after heat preservation treatment at 1220°C;

[0061] S2, the intermediate melt obtained in step S1 is transferred to a holding furnace, and after the composition is qualified, horizontal continuous casting is carried out by applying electromagnetic assistance, and a horizontal continuous casting strip is obtained after the casting is completed; wherein, the temperature of the horizontal continuous casting is 1200°C, and the horizontal continuous casting adopts a pull-stop-withdraw casting process, and the casting speed is 16mm / min; the electromagnetic assistance parameters applied are as follows: the frequency is 23Hz, the current is 18A, and the cooling water temperature of the electromagnetic stirrer is 42°C;

[0062] S3, the horizontal continuous casting strip obtained in step S2 is subjected to homogenization annealing, double-sided milling and 6-pass cold rolling deformation treatment in sequence, and then placed in a bell furnace for annealing. After the annealing treatment, it is degreased, pickled and cleaned in sequence and then cut to obtain a fixed-length flat strip; wherein the parameters of the homogenization annealing treatment are as follows: the temperature is 740°C and the holding time is 7h; the annealing treatment parameters in the bell furnace are as follows: the temperature is 560°C and the holding time is 4h; in the 6-pass cold rolling deformation treatment, the deformation amount of each pass is as follows: 25%→33%→29%→28%→23%→21%; the parameters of the fixed-length flat strip finally obtained in this step are as follows: Vickers hardness is 58HV, conductivity is 85%IACS, and elongation is 40%;

[0063] S4, forging the fixed-length flat strip blank obtained in step S3 on a forging press to obtain a profiled strip blank, placing the profiled strip blank in a continuous annealing furnace for annealing and then brushing to obtain a profiled strip blank; wherein the forging speed of the forging treatment is 9 m / min, and the annealing temperature in the continuous annealing furnace is 720° C.;

[0064] S5. The special-shaped strip obtained in step S4 is subjected to finish rolling, stamping treatment and slitting treatment in sequence to obtain a special-shaped copper strip, wherein the reduction amount of the finish rolling is 0.03 mm.

[0065] Example 3

[0066] The present embodiment provides a special-shaped copper strip, which is composed of the following components by mass percentage: Fe: 0.095%, P: 0.032%, Zn: 0.01%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 2.97. The special-shaped copper strip in the present embodiment is prepared by the following preparation method:

[0067] S1, placing zinc flakes and electrolytic copper in a horizontal continuous casting smelting furnace for smelting treatment at a smelting temperature of 1230°C, and after being completely melted, successively adding the baked iron flakes and copper-phosphorus master alloy, and obtaining an intermediate melt after heat preservation treatment at 1200°C;

[0068] S2, the intermediate melt obtained in step S1 is transferred to a holding furnace, and after the composition is qualified, horizontal continuous casting is carried out by applying electromagnetic assistance, and a horizontal continuous casting strip is obtained after the casting is completed; wherein, the temperature of the horizontal continuous casting is 1180°C, and the horizontal continuous casting adopts a pull-stop-withdraw casting process, and the casting speed is 15mm / min; the electromagnetic assistance parameters applied are as follows: frequency is 30Hz, current is 15A, and the cooling water temperature of the electromagnetic stirrer is 45°C;

[0069] S3, the horizontal continuous casting strip obtained in step S2 is subjected to homogenization annealing, double-sided milling and 6-pass cold rolling deformation treatment in sequence, and then placed in a bell furnace for annealing. After the annealing treatment, it is degreased, pickled and cleaned in sequence and then cut to obtain a fixed-length flat strip; wherein the parameters of the homogenization annealing treatment are as follows: the temperature is 750°C and the holding time is 6h; the annealing treatment parameters in the bell furnace are as follows: the temperature is 540°C and the holding time is 5h; in the 6-pass cold rolling deformation treatment, the deformation amount of each pass is as follows: 25%→33%→29%→28%→23%→21%; the parameters of the fixed-length flat strip finally obtained in this step are as follows: Vickers hardness is 62HV, conductivity is 86%IACS, and elongation is 37%;

[0070] S4, forging the fixed-length flat strip blank obtained in step S3 on a forging press to obtain a profiled strip blank, placing the profiled strip blank in a continuous annealing furnace for annealing and then brushing to obtain a profiled strip blank; wherein the forging speed of the forging treatment is 10 m / min, and the annealing temperature in the continuous annealing furnace is 740° C.;

[0071] S5. The special-shaped strip obtained in step S4 is subjected to finish rolling, stamping treatment and slitting treatment in sequence to obtain a special-shaped copper strip, wherein the reduction amount of the finish rolling is 0.02 mm.

[0072] Example 4

[0073] The present embodiment provides a special-shaped copper strip, which is composed of the following components by mass percentage: Fe: 0.08%, P: 0.025%, Zn: 0.04%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 3.2. The special-shaped copper strip in the present embodiment is prepared by the following preparation method:

[0074] S1. Place zinc flakes and electrolytic copper in a horizontal continuous casting smelting furnace for smelting at a temperature of 1250° C. After they are completely melted, add the baked iron flakes and copper-phosphorus master alloy in sequence, and obtain an intermediate melt after heat preservation at 1215° C.;

[0075] S2. Convert the intermediate melt obtained in step S1 to a holding furnace, and after the composition is qualified, carry out horizontal continuous casting by applying electromagnetic assistance, and obtain a horizontal continuous casting strip after the casting is completed; wherein, the temperature of the horizontal continuous casting is 1195°C, and the horizontal continuous casting adopts a pull-stop-withdraw casting process, and the casting speed is 14mm / min; the electromagnetic assistance parameters applied are as follows: the frequency is 26Hz, the current is 21A, and the cooling water temperature of the electromagnetic stirrer is 44°C;

[0076] S3, the horizontal continuous casting strip obtained in step S2 is subjected to homogenization annealing, double-sided milling and 6-pass cold rolling deformation treatment in sequence, and then placed in a bell furnace for annealing. After the annealing treatment, it is degreased, pickled and cleaned in sequence and then cut to obtain a fixed-length flat strip; wherein the parameters of the homogenization annealing treatment are as follows: the temperature is 720°C and the holding time is 8h; the annealing treatment parameters in the bell furnace are as follows: the temperature is 550°C and the holding time is 5h; in the 6-pass cold rolling deformation treatment, the deformation amount of each pass is as follows: 25%→33%→29%→28%→23%→21%; the parameters of the fixed-length flat strip finally obtained in this step are as follows: Vickers hardness is 63HV, conductivity is 89%IACS, and elongation is 36%;

[0077] S4, forging the fixed-length flat strip blank obtained in step S3 on a forging press to obtain a profiled strip blank, placing the profiled strip blank in a continuous annealing furnace for annealing and then brushing to obtain a profiled strip blank; wherein the forging speed of the forging treatment is 8 m / min, and the annealing temperature in the continuous annealing furnace is 700° C.;

[0078] S5. The special-shaped strip obtained in step S4 is subjected to finish rolling, stamping treatment and slitting treatment in sequence to obtain a special-shaped copper strip, wherein the reduction amount of the finish rolling is 0.028 mm.

[0079] Comparative Example 1

[0080] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that the special-shaped copper strip in this comparative example is composed of the following components in mass percentage: Fe: 0.056%, P: 0.021%, Zn: 0.02%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 2.67. The preparation method is the same as that in Example 1, and will not be repeated here.

[0081] Comparative Example 2

[0082] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that the special-shaped copper strip in this comparative example is composed of the following components in mass percentage: Fe: 0.072%, P: 0.02%, Zn: 0.02%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is 3.6. The preparation method is the same as that in Example 1, and will not be repeated here.

[0083] Comparative Example 3

[0084] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that the special-shaped copper strip in this comparative example is composed of the following components in mass percentage: Fe: 0.056%, P: 0.018%, Zn: 0.02%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 3.1. The preparation method is the same as that in Example 1, and will not be repeated here.

[0085] Comparative Example 4

[0086] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that the special-shaped copper strip in this comparative example is composed of the following components in mass percentage: Fe: 0.112%, P: 0.032%, Zn: 0.02%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is 3.5. The preparation method is the same as that in Example 1, and will not be repeated here.

[0087] Comparative Example 5

[0088] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that the special-shaped copper strip in this comparative example is composed of the following components in mass percentage: Fe: 0.056%, P: 0.02%, Zn: 0.05%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 2.8. The preparation method is the same as that in Example 1, and will not be repeated here.

[0089] Comparative Example 6

[0090] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that the special-shaped copper strip in this comparative example is composed of the following components in mass percentage: Fe: 0.056%, P: 0.02%, Zn: 0.00%, and the balance is Cu, and the mass ratio of Fe to P in the special-shaped copper strip is: 2.8. The preparation method is the same as that in Example 1, and will not be repeated here.

[0091] Comparative Example 7

[0092] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that, during the preparation process of the special-shaped copper strip in this comparative example, in step S2, there is no electromagnetic assistance method in the horizontal continuous casting process, and the rest is the same as Example 1 and will not be repeated here.

[0093] Comparative Example 8

[0094] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that, during the preparation process of the special-shaped copper strip in this comparative example, a semi-continuous casting method is adopted in step S2 in combination with electromagnetic assistance, and the temperature of the semi-continuous casting is 1190°C. The rest is the same as Example 1 and will not be repeated here.

[0095] Comparative Example 9

[0096] This comparative example provides a special-shaped copper strip, which is different from Example 1 only in that, during the preparation process of the special-shaped copper strip in this comparative example, in step S3, in the 6-pass cold rolling deformation treatment, the deformation amount of each pass is: 25%→35%→28%→27%→23%→21%, and the rest is the same as Example 1 and will not be repeated here.

[0097] The hardness of the special-shaped copper strips prepared in Examples 1-4 and Comparative Examples 1-9 was tested, and the test results are shown in Table 1:

[0098] Table 1: Performance test results of special-shaped copper strips obtained in Examples 1-4 and Comparative Examples 1-9

[0099]

[0100] From the above results, it can be seen that the improvement of the element composition of the special-shaped copper strip material in the present application has a certain synergistic effect on the improvement of the comprehensive performance of the special-shaped copper strip, which can greatly improve the hardness of the special-shaped copper strip while improving its surface performance, processing performance and lower internal stress. Specifically, referring to Example 1, Comparative Example 1 and Comparative Example 2, the mass ratios of Fe and P are 2.67 and 3.6, respectively, which are lower or higher than the ratio range (2.8-3.5) specified in the present invention. Although the contents of Fe and P are within the range specified in the present invention, the performance of the obtained special-shaped copper strip is still reduced. Considering that in the combination of Fe and P, excessive iron will make the material brittle and affect ductility, while excessive phosphorus may cause Hydrogen embrittlement reduces the toughness of the material, so the element ratio of Fe and P plays an important role in the present invention; referring to the data of Example 1, Comparative Example 3 and Comparative Example 4, it can be seen that although the ratio of Fe element to P element is controlled within the range defined in the present invention, if Fe element and P element are not within the range defined in the present invention, the performance of the obtained special-shaped copper strip will still be reduced. It is considered that after the Fe element is increased, excessive iron will precipitate during the cooling process to form second phase particles, which will affect the microstructure and properties of the material. After the P element is increased, it forms hard and brittle compounds with copper, such as Cu3P. These compounds are unevenly distributed in the material and will become the starting point of cracks, reducing the fracture toughness of the material.

[0101] With reference to Example 1, Comparative Example 5 and Comparative Example 6, it can be seen that a small amount of Zn element has a positive effect on the performance of the special-shaped copper strip, while a certain amount of Zn element will have a negative impact on the special-shaped copper strip. The main reasons are as follows: when the zinc content is below 0.04%, as the zinc content increases, the addition of zinc forms a solid solution, and the strength and plasticity of the copper material continue to increase. However, once it exceeds the threshold, the plasticity of the special-shaped copper strip decreases rapidly. Therefore, it is necessary to strictly control the composition and ratio of the elements in the special-shaped copper strip to obtain a special-shaped copper strip with higher hardness.

[0102] It can be seen from Example 1 and Comparative Example 7 that compared with the case where electromagnetic assistance is applied, the flatness and warpage of the special-shaped copper strip obtained without electromagnetic assistance are greatly reduced, and correspondingly, other properties are also reduced. This is considered to be because compared with the case where electromagnetic assistance is not applied, the segregation in the structural parts with electromagnetic assistance is reduced, and the formation of pores and inclusions is suppressed, thereby improving the density and flatness and other mechanical properties of the casting.

[0103] It can be seen from Example 1 and Comparative Example 8 that the flatness and warpage obtained by the full-continuous casting process of the present invention are greatly reduced, while other mechanical properties are also reduced. Considering that: full-continuous casting is a completely continuous process, in which molten metal continuously flows from a furnace into a crystallizer and solidified metal billets are continuously pulled out from the other end of the crystallizer, more uniform material quality can be provided because the cooling and solidification conditions are more controllable and the vibration of the crystallizer can improve the grain structure.

[0104] With reference to Example 1 and Comparative Example 9, it can be seen that the present invention further limits the optimal deformation amount of each pass. Even if the total deformation amount of Comparative Example 9 is the same as that of Example 1, the performance of the special-shaped copper strip obtained therefrom is relatively reduced. This is because limiting the deformation amount of each pass helps to control the microstructure of the material, such as grain size, dislocation density and texture, thereby affecting the mechanical properties of the material, such as strength, plasticity, hardness and toughness. The number of passes and the deformation amount of each pass used in the present invention are strictly limited according to the material composition of the present invention and are specific. Therefore, the above-mentioned deformation amount of the present invention can obtain a special-shaped copper strip with optimal performance.

[0105] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A special-shaped copper strip, characterized in that: In terms of mass percentage, the special-shaped copper strip is composed of the following components: Composition: Fe: 0.05-0.1%, P: 0.02-0.032%, Zn: 0.01-0.04%, and the balance is Cu, and in the special-shaped copper strip, the mass ratio of Fe to P is: 2.8-3.

5.

2. A method for preparing the special-shaped copper strip according to claim 1, characterized in that: The preparation method specifically comprises the following steps: S1, smelting the zinc sheet and electrolytic copper, and after they are completely melted, sequentially adding the baked iron sheet and copper-phosphorus master alloy, and obtaining an intermediate melt through heat preservation treatment; S2, transferring the intermediate melt obtained in step S1 to a holding furnace, and after the composition is qualified, performing horizontal continuous casting by applying electromagnetic assistance, and obtaining a horizontal continuous casting strip after the casting is completed; S3, subjecting the horizontal continuous casting strip obtained in step S2 to homogenization annealing, double-sided milling and 6-pass cold rolling deformation treatments, placing the strip in a bell furnace for annealing, degreasing, pickling and cleaning after the annealing, and then slitting to obtain a fixed-length flat strip; S4, subjecting the fixed-length flat strip blank obtained in step S3 to forging treatment on a forging press to obtain a profiled strip blank, placing the profiled strip blank in a continuous annealing furnace for annealing treatment, and then brushing to obtain a profiled strip blank; S5. The special-shaped strip obtained in step S4 is subjected to finish rolling, stamping treatment and slitting treatment in sequence to obtain a special-shaped copper strip.

3. The method for preparing the special-shaped copper strip according to claim 2, characterized in that: In the step S1, the smelting process is carried out in a horizontal continuous casting smelting furnace, and the smelting temperature is 1230-1260°C; the insulation temperature is 1200-1220°C.

4. The method for preparing the special-shaped copper strip according to claim 2, characterized in that: In step S2, the temperature of horizontal continuous casting is 1180-1200°C, and the horizontal continuous casting adopts a pull-stop-withdraw casting process with a casting speed of 14-16mm / min; the applied electromagnetic auxiliary parameters are as follows: frequency is 20-30Hz, current is 15-25A, and cooling water temperature of the electromagnetic stirrer is 40-45°C.

5. The method for preparing the special-shaped copper strip according to claim 2, characterized in that: In step S3, the parameters of the homogenization annealing treatment are as follows: temperature is 720-750° C., and the holding time is 6-8 hours; the parameters of the annealing treatment in the bell furnace are as follows: temperature is 530-560° C., and the holding time is 4-6 hours.

6. The method for preparing a special-shaped copper strip according to claim 2, characterized in that: In step S3, in the 6-pass cold rolling deformation process, the deformation amount of each pass is: 25%→33%→29%→28%→23%→21%。 7. The method for preparing a special-shaped copper strip according to claim 2, characterized in that: The parameters of the fixed-length flat strip obtained in step S3 are as follows: Vickers hardness is 58-63HV, electrical conductivity is ≥ 85% IACS, elongation ≥ 36%.

8. The method for preparing a special-shaped copper strip according to claim 2, characterized in that: In the step S4, the forging speed of the forging process is 8-10 m / min, and the annealing temperature in the continuous annealing furnace is 700-750°C.

9. The method for preparing a special-shaped copper strip according to claim 2, characterized in that: In the step S5, the reduction amount of the finish rolling is 0.02-0.03 mm.

10. The method for preparing a special-shaped copper strip according to claim 2, characterized in that: In the step S5, the Vickers hardness of the special-shaped copper strip is 100-115 HV.