Preparation method for reducing surface glossiness of copper strip
Through degreasing, water washing, pickling and chemical corrosion, microconcave structure on the surface of the copper belt is formed, which reduces the glossiness, and improves corrosion resistance and wear resistance through passivation and coating treatment, solving the glossiness of the copper belt surface High problems achieve wider application potential.
Patent Information
- Application Number
- CN202410954325.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
AI Technical Summary
The excessive gloss of the copper tape surface affects its corrosion resistance, wear resistance and solderability.
Through degreasing, water washing, pickling, neutralization and chemical corrosion, a microconcave and convex structure on the surface of the copper belt is formed to reduce gloss, and corrosion resistance and wear resistance are improved through passivation and coating treatment.
The matte effect on the surface of the copper tape is achieved, while improving its corrosion resistance, wear resistance and solderability, extending service life and expanding application range.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper strip surface treatment, and in particular relates to a preparation method for reducing the surface glossiness of a copper strip. Background Art
[0002] Copper strip is a common metal material with excellent electrical conductivity, thermal conductivity and plasticity. It is made of copper alloy through rolling, stretching and other processes, usually in strip shape with varying widths. The thickness of copper strip is generally between 0.1 mm and 3 mm, and the length can be cut as needed. Copper strip has good mechanical properties, including tensile strength, elongation and hardness. This makes copper strip widely used in many industrial fields. First of all, copper strip has very good electrical conductivity, so it is widely used in the electronics, electrical and communications industries. It can be used to manufacture electronic products such as wires, cables, circuit boards, and power transmission and distribution equipment for power systems. Secondly, copper strip also has excellent thermal conductivity, so it is widely used in radiators, heat exchangers and other fields. It can effectively conduct heat to ensure the normal operation and stability of equipment. In addition, copper strip can also be used to make various structural parts and decorations. It has good plasticity and can be processed into parts of various shapes through stamping, bending and other processes, which are used in construction, automobiles, aerospace and other industries. Copper strip also has excellent corrosion resistance, especially after special treatment, such as passivation, coating, etc., which can further improve its corrosion resistance, wear resistance and weldability. This makes copper strip have a wide range of application prospects in marine engineering, chemical equipment and other fields.
[0003] However, the surface gloss of common copper strips is too high and cannot effectively scatter light, which affects the corrosion resistance, wear resistance and solderability of the copper strips during storage. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method for reducing the surface gloss of a copper strip in order to solve the above-mentioned problem.
[0005] The technical solution adopted by the present invention is as follows: a preparation method for reducing the surface glossiness of a copper strip, the method comprising the following steps:
[0006] S 1: First, the copper strip is dehydrogenated. The purpose of this step is to remove grease and dirt on the surface of the copper strip to ensure that the surface of the copper strip is clean and ready for subsequent treatment. Degreasing treatment is usually carried out using organic solvents or alkaline solutions. During the degreasing process, the concentration, temperature and time of the degreasing agent need to be controlled to ensure the degreasing effect.
[0007] S2: After degreasing, the copper strip needs to be thoroughly washed to remove residual degreasing agent and loose dirt. Clean water is required during the washing process to avoid leaving water marks and other contaminants on the surface of the copper strip.
[0008] S3: After water washing, pickling treatment is carried out. This step is to remove oxides and dirt on the surface of the copper strip and further purify the surface of the copper strip. Commonly used pickling solutions include sulfuric acid, hydrochloric acid or nitric acid. During the pickling process, the concentration, temperature and time of the pickling solution need to be controlled to avoid excessive corrosion to the copper strip.
[0009] S4: After pickling, the copper strip needs to be washed with water to remove the residual pickling solution. Then, the copper strip is neutralized with a neutralizer to remove the residual acidic substances and avoid corrosion to the copper strip.
[0010] S5: After the neutralization treatment, the copper strip surface is chemically etched. This step is the key to reducing the glossiness of the copper strip surface. Through chemical etching, a layer of tiny bumps can be formed on the surface of the copper strip, which can reduce the glossiness of the copper strip surface and make it more matte. During the electrochemical etching process, the concentration, temperature and time of the etching solution need to be controlled to obtain the ideal etching effect.
[0011] S6: After chemical corrosion, the copper strip needs to be washed with water to remove the residual corrosion liquid. Then, the copper strip is dried to remove moisture and avoid leaving water marks on the surface of the copper strip. S7: In order to further improve the performance of the copper strip, some post-treatments can be performed, such as passivation treatment, coating treatment, etc. These treatments can further improve the corrosion resistance, wear resistance and solderability of the copper strip.
[0012] S8: Finally, the treated copper strips are inspected for appearance and tested for performance to ensure that they meet the requirements. Then, the qualified copper strips are packaged to prevent contamination and damage during transportation and storage.
[0013] In a preferred embodiment, in step S1, the degreasing treatment uses an organic solvent such as acetone, isopropanol or n-hexane, or an alkaline solution such as sodium hydroxide or potassium hydroxide. In the degreasing process, for organic solvent degreasing, the copper strip can be immersed in the solvent, the temperature is controlled between room temperature and 50°C, and the immersion time is 1-2 minutes. For alkaline solution degreasing, the copper strip can be immersed in a 5%-10% sodium hydroxide solution, the temperature is controlled between 60-80°C, and the immersion time is generally 10-30 seconds.
[0014] In a preferred embodiment, in step S2, the water washing can be performed by spraying, soaking or brushing to ensure that the degreasing agent and loose dirt on the surface of the copper strip are thoroughly cleaned. The water washing temperature is generally controlled between room temperature and 40°C, and the time is 5-10 seconds.
[0015] In a preferred embodiment, in step S3, the pickling solution commonly used in the pickling treatment includes sulfuric acid, hydrochloric acid or nitric acid. Use 5%-10% sulfuric acid solution, 5%-10% hydrochloric acid solution or 5%-10% nitric acid solution for pickling. During the pickling process, it is necessary to control the concentration, temperature and time of the pickling solution. The pickling temperature is generally controlled between room temperature and 60°C, and the time is generally 1-2 minutes. After pickling, it is necessary to perform a thorough water wash to remove the residual pickling solution.
[0016] In a preferred embodiment, in step S4, after washing with water, the copper strip can be neutralized with a neutralizer to remove residual acidic substances. Commonly used neutralizers include alkaline solutions such as sodium hydroxide and potassium hydroxide. The copper strip can be immersed in a 5%-10% sodium hydroxide solution, the temperature is controlled between room temperature and 40°C, and the immersion time is 1-2 minutes. After neutralization, it is necessary to wash thoroughly with water to remove the residual neutralizer.
[0017] In a preferred embodiment, in step S5, 5%-10% sulfuric acid solution, 5%-10% hydrochloric acid solution or 5%-10% nitric acid solution is used for corrosion. During the electrochemical corrosion process, the concentration, temperature and time of the corrosion solution need to be controlled. The corrosion temperature is generally controlled between room temperature and 50°C, and the time is generally 3-5 minutes. After corrosion, it is necessary to wash thoroughly with water to remove the residual corrosion solution.
[0018] In a preferred embodiment, in step S6, after washing, the copper strip is dried to remove moisture, and the copper strip is placed in a well-ventilated place to dry naturally, or is dried using a hot air dryer at a temperature of 100-150° C., and the time is generally 5-30 minutes.
[0019] In a preferred embodiment, in step S7, a passivation treatment is performed, and the copper strip is treated with a passivation solution such as chromic acid, phosphate or silicate to improve its corrosion resistance.
[0020] In a preferred embodiment, in step S7, after passivation, a coating treatment may be performed, for example, coating the copper strip with epoxy coating, polyurethane coating or acrylic coating to improve its wear resistance and solderability.
[0021] In a preferred embodiment, in step S8, the performance test may include tensile strength, elongation, hardness, corrosion resistance and solderability, etc. After passing the test, the copper strip is packaged, which may be coiled, vacuum packed or moisture-proof packed, etc., to prevent contamination and damage during transportation and storage.
[0022] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0023] 1. In the present invention, grease, dirt, oxides and other impurities on the surface of the copper strip are completely removed through pretreatment steps such as degreasing, washing, pickling and neutralization, creating ideal surface conditions for subsequent chemical corrosion. This series of treatments not only ensures the cleanliness of the copper strip surface, but also lays the foundation for forming a uniform and controllable corrosion effect. In particular, by accurately controlling the concentration, temperature and treatment time of chemical reagents such as degreasing agents, pickling solutions, neutralizing agents, etc., it can be ensured that the copper strip surface will not have problems of over-corrosion or under-corrosion, thereby reducing the glossiness while maintaining the original physical and mechanical properties of the copper strip material.
[0024] 2. In the present invention, by controlling the type and concentration of the etching solution, the etching temperature and time, a microscopic concave-convex structure can be formed on the surface of the copper strip, which effectively scatters light, reduces specular reflection, and achieves a matte effect. Moreover, through post-treatment such as passivation and coating treatment, the corrosion resistance, wear resistance and solderability of the copper strip can be further enhanced, which not only improves the service life of the copper strip, but also expands its application range. Finally, after strict appearance inspection and performance testing, the quality of each batch of copper strips is ensured to meet the high standards of different fields, so that the product can maintain stable performance during transportation and storage and is not easily damaged. These comprehensive measures make the copper strip prepared by this method have a wide range of application potentials in the electronics, electrical, communications and decoration industries. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] Example:
[0027] A preparation method for reducing the surface glossiness of a copper strip, the method comprising the following steps:
[0028] S 1: First, the copper strip is dehydrogenated. The purpose of this step is to remove grease and dirt on the surface of the copper strip to ensure that the surface of the copper strip is clean and ready for subsequent treatment. Degreasing treatment is usually carried out using organic solvents or alkaline solutions. During the degreasing process, the concentration, temperature and time of the degreasing agent need to be controlled to ensure the degreasing effect.
[0029] S2: After degreasing, the copper strip needs to be thoroughly washed to remove residual degreasing agent and loose dirt. Clean water is required during the washing process to avoid leaving water marks and other contaminants on the surface of the copper strip.
[0030] S3: After water washing, pickling treatment is carried out. This step is to remove oxides and dirt on the surface of the copper strip and further purify the surface of the copper strip. Commonly used pickling solutions include sulfuric acid, hydrochloric acid or nitric acid. During the pickling process, the concentration, temperature and time of the pickling solution need to be controlled to avoid excessive corrosion to the copper strip.
[0031] S4: After pickling, the copper strip needs to be washed with water to remove the residual pickling solution. Then, the copper strip is neutralized with a neutralizer to remove the residual acidic substances and avoid corrosion to the copper strip.
[0032] S5: After the neutralization treatment, the copper strip surface is chemically etched. This step is the key to reducing the glossiness of the copper strip surface. Through chemical etching, a layer of tiny bumps can be formed on the surface of the copper strip, which can reduce the glossiness of the copper strip surface and make it more matte. During the electrochemical etching process, the concentration, temperature and time of the etching solution need to be controlled to obtain the ideal etching effect.
[0033] S6: After chemical corrosion, the copper strip needs to be washed with water to remove the residual corrosion liquid. Then, the copper strip is dried to remove moisture and avoid leaving water marks on the surface of the copper strip. S7: In order to further improve the performance of the copper strip, some post-treatments can be performed, such as passivation treatment, coating treatment, etc. These treatments can further improve the corrosion resistance, wear resistance and solderability of the copper strip.
[0034] S8: Finally, the treated copper strips are inspected for appearance and tested for performance to ensure that they meet the requirements. Then, the qualified copper strips are packaged to prevent contamination and damage during transportation and storage.
[0035] In step S1, the degreasing treatment uses an organic solvent such as acetone, isopropanol or n-hexane, or an alkaline solution such as sodium hydroxide or potassium hydroxide. In the degreasing process, for organic solvent degreasing, the copper strip can be immersed in the solvent, the temperature is controlled between room temperature and 50°C, and the immersion time is 1-2 minutes. For alkaline solution degreasing, the copper strip can be immersed in a 5%-10% sodium hydroxide solution, the temperature is controlled between 60-80°C, and the immersion time is generally 10-30 seconds.
[0036] In step S2, the water washing can be performed by spraying, soaking or brushing to ensure that the degreaser and loose dirt on the surface of the copper strip are thoroughly cleaned. The water washing temperature is generally controlled between room temperature and 40°C, and the time is 5-10 seconds.
[0037] In step S3, the pickling solution commonly used in the pickling treatment includes sulfuric acid, hydrochloric acid or nitric acid. Use 5%-10% sulfuric acid solution, 5%-10% hydrochloric acid solution or 5%-10% nitric acid solution for pickling. During the pickling process, the concentration, temperature and time of the pickling solution need to be controlled. The pickling temperature is generally controlled between room temperature and 60°C, and the time is generally 1-2 minutes. After pickling, a thorough water wash is required to remove the residual pickling solution.
[0038] In step S4, after washing with water, the copper strip can be neutralized with a neutralizer to remove residual acidic substances. Commonly used neutralizers include alkaline solutions such as sodium hydroxide and potassium hydroxide. The copper strip can be soaked in a 5%-10% sodium hydroxide solution, the temperature is controlled between room temperature and 40°C, and the soaking time is 1-2 minutes. After neutralization, it is necessary to wash thoroughly with water to remove the residual neutralizer.
[0039] In step S5, 5%-10% sulfuric acid solution, 5%-10% hydrochloric acid solution or 5%-10% nitric acid solution is used for corrosion. During the electrochemical corrosion process, the concentration, temperature and time of the corrosion solution need to be controlled. The corrosion temperature is generally controlled between room temperature and 50°C, and the time is generally 3-5 minutes. After corrosion, it is necessary to wash thoroughly with water to remove the residual corrosion solution.
[0040] In step S6, after washing, the copper strip is dried to remove moisture, and the copper strip is placed in a well-ventilated place to dry naturally, or is dried using a hot air dryer at a temperature of 100-150° C., and the time is generally 5-30 minutes.
[0041] In step S7, a passivation treatment is performed, using a passivation solution such as chromic acid, phosphate or silicate to treat the copper strip to improve its corrosion resistance.
[0042] In step S7, after passivation, a coating treatment may be performed, for example, coating the copper strip with epoxy coating, polyurethane coating or acrylic coating to improve its wear resistance and solderability.
[0043] In step S8, the performance test may include tensile strength, elongation, hardness, corrosion resistance and solderability, etc. After passing the test, the copper strip is packaged, which may be coiled, vacuum packed or moisture-proof packed to prevent contamination and damage during transportation and storage.
[0044] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A preparation method for reducing the surface gloss of a copper strip, characterized in that: The method comprises the following steps: S1: First, the copper strip is degreased to remove grease and dirt on the surface of the copper strip to ensure that the surface of the copper strip is clean in preparation for subsequent processing; the degreasing treatment is carried out using an organic solvent or an alkaline solution; S2: After degreasing, the copper strip needs to be thoroughly washed to remove residual degreasing agent and loose dirt. Clean water is required during the washing process to avoid leaving water marks and other contaminants on the surface of the copper strip; S3: After water washing, pickling treatment is performed to remove oxides and dirt on the surface of the copper strip and further purify the surface of the copper strip; the pickling solution includes sulfuric acid, hydrochloric acid or nitric acid; S4: After the pickling treatment, the copper strip needs to be washed with water to remove the residual pickling solution; then, the copper strip is neutralized with a neutralizer to remove the residual acidic substances and avoid corrosion to the copper strip; S5: After the neutralization treatment, the surface of the copper strip is chemically corroded. Through chemical corrosion, a layer of tiny bumps is formed on the surface of the copper strip. These bumps reduce the glossiness of the surface of the copper strip, making it more matte. S6: After chemical etching, the copper strip needs to be washed with water to remove the residual etching solution; then, the copper strip is dried to remove moisture and avoid leaving water marks on the surface of the copper strip; S7: In order to further improve the performance of the copper strip, post-treatment is performed, including passivation treatment and coating treatment; S8: Finally, the treated copper strips are inspected for appearance and tested for performance to ensure that they meet the requirements. Then, the qualified copper strips are packaged to prevent contamination and damage during transportation and storage.
2. A method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In the step S1, the degreasing treatment uses acetone, isopropanol or n-hexane organic solvent, or uses sodium hydroxide, potassium hydroxide alkaline solution; in the degreasing process, for organic solvent degreasing, the copper strip is immersed in the solvent, the temperature is controlled between room temperature and 50°C, and the immersion time is 5-10 minutes; for alkaline solution degreasing, the copper strip is immersed in 5%-10% sodium hydroxide solution, the temperature is controlled between 60-80°C, and the immersion time is 10-30 seconds.
3. A method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In step S2, during water washing, spraying, immersion or brushing is adopted to ensure that the degreaser and loose dirt on the surface of the copper strip are thoroughly cleaned; the water washing temperature is controlled between room temperature and 40° C., and the washing time is 5-10 seconds.
4. A method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In step S3, the pickling solution commonly used in the pickling treatment includes sulfuric acid, hydrochloric acid or nitric acid; 5%-10% sulfuric acid solution, 5%-10% hydrochloric acid solution or 5%-10% nitric acid solution is used for pickling; during the pickling process, the concentration, temperature and time of the pickling solution need to be controlled; the pickling temperature is controlled between room temperature and 60°C, and the time is 1-2 minutes; after pickling, it is necessary to perform a thorough water wash to remove the residual pickling solution.
5. The method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In the step S4, after washing with water, the copper strip is neutralized with a neutralizer to remove residual acidic substances; the neutralizer includes an alkaline solution of sodium hydroxide and potassium hydroxide; the copper strip is immersed in a 5%-10% sodium hydroxide solution, the temperature is controlled between room temperature and 40°C, and the immersion time is 1-2 minutes; after neutralization, it is necessary to wash thoroughly with water to remove the residual neutralizer.
6. A method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In step S5, 5%-10% hydrochloric acid solution or 5%-10% nitric acid solution is used for corrosion; during the electrochemical corrosion process, the concentration, temperature and time of the corrosion solution need to be controlled; the corrosion temperature is controlled between room temperature and 50°C, and the time is 3-5 minutes; after corrosion, it is necessary to perform a thorough water wash to remove the residual corrosion solution.
7. A method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In step S6, after washing, the copper strip is dried to remove moisture, and the copper strip is placed in a well-ventilated place to dry naturally, or is dried using a hot air dryer at a temperature of 100-150° C. for 5-30 minutes.
8. The method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In the step S7, a passivation treatment is performed, using a chromic acid, phosphate or silicate passivation solution to treat the copper strip to improve its corrosion resistance.
9. The method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In the step S7, after passivation, a coating treatment is performed, for example, epoxy coating, polyurethane coating or acrylic coating is used to coat the copper strip to improve its wear resistance and solderability.
10. The method for reducing the surface gloss of a copper strip according to claim 1, characterized in that: In step S8, the performance tests include tensile strength, elongation, hardness, corrosion resistance and solderability; after passing the test, the copper strip is packaged by winding, vacuum packaging or mildew-proof packaging.