Preparation method of ZnCdS / PVDF (Polyvinylidene Fluoride) material for treating printing and dyeing wastewater, ZnCdS / PVDF material and application of ZnCdS / PVDF material
Through the combination of ZnCdS and PVDF materials, ZnCdS/PVDF films were prepared by hydrothermal method and solvent sol method, which solved the problems of low solar energy utilization and photochemical instability of photocatalytic materials in printing and dyeing wastewater treatment, and achieved efficient photocatalytic and Improved piezoelectric performance.
Patent Information
- Application Number
- CN202410941068.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
In the treatment of printing and dyeing wastewater, existing photocatalytic materials have problems such as low solar energy utilization rate, lack of obvious quantum effects, inability to effectively separate photogenerated electron-holes, and photochemical instability.
ZnCdS and PVDF materials were used to prepare ZnCdS samples by hydrothermal method, and ZnCdS/PVDF materials were prepared by solvent sol method. Combined with ultrasonic treatment and drying technology, a thin film with high efficiency photocatalytic activity was formed.
The photocatalytic activity is significantly improved within the visible light range. ZnCdS/PVDF-10 exhibits better photocatalytic activity, and promotes the generation of β phase in PVDF, improves piezoelectric properties, and solves the photocatalysis in the original technology Problems of instability and low electron-hole separation efficiency.
Smart Images

Figure CN118892869A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of photocatalytic material preparation, and in particular to a preparation method of a ZnCdS / PVDF material for printing and dyeing wastewater treatment, a ZnCdS / PVDF material and an application thereof. Background Art
[0002] Photocatalytic technology can effectively remove organic pollutants and harmful bacteria from water by using sunlight as a driving force. It is easy to operate, clean energy and does not produce secondary pollution, which has brought revolutionary changes to the field of water treatment. Piezoelectric catalytic technology uses the electric field generated by piezoelectric materials under mechanical stress to further promote the catalytic reaction. This technology can not only carry out catalytic reactions without the need for external power supply, but also is efficient and stable, providing new possibilities for sewage treatment. When photocatalysis and piezoelectric catalytic technologies work together, they can complement and promote each other to achieve a more significant sewage purification effect. The clean energy and efficient degradation ability provided by photocatalytic technology, combined with the efficient and stable piezoelectric catalytic technology, can achieve efficient, rapid and thorough treatment of sewage. This synergistic effect not only improves the efficiency of sewage treatment, but also further reduces the treatment cost, bringing huge application potential to the field of environmental purification. Therefore, the method of synergistic sewage treatment by photocatalysis and piezoelectric catalysis has become an important development direction in the current and future sewage treatment field with its unique advantages and broad application prospects, and this combination technology will play a more important role in future environmental governance.
[0003] Organic piezoelectric materials are generally more flexible than traditional inorganic piezoelectric materials. Due to its significant piezoelectric coefficient, PVDF is considered an ideal candidate material that can work synergistically with photocatalysts to generate an influential electric field environment. At present, studies have achieved efficient piezoelectric photocatalytic degradation of RhB by dispersing ZnO nanorods on PVDF and driving it with water flow induced by magnetic stirring. A 99% RhB removal rate was achieved within 100 minutes, which is significantly higher than the 59% removal effect when relying solely on photocatalysis. The pioneering research of BAGCHI et al. revealed that with the assistance of ultrasound, MoS2 / PVDF films can effectively decompose various dyes even in the absence of light and show excellent renewable performance.
[0004] Photocatalytic technology has become a useful way to solve the energy crisis and environmental pollution problems, and there are many scientific research results. However, in the photocatalytic degradation of printing and dyeing wastewater, the above materials have problems such as low solar energy utilization, unclear quantum effect, ineffective separation of photogenerated electrons and holes, and photochemical instability. Summary of the invention
[0005] The present invention provides a preparation method of a ZnCdS / PVDF material for treating printing and dyeing wastewater, a ZnCdS / PVDF material and an application thereof, aiming to solve the above-mentioned problems existing in the background technology.
[0006] The technical solution provided by the present invention is as follows:
[0007] The first aspect of the present invention provides a method for preparing a ZnCdS / PVDF material for treating printing and dyeing wastewater, comprising the following steps:
[0008] Dissolve cadmium acetate dihydrate, zinc acetate dihydrate and thioacetamide in deionized water in sequence, and stir evenly to obtain a first solution;
[0009] Adding NaOH solution to the first solution and stirring to form a suspension;
[0010] The suspension is subjected to hydrothermal treatment, washed alternately with deionized water and alcohol for multiple times, and then dried to obtain a ZnCdS sample;
[0011] The PVDF is mixed with the ZnCdS sample and N,N-dimethylformamide respectively, and stirred to form a sol;
[0012] The sol is subjected to ultrasonic treatment, and the sol is evenly spread to form a film using a doctor blade. After the film is formed, it is dried and cooled to room temperature in sequence to obtain the ZnCdS / PVDF material.
[0013] Further, the cadmium acetate dihydrate and the zinc acetate dihydrate are both 10 mmol;
[0014] The amount of the thioacetamide is 25 mmol.
[0015] Furthermore, the concentration of the NaOH solution is 4 mol / L.
[0016] Further, the suspension is subjected to hydrothermal treatment, washed alternately with deionized water and alcohol for multiple times, and then dried to obtain a ZnCdS sample, specifically:
[0017] The suspension was placed in a high-pressure reactor, and then placed in a drying oven for hydrothermal treatment, with the temperature set at 180°C and the time set at 8 hours. After the autoclave was at room temperature, it was taken out, and washed alternately with deionized water and alcohol three times, and then placed in an oven for drying again, with the temperature set at 80°C and the time set at 5 hours, to obtain the ZnCdS sample.
[0018] Furthermore, the mass fraction of the ZnCdS sample in the sol is 5%, 10%, 15%, 20%, 30%, 35% or 45%.
[0019] Further, the mass of the PVDF is 0.5 g, and the mass of the ZnCdS sample is 0.0265 g, 0.0556 g, 0.0882 g, 0.1250 g, 0.2143 g, 0.2692 g or 0.4090 g;
[0020] The volume of the N,N-dimethylformamide is 5 ml.
[0021] Further, the sol is subjected to ultrasonic treatment, and the sol is evenly spread to form a film using a doctor blade, and after the film is formed, it is dried and cooled to room temperature in sequence to obtain the ZnCdS / PVDF material, specifically:
[0022] The sol was placed in an ultrasonic instrument for 3 hours, and then the sonicated sol was poured onto a coated glass plate. The scraper was set to 0.3 mm, and the sol was evenly spread into a film using the scraper. The film was placed in a drying oven at 60° C. for 3 hours, and cooled to room temperature to finally obtain the ZnCdS / PVDF material.
[0023] The second aspect of the present invention provides a ZnCdS / PVDF material obtained by the above-mentioned method for preparing the ZnCdS / PVDF material for treating printing and dyeing wastewater.
[0024] The third aspect of the present invention provides the use of the above-mentioned ZnCdS / PVDF material in the preparation of a ZnCdS / PVDF piezoelectric sensor.
[0025] A fourth aspect of the present invention provides the use of the above-mentioned ZnCdS / PVDF material in the photocatalytic degradation of printing and dyeing wastewater.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The invention prepares ZnCdS / PVDF material by mixing ZnCdS and PVDF. First, the semiconductor material ZnCdS is prepared by a hydrothermal method, and then the ZnCdS / PVDF material is prepared by a solvent sol method. The piezoelectric effect of the PVDF film and the photocatalytic degradation efficiency of the mixed film of ZnCdS and PVDF are analyzed and tested. Then, the catalytic degradation performance of the ZnCdS / PVDF catalytic film with different proportions on rhodamine B under simulated visible light irradiation is studied with the ZnCdS / PVDF material as the object and RhB as the target pollutant. Then, on the basis of preparing the ZnCdS / PVDF material, the photoelectric performance of the composite material is empirically analyzed, the piezoelectric effect of the composite material is tested by a piezoelectric performance test, and the feasibility of the material prepared by the research experiment is confirmed by photoelectric performance tests such as high-power scanning electron microscopy, X-ray diffraction, infrared spectroscopy, electron paramagnetic resonance, ultraviolet diffuse reflection, impedance and electron spin resonance. The results show that the ZnCdS / PVDF material prepared by the present invention exhibits efficient photocatalytic activity in the visible light range, and the ZnCdS / PVDF material has reached the condition range for degradation of dye molecules using visible light, and ZnCdS / PVDF-10 has a more superior photocatalytic activity; at the same time, the addition of the ZnCdS material promotes the generation of the β phase in PVDF, thereby improving the piezoelectric properties of the ZnCdS / PVDF material. The existing technology solves the problems of low solar energy utilization, unclear quantum effect, ineffective separation of photogenerated electrons and holes, and photochemical instability in the process of printing and dyeing wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The SEM images of ZnCdS / PVDF-20 at different magnifications in the embodiments of the present invention, wherein (a) 1 μm, (b) 300 nm, (c) 100 nm, and (d) grain size statistics;
[0029] Figure 2 The XRD spectra of ZnCdS / PVDF material samples with different ratios and the XRD spectra of pure PVDF samples in the embodiments of the present invention, wherein (a) the XRD spectra of ZnCdS / PVDF material samples with different ratios, (b) the XRD spectra of pure PVDF samples;
[0030] Figure 3 The infrared spectra of ZnCdS / PVDF material samples with different ratios prepared in the embodiments of the present invention are shown;
[0031] Figure 4 The EPR spectrum of the ZnCdS / PVDF-20 thin film material sample prepared in the embodiment of the present invention;
[0032] Figure 5The UV-visible diffuse reflectance spectra of the ZnCdS / PVDF material samples of different ratios prepared in the embodiments of the present invention and the Tauc plots of the ZnCdS / PVDF material samples of different ratios, wherein (a) is the UV-visible diffuse reflectance spectra of the ZnCdS / PVDF material samples of different ratios; (b) is the Tauc plot of the ZnCdS / PVDF material samples of different ratios;
[0033] Figure 6 The impedance spectra of ZnCdS / PVDF material samples with different ratios prepared in the embodiments of the present invention are shown;
[0034] Figure 7 (a) is the UV-visible absorption spectra of RhB degradation by samples with different ratios; (b) is the photocatalytic activity diagram of RhB degradation by samples with different ratios; (c) is the first-order kinetic fitting curve diagram of samples with different ratios; (d) is the degradation rate comparison diagram of samples with different ratios;
[0035] Figure 8 The ESR spectrum of the ZnCdS / PVDF-20 thin film material sample prepared in the embodiment of the present invention: (a) ·OH; (b) (c)h + ; (d) Comparison of different active substances after 10 min of reaction;
[0036] Fig. 9 This is a current diagram of a piezoelectric sensor made of ZnCdS / PVDF materials with different ratios prepared in an embodiment of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the embodiments described below are part of the embodiments of the present application, not all of the embodiments.
[0038] Therefore, the detailed description of the embodiments of the present application provided below in conjunction with the accompanying drawings is intended to represent only selected embodiments of the present application, and is not intended to limit the scope of protection claimed in the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
[0039] Example 1
[0040] This embodiment provides a method for preparing a ZnCdS / PVDF material for treating printing and dyeing wastewater, including two steps of preparing a ZnCdS sample and preparing a ZnCdS / PVDF material.
[0041] 1.1 Preparation of ZnCdS samples
[0042] ZnCdS is synthesized by hydrothermal reaction. 2665.3 mg of cadmium acetate dihydrate (10 mmol), 2195.1 mg of zinc acetate dihydrate (10 mmol) and 1878.3 mg of thioacetamide (25 mmol) were dissolved in 40 mL of deionized water in turn, and stirred on a magnetic stirrer for 15 min to form a transparent and uniform mixed solution; then, 1.6 g of NaOH was weighed and dissolved in 10 mL of deionized water to prepare a 4 mol / L solution, and the prepared NaOH solution was quickly added to the mixed solution, and the mixed solution quickly turned into a thick yellow solution. Continue stirring for 30 min to ensure the formation of a uniform suspension; then put the suspension into a high-pressure reactor and put it into a drying oven for hydrothermal treatment, setting the temperature to 180 ° C for 8 hours, and then take it out after the high-pressure reactor reaches room temperature, wash it with deionized water and alcohol alternately three times, and put it into the oven again to dry, setting the temperature to 80 ° C for 5 hours to obtain the final ZnCdS sample.
[0043] 1.2 Preparation of ZnCdS / PVDF materials
[0044] PVDF was mixed with ZnCdS samples of different masses and N,N-dimethylformamide to prepare ZnCdS / PVDF materials with different ratios.
[0045] In this embodiment, the above specific operation is: 0.5g of PVDF and 0.0265g, 0.0556g, 0.0882g, 0.1250g, 0.2143g, 0.2692g, 0.4090g of ZnCdS samples were mixed with 5ml of N, N-dimethylformamide, and placed in a magnetic stirrer for 2h to form a uniform particle-free sol (5%, 10%, 15%, 20%, 30%, 35%, 45%); then the uniformly stirred sol was placed in an ultrasonic instrument for 3h; the sol was poured onto a smeared glass plate, and scraped The mold knife was set at 0.3 mm, and a scraper was used to evenly spread the sol into a film; and dried in a drying oven at 60°C for 3 h, cooled to room temperature, and finally obtained ZnCdS / PVDF materials with different proportions (5%, 10%, 15%, 20%, 30%, 35%, 45%), recorded as ZnCdS / PVDF-5, ZnCdS / PVDF-10, ZnCdS / PVDF-15, ZnCdS / PVDF-20, ZnCdS / PVDF-30, ZnCdS / PVDF-35, ZnCdS / PVDF-45.
[0046] Example 2
[0047] This embodiment provides a method for preparing a ZnCdS / PVDF piezoelectric sensor, specifically:
[0048] The PDMS and ZnCdS / PVDF films were cut into pieces of the same size, and then the PDMS film was pasted on the smooth side of the ZnCdS / PVDF film to obtain PDMS-ZnCdS / PVDF. Copper tapes were then pasted on the upper and lower surfaces as copper electrodes, and two wires were led out to prepare the ZnCdS / PVDF piezoelectric sensor.
[0049] Example 3 Performance Test
[0050] 3.1 Determination of piezoelectric properties
[0051] In this example, the piezoelectric properties of the ZnCdS / PVDF material prepared in Example 1 were tested on an electrochemical workstation.
[0052] Preparation method of working electrode: Cut the ZnCdS / PVDF material and PDMS prepared in Example 1 into pieces of the same size, and then paste the PDMS film on the smooth side of the ZnCdS / PVDF film to obtain PDMS-ZnCdS / PVDF. Then paste copper tape on the upper and lower surfaces as copper electrodes, lead out two wires, and prepare a piezoelectric sensor. Use a linear reciprocating machine to apply vertical pressure to the PDMS-ZnCdS / PVDF composite film, and the pressure is about 8N. Connect the two wires in the electrochemical workstation to the piezoelectric sensor, select the it Amperometric it Curve function on the CH instruments software, set the sampling interval to 0.1, the running time to 300s, the static time to 0, and the sensitivity to 1.0e -6 .
[0053] 3.2 Characterization of samples
[0054] High-magnification scanning electron microscope (SEM) spectra were obtained using Gemini 300, ZEISS; X-ray powder diffraction (XRD) spectra of the samples were obtained using BrukerD8 Advance X-ray diffractometer; infrared spectrum images (FTIR) of the samples were obtained using Nicolet NEXUS670 infrared transform spectrometer; electron paramagnetic resonance (EPR) spectra were obtained using Bruker A300; ultraviolet-visible diffuse reflectance spectra (UV-vis DRS) of the samples were obtained using Shimadzu, UV 3600 transmission spectrophotometer; impedance information of the samples was tested using Shanghai Chenhua CHI760E electrochemical workstation; electron spin resonance (ESR) spectra were obtained using BrukerA300.
[0055] 3.3 Determination of photocatalytic performance
[0056] A photocatalytic reaction apparatus produced by Beijing Zhongjiao Jinyuan Technology Co., Ltd. was used, and the light source was a CEL-HXF300 xenon lamp as the device for the photocatalytic reaction, and the diameter of the light source was about 56 mm. A 50 mL conical bottle was used as the photocatalytic reactor, and the bottle mouth was 6 cm away from the light source.
[0057] Experimental steps for photocatalytic degradation: First, prepare a 20-fold diluted Rhodamine B solution. The concentration of the solution prepared in the laboratory is 400 mg / L, and the concentration of the solution required for the experiment is 20 mg / L. Therefore, the ratio of the original concentration solution to water is 1:19. The 7 samples are sorted from small to large according to the ZnCdS content ratio and prepared in groups. The first group has a content of 5%, 10%, and 15%, and the second group has a content of 20%, 30%, 35%, and 45%. Take 10ml of the original solution and 190ml of water together to prepare a 200ml solution, put a magnetic stirrer and stir. Prepare a solution slightly more than 200ml, take 0.8ml of the solution in a centrifuge tube, and then use a measuring cylinder to weigh 50ml of the solution in turn and pour it into a conical flask marked with a number. At this time, the magnetic should be in the conical flask. The preparation method of the second group of solutions is the same as above.
[0058] Weigh 50 mg of the ZnCdS / PVDF material sample prepared in Example 1 and cut it into pieces. Prepare 7 samples of different proportions, record and label them. Then pour the drugs into conical flasks with corresponding digital labels. Take 0.8 mL of solution for stock solution comparison. Place two groups of conical flasks containing film materials and Rhodamine B solution on a magnetic stirrer for stirring, wrap the conical flasks with tin foil to create a dark reaction environment, so that the photocatalyst and Rhodamine B solution reach adsorption equilibrium. After the dark reaction is completed, use a pipette to transfer 0.8 mL of solution into a centrifuge tube. Continue to divide the samples into two groups. Put the conical flasks into the ultrasonic machine according to the labels. Turn on the xenon light source switch, set the time to 180 minutes, take samples once every 30 minutes, and conduct photocatalytic degradation experiments. The ultrasonic machine works at 100% power and controls the temperature within 26°C.
[0059] Use a pipette to inject 2.4 ml of deionized water into each of the 7 groups of samples, pour the stock solution and all samples into the cuvette in order, use Morpho software to analyze and save the data, and use Origin software to process the data and make graphic analysis.
[0060] 3.4 Photoelectric performance test
[0061] Electrochemical impedance was detected on an electrochemical workstation (CHI660E, Shanghai Changhua Instrument Co., Ltd.). The photoelectrochemical properties of the samples were tested using a typical three-electrode (working electrode, reference electrode and counter electrode) configuration. For the working electrode, the prepared ZnCdS / PVDF materials of different proportions were cut into appropriate sizes and pasted on conductive glass with double-sided carbon conductive tape. The reference electrode was a calomel electrode, and the counter electrode was a platinum wire. The electrolyte was prepared from a 0.2M Na2SO4 solution. A 300W xenon lamp (CEL-HXF300) with a 420nm UV filter was used to simulate sunlight.
[0062] Example 4 Results and Analysis
[0063] 4.1 Optical performance analysis
[0064] 4.1.1 SEM image analysis
[0065] The geometry, size, microstructure and distribution of ZnCdS / PVDF film samples were investigated by high-magnification scanning electron microscopy (SEM) tests. Figure 1 As shown in (a) and (b), the prepared ZnCdS is uniformly distributed on the surface of the PVDF film in the form of nanoparticles. This avoids the local agglomeration of the ZnCdS complex, which is beneficial for the ZnCdS complex to expose a larger specific surface area, increase more reactive sites, and thus improve the photocatalytic reaction activity. The ZnCdS / PVDF-20 film sample was magnified for observation, as shown in Figure 1. Figure 1 As shown in (c), the film sample exhibits ZnCdS nanoparticles of different sizes, with an average particle size of about 60nm. At the same time, these particles do not have a specific geometric shape. Due to the different sizes, the total specific surface area of the material increases, and small grains usually have a quantum size effect, which may cause the light absorption of the material to extend to the visible light or even the near-infrared region. Therefore, the ZnCdS composite can better utilize sunlight and improve the photocatalytic efficiency. In addition, homogeneous heterojunctions may be formed between grains of different sizes, which helps to promote the separation of electrons and holes and reduce their recombination, thereby improving the quantum efficiency of the photocatalytic reaction.
[0066] 4.1.2 XRD pattern analysis
[0067] X-ray diffraction (XRD) is often used to analyze the phase characteristics of samples. XRD is used to detect the structure and composition of ZnCdS / PVDF material samples. Figure 2 They respectively represent the XRD patterns of ZnCdS / PVDF material samples with different ratios and the XRD patterns of pure PVDF film material samples. Figure 2(a) It can be seen that three characteristic peaks appear at 2θ=27.65°, 45.73° and 54.22°. After comparison with other references, it is found that they are located on the (102), (110) and (200) crystal planes, corresponding to the characteristic peaks of ZnCdS, which can prove the presence of ZnCdS in the ZnCdS / PVDF material sample. Figure 2 (b) It can be seen that pure PVDF has α characteristic peaks at 2θ=13.14° and 28.3°, corresponding to the crystal planes (100) and (021), and β characteristic peaks at 2θ=20°, corresponding to the crystal plane (002), proving the presence of PVDF in the ZnCdS / PVDF material sample. According to the spectrum analysis, the ZnCdS / PVDF material sample has been successfully prepared. Comparison of ZnCdS / PVDF material samples with different proportions shows that there is no characteristic peak shift, and after adding ZnCdS, the peak intensity range is expanded from 200-1200 to 20000-100000, and the β peak of PVDF is significantly enhanced, indicating that ZnCdS has a promoting effect on the formation of β phase in PVDF.
[0068] 4.1.3 Infrared spectroscopy analysis
[0069] Infrared analysis can determine the surface material and chemical bonds of the prepared samples. Figure 3 The infrared spectra (FTIR) of ZnCdS / PVDF materials with different ratios are shown in the figure. -1 The place is The out-of-plane swing peak of the group. At 833-872cm -1 The out-of-plane bending peak of the COH group at 1163 cm -1 The peak at 1404cm is the contraction vibration peak of the CO(H) group. -1 The peak at 3035cm is the bending vibration peak of the CH hydrogen-containing group, where CH2 is clustered. -1 Nearby is the stretching vibration absorption peak of OH. The OH bonds are associated within the molecule, indicating the aggregation of water molecules.
[0070] 4.1.4 EPR spectrum analysis
[0071] like Figure 4The electron paramagnetic resonance (EPR) spectrum of the ZnCdS / PVDF-20 film sample is shown. The oxygen vacancies or electrons trapped in the oxygen vacancies at g = 2.004 are only generated by the oxidative active substances after the ZnCdS complex generates electrons under light conditions. Oxygen vacancies, as a crystal defect, can act as reactive sites during the reaction. When light is irradiated to the surface of the ZnCdS complex, photogenerated electrons and holes are generated. These photogenerated electrons can be captured by oxygen vacancies or other defects and participate in subsequent redox reactions. The presence of captured electrons helps promote the photocatalytic reaction and improve the reaction rate and efficiency.
[0072] 4.1.5 UV-Vis Diffuse Reflectance Spectroscopy Analysis
[0073] Figure 5 It is the UV-visible diffuse reflectance spectrum, which can test the light absorption performance of the catalyst. The optical properties of the sample are analyzed using the UV-visible diffuse reflectance spectrum. The ZnCdS / PVDF materials of different ratio series have high visible light absorption intensity in the range of 200-900nm. The absorption band edge of ZnCdS / PVDF-45 is about 468nm. There is no obvious shift in the absorption band edge. The band gap width of the sample can be calculated according to formula (1):
[0074]
[0075] α is the absorption coefficient, h is Planck's constant, υ is the frequency, A is a constant, E g is the bandgap width. The value of n depends on the type of semiconductor. When the semiconductor has a direct bandgap, n = 1 / 2, and when it has an indirect bandgap, n = 2. Figure 5 .Depend on Figure 5 (a) It can be seen that the absorption edges of ZnCdS / PVDF under different ratios are similar, and Figure 5 (b) shows that the band gap width calculated by the Tauc-plot method is between 2.44eV and 2.56eV. The band gap width of the photocatalytic water splitting reaction under visible light is not less than 1.23eV. This shows that the ZnCdS / PVDF material sample has reached the condition range for water splitting using visible light.
[0076] 4.1.6 Electrochemical impedance spectroscopy
[0077] Electrochemical impedance spectroscopy (EIS) was used to infer that photogenerated charge transfer occurred between ZnCdS and PVDF.
[0078] Electrochemical impedance spectroscopy (EIS) can verify the charge transfer during the photocatalytic process. In the EIS spectrum, the smaller the arc radius, the lower the electrochemical impedance, indicating that the conductivity of the material is stronger, which is conducive to the rapid transmission of electrons. Figure 6 The impedance spectra of ZnCdS / PVDF material samples with different ratios are shown in Figure 2. Figure 6 The results show that the arc radius is smaller in ZnCdS / PVDF-10, which indicates that under visible light irradiation, the resistance of electrons is smaller, so the electrons migrate to the surface of the material faster. This also further verifies that ZnCdS / PVDF-10 has superior photocatalytic activity.
[0079] 4.2 Performance analysis of photocatalytic degradation of RhB
[0080] During the photocatalytic process, the degradation rate (D) and first-order reaction rate constant (K) of RhB can be calculated by formulas (2) and (3):
[0081] D=(1-C / C0)×100% (2)
[0082] -Ln(C / C0)=Kt (3)
[0083] Where C0 and C represent the initial dye concentration and the concentration after different reaction times, respectively.
[0084] Figure 7 (a) shows the UV-visible absorption spectra of RhB degraded by samples with different ratios. Figure 7 (a) It can be seen that the wavelength of the maximum absorbance of RhB is 533.48nm; Figure 7 (b) The photocatalytic activity diagram of RhB degradation of samples with different ratios. Figure 7 (b) It can be seen that the self-degradation of RhB is not obvious when the ZnCdS content is lower than 45%. When the sample content is lower than 45%, the concentration of Rhodamine B catalyzed within 30 minutes of dark reaction adsorption is also not obvious, indicating that the ZnCdS content has little effect on the self-degradation and dark reaction adsorption of Rhodamine B in the catalytic process. The ZnCdS / PVDF material cannot completely degrade RhB within 30 minutes. When the ZnCdS content is 20%, the degradation efficiency of RhB within 90 minutes of light reaction is the highest, which is 75.8%. Figure 7 (c) is the first-order kinetic fitting curve of RhB degradation of different samples obtained by -Ln(C / C0) curve fitting. Figure 7 (c) It can be seen that the degradation rate of ZnCdS / PVDF material is the fastest when the ZnCdS content is 20%; Figure 7 (d) is the comparison of degradation rates of samples with different proportions. Figure 7(d) It can be seen that with the increase of ZnCdS content, the reaction rate shows a trend of first increasing and then decreasing. When the content is 20%, the degradation rate is the fastest, which is 0.0065min. -1 Therefore, the ZnCdS / PVDF material prepared by the present invention has the fastest degradation rate of RhB when the ZnCdS content is 20%. Compared with the existing related materials, the material is more suitable for the treatment of printing and dyeing wastewater.
[0085] 4.3 ESR spectrum analysis
[0086] In order to explore the main active substances in the reaction process and investigate the carrier dynamics and mechanism, electron spin resonance (ESR) technology was used to analyze superoxide radicals ( Hydroxyl radicals (·OH) and holes (h + ) for detection and analysis. DMPO reagent was used to capture ·OH during the photoreaction process. Figure 8 As shown in (a), after 1min, 5min, and 10min of light irradiation, characteristic peaks with a peak intensity ratio of 1:2:2:1 appeared, which belongs to the DMPO-·OH signal. Figure 8 As shown in (b), DMPO reagent was used to The peak intensity ratio of 1:1:1:1 was observed. The results show that during the photocatalytic reaction, active substances and ·OH, and their respective peaks increase with reaction time, indicating an increase in the amount of active substances generated. Figure 8 As shown in (c), TEMPO is a nitroxide free radical with a stable unpaired electron that can be detected by ESR. The electrons generated by the photocatalytic reaction are captured by TEMPO, making it neutral, causing the paramagnetic signal to disappear. Therefore, the strength of the TEMPO signal can be used to detect h + Under light irradiation, the TEMPO signal intensity ratio is 1:1:1, and the peak intensity gradually increases with the increase of light irradiation. The longer the illumination time, the stronger the corresponding peak intensity, indicating that the less electrons are continuously generated by light irradiation, and the corresponding h + Therefore, h + It does not act as the main reactive substance in the reaction process. To compare the main active substances in the reaction process, we compared the peak intensities of the three active substances after 10 minutes of light reaction. It is very obvious. The sequential signal of is higher than that of ·OH, which is the main reactive substance in this study system. In summary, under the light condition, more and more ·OH and The appearance of indicates that the ZnCdS heterojunction generates more and more electrons and holes, which is mainly attributed to the large specific surface area and the effective improvement of visible light absorption, which promotes the separation of photogenerated electrons and holes. In addition, the ESR analysis results confirm that in the process of photocatalytic degradation of Rhodamine B, It plays a major role, and ·OH plays a supporting role.
[0087] 3.4 Piezoelectric performance analysis
[0088] The piezoelectric sensor was prepared using PVDF composite film, and the output performance of the sensor was measured on an electrochemical workstation. Fig. 9 The current generated by the sensor by applying vertical pressure is given in Fig. 9 As shown in the figure, with the increase of the percentage of ZnCdS in the material, the piezoelectric current of the ZnCdS / PVDF composite film at 30% is the largest, which is 1.2μA. Combined with the XRD spectrum analysis, the results show that the addition of ZnCdS material promotes the generation of β phase in PVDF, thereby improving the piezoelectric properties of the composite film.
[0089] The above is only the best specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions within the technical scope disclosed in the present application shall be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing a ZnCdS / PVDF material for treating printing and dyeing wastewater, characterized in that: The following steps are involved: Dissolving cadmium acetate dihydrate, zinc acetate dihydrate and thioacetamide in deionized water in sequence, and stirring evenly to obtain a first solution; Adding NaOH solution to the first solution and stirring to form a suspension; The suspension is subjected to hydrothermal treatment, washed alternately with deionized water and alcohol for multiple times, and then dried to obtain a ZnCdS sample; The PVDF is mixed with the ZnCdS sample and N,N-dimethylformamide respectively, and stirred to form a sol; The sol is subjected to ultrasonic treatment, and the sol is evenly spread to form a film using a doctor blade. After the film is formed, it is dried and cooled to room temperature in sequence to obtain the ZnCdS / PVDF material.
2. The method for preparing the ZnCdS / PVDF material for treating printing and dyeing wastewater according to claim 1, characterized in that: The cadmium acetate dihydrate and the zinc acetate dihydrate are both 10 mmol; The amount of the thioacetamide is 25 mmol.
3. The method for preparing the ZnCdS / PVDF material for treating printing and dyeing wastewater according to claim 1, characterized in that: The concentration of the NaOH solution is 4 mol / L.
4. The method for preparing the ZnCdS / PVDF material for treating printing and dyeing wastewater according to claim 1, characterized in that: The suspension is subjected to hydrothermal treatment, washed alternately with deionized water and alcohol for multiple times, and then dried to obtain a ZnCdS sample, specifically: The suspension was placed in a high-pressure reactor, and then placed in a drying oven for hydrothermal treatment, with the temperature set at 180°C and the time set at 8 hours. After the autoclave was at room temperature, it was taken out, and washed alternately with deionized water and alcohol three times, and then placed in an oven for drying again, with the temperature set at 80°C and the time set at 5 hours, to obtain the ZnCdS sample.
5. The method for preparing the ZnCdS / PVDF material for treating printing and dyeing wastewater according to any one of claims 1 to 4, characterized in that: The mass fraction of the ZnCdS sample in the sol is 5%, 10%, 15%, 20%, 30%, 35% or 45%.
6. The method for preparing the ZnCdS / PVDF material for treating printing and dyeing wastewater according to claim 5, characterized in that: The mass of the PVDF is 0.5 g, and the mass of the ZnCdS sample is 0.0265 g, 0.0556 g, 0.0882 g, 0.1250 g, 0.2143 g, 0.2692 g or 0.4090 g; The volume of the N,N-dimethylformamide is 5 ml.
7. The method for preparing the ZnCdS / PVDF material for treating printing and dyeing wastewater according to claim 5, characterized in that: The sol is subjected to ultrasonic treatment, and the sol is evenly spread to form a film using a doctor blade. After the film is formed, the sol is dried and cooled to room temperature in sequence to obtain the ZnCdS / PVDF material, specifically: The sol was placed in an ultrasonic instrument for 3 hours, and then the sonicated sol was poured onto a coated glass plate. The scraper was set to 0.3 mm, and the sol was evenly spread into a film using the scraper. The film was placed in a drying oven at 60° C. for 3 hours, and cooled to room temperature to finally obtain the ZnCdS / PVDF material.
8. A ZnCdS / PVDF material, characterized in that: The material is obtained by the preparation method of the ZnCdS / PVDF material for treating printing and dyeing wastewater as described in any one of claims 1 to 7.
9. Use of the ZnCdS / PVDF material as claimed in claim 8 in the preparation of a ZnCdS / PVDF piezoelectric sensor.
10. Use of the ZnCdS / PVDF material as claimed in claim 8 in the photocatalytic degradation of printing and dyeing wastewater.