Flotation reagent and preparation method and application thereof

By using flotation agents of alkyl sulfhydrazide, fatty alcohol polyoxyethylene ether and nonionic surfactant in a weak acid slurry environment, the separation of feldspar and quartz is achieved by using mechanical action, and the separation difficulty under neutral pH conditions is solved. The problem of Yamato environmental pollution has improved resource utilization and separation efficiency.

CN118892916AInactive Publication Date: 2024-11-05宜丰国轩锂业有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410931959.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Under neutral pH conditions, the separation of feldspar and quartz is extremely difficult. The existing fluorine- and acid-free methods have been poorly explored in recent years due to their toxicity and environmental destructiveness, resulting in insufficient exploration of fluorine-free and acid-free methods, resulting in feldspar The problem of waste of resources and the reduction of SiO2 content in quartz mines.

Method used

Flotation agents including alkylsulfhydrazides, fatty alcohol polyoxyethylene ethers and nonionic surfactants are used to achieve flotation separation between feldspar and quartz in a weak acid slurry environment through mechanical actions such as hydrogen bonds and covalent bonds. Improve selectivity and efficiency.

Benefits of technology

Effectively separate feldspar and quartz in a weak acid slurry environment, improving the selection efficiency of feldspar, achieving the maximum utilization of ore resources in quartz ore, and being environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004939963360000031
    Figure BDA0004939963360000031
  • Figure BDA0004939963360000041
    Figure BDA0004939963360000041
  • Figure BDA0004939963360000051
    Figure BDA0004939963360000051
Patent Text Reader

Abstract

The invention provides a flotation reagent and a preparation method and application thereof, and relates to the technical field of mineral flotation. The flotation reagent comprises the following raw materials in parts by weight: 3-6 parts of alkyl thiohydrazide, 2-3 parts of fatty alcohol-polyoxyethylene ether and 0.5-1 part of a nonionic surfactant. The preparation method of the flotation reagent comprises the following step of uniformly mixing the alkyl thiohydrazide, the fatty alcohol-polyoxyethylene ether and the nonionic surfactant to obtain the flotation reagent. The prepared flotation reagent can effectively achieve flotation separation of feldspar and quartz in a weak acid ore pulp environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of mineral flotation, and in particular to a flotation agent and a preparation method and application thereof. Background Art

[0002] The reserves of feldspar and quartz are huge in the world, and feldspar and quartz are widely used in the ceramic and glass industries. However, in nature, quartz deposits are usually accompanied by feldspar and silicate minerals such as kaolin, which reduces the SiO2 content in quartz ore and also causes waste of feldspar and other minerals. However, under neutral pH slurry conditions, the physical and chemical properties of feldspar and quartz surfaces are similar, which makes it extremely difficult to separate the two under neutral conditions. At present, there are three main methods for flotation separation of feldspar and quartz: fluorine-containing acid, fluorine-free acid, and fluorine-free and acid-free methods. Although the fluorine-containing acid method has a good separation effect, it is toxic and has great damage to the environment, and it has been gradually banned. In response to the above problems, in recent years, researchers have conducted a large number of exploratory tests on the fluorine-free acid method and the fluorine-free and acid-free method. Among them, the flotation agent for separating feldspar from quartz under fluorine-free weak acid conditions is not only environmentally friendly, but also can significantly improve the separation efficiency of feldspar, which is of great significance to the maximization of ore resource utilization in quartz mines. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a flotation reagent and a preparation method and application thereof.

[0004] The invention provides a flotation reagent, which comprises the following raw materials in parts by weight: 3-6 parts of alkyl sulfhydrazide, 2-3 parts of fatty alcohol polyoxyethylene ether, and 0.5-1 part of nonionic surfactant.

[0005] Preferably, the alkyl sulfhydrazide is selected from one or more of n-hexyl sulfhydrazide and n-octyl sulfhydrazide.

[0006] Preferably, the fatty alcohol polyoxyethylene ether is selected from one or more of lauryl alcohol polyoxyethylene ether and hexadecanol polyoxyethylene ether.

[0007] Preferably, the nonionic surfactant includes dodecyl polyoxyethylene ether and octanol polyoxyethylene ether.

[0008] More preferably, the mass ratio of the dodecyl polyoxyethylene ether to the octanol polyoxyethylene ether is (4-6):(1-3).

[0009] The present invention also provides a method for preparing a flotation reagent, comprising the following steps:

[0010] Alkyl sulfhydrazide, fatty alcohol polyoxyethylene ether and nonionic surfactant are uniformly mixed to obtain a flotation agent.

[0011] Preferably, the method for preparing the flotation agent aqueous solution comprises adding deionized water to the flotation agent to prepare the flotation agent aqueous solution.

[0012] More preferably, the mass fraction of the flotation agent in the flotation agent aqueous solution is 5-10wt%.

[0013] The present invention also provides the use of the flotation agent described in the above technical solution or the flotation agent prepared by the preparation method described in the above technical solution in the flotation separation of feldspar and quartz in a weak acid slurry environment.

[0014] The beneficial effects of the present invention are:

[0015] The flotation reagent of the present invention includes alkyl sulfhydrazide, fatty alcohol polyoxyethylene ether, and nonionic surfactant. The prepared flotation reagent can effectively realize the flotation separation of feldspar and quartz in a weakly acidic pulp environment. In the present invention, the alkyl sulfhydrazide generally contains an alkyl chain, which can form a hydrogen bond or a covalent bond with the hydroxyl group on the surface of the feldspar, thereby realizing chemical adsorption; in addition, the sulfhydrazide functional group may also coordinate with the metal ions on the surface of the feldspar, thereby enhancing its adsorption effect and improving the selectivity of the collector; at the same time, the alkyl chain makes the sulfhydrazide molecule have a certain hydrophobicity, which helps it to form a hydrophobic area on the surface of the feldspar, thereby promoting interaction with the hydrophobic area on the surface of the feldspar, and then adsorption occurs. In the present invention, the fatty alcohol polyoxyethylene ether molecule contains a hydrophilic polyoxyethylene chain, and the hydrophilic polyoxyethylene chain can form a hydrogen bond or hydration with the hydroxyl group on the surface of the feldspar through physical forces such as van der Waals force, thereby realizing physical adsorption. DETAILED DESCRIPTION

[0016] The technical solution of the present invention is described in detail through specific embodiments.

[0017] Unless otherwise specified, the materials, reagents, etc. used in the following examples and comparative examples can be obtained from commercial sources.

[0018] Example 1

[0019] A method for preparing a flotation agent comprises the following steps:

[0020] 60 g of n-hexylsulfhydrazide, 30 g of hexadecyl polyoxyethylene ether and 10 g of a nonionic surfactant are mixed evenly to obtain a flotation agent, and the flotation agent is dissolved in 2 L of deionized water to obtain a 5 wt % flotation agent aqueous solution; wherein the nonionic surfactant is a mixture of dodecyl polyoxyethylene ether and octanol polyoxyethylene ether in a mass ratio of 5:2.

[0021] Taking a quartz sand mine in Fengyang as the ore sample, its chemical composition is shown in Table 1:

[0022] Table 1

[0023]

[0024] The flotation reagent prepared above is used in the flotation separation of feldspar and quartz in a weakly acidic slurry environment. The flotation reagent is used to perform a coarse and fine flotation on the ore sample. The flotation process includes:

[0025] (1) Ore sample pretreatment: crush the ore sample by ball milling, so that the ore sample fineness is less than 0.074 mm, accounting for 15%, and the raw ore after ball milling is screened to remove the fine sand with a fineness of less than 0.074 mm to obtain the raw ore for floating;

[0026] (2) Positive flotation enrichment: add 400g of the raw ore to the flotation tank, add 1200g of tap water to adjust the slurry, stir thoroughly, add sulfuric acid to adjust the slurry to pH 5, then add 420g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is feldspar concentrate, and the product in the flotation tank is quartz rough concentrate; add sulfuric acid to the quartz rough concentrate to adjust the pH to 5 again, then add 150g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is quartz middling ore, and the product in the flotation tank is quartz concentrate;

[0027] The total content of K2O and Na2O in the obtained feldspar concentrate is 9.53%, which meets the standard requirements for industrial preparation of ceramics; the SiO2 content in the obtained quartz concentrate is 99.21%, which meets the standard requirements for materials used in the photovoltaic glass industry (≥99%).

[0028] Example 2

[0029] A method for preparing a flotation agent comprises the following steps:

[0030] 60 g of n-hexylsulfhydrazide, 30 g of hexadecyl polyoxyethylene ether and 10 g of a nonionic surfactant are mixed evenly to obtain a flotation agent, and the flotation agent is dissolved in 2 L of deionized water to obtain a 5 wt % flotation agent aqueous solution; wherein the nonionic surfactant is a mixture of dodecyl polyoxyethylene ether and octanol polyoxyethylene ether in a mass ratio of 5:2.

[0031] Taking a kaolin mine in Yichun as the ore sample, its chemical composition is shown in Table 2:

[0032] Table 2

[0033]

[0034] The flotation reagent prepared above is used in the flotation separation of feldspar and quartz in a weakly acidic slurry environment. The flotation reagent is used to perform a coarse and fine flotation on the ore sample. The flotation process includes:

[0035] (1) Ore sample pretreatment: The ore sample is crushed and ball-milled to make the ore sample with a fineness less than 0.074 mm account for 16%, and the raw ore after ball milling is screened to remove the fine sand with a fineness less than 0.074 mm to obtain the raw ore for floating;

[0036] (2) Positive flotation enrichment: add 400g of the raw ore to the flotation tank, add 1200g of tap water to adjust the slurry, stir thoroughly, add sulfuric acid to adjust the slurry to pH 5, then add 500g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is feldspar concentrate, and the product in the flotation tank is quartz rough concentrate; add sulfuric acid to the quartz rough concentrate to adjust the pH to 5 again, then add 200g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is quartz middling ore, and the product in the flotation tank is quartz concentrate;

[0037] The total content of K2O and Na2O in the obtained feldspar concentrate is 9.21%, which meets the standard requirements for industrial preparation of ceramics; the SiO2 content in the obtained quartz concentrate is 99.56%, which meets the standard requirements for materials used in the photovoltaic glass industry (≥99%).

[0038] Comparative Example 1

[0039] A method for preparing a flotation agent comprises the following steps:

[0040] Take 60g of n-hexylsulfhydrazide and 10g of non-ionic surfactant and mix them evenly to obtain a flotation agent, and dissolve the flotation agent in 1.4L of deionized water to obtain a 5wt% flotation agent aqueous solution; wherein the non-ionic surfactant is a mixture of dodecyl polyoxyethylene ether and octanol polyoxyethylene ether prepared in a mass ratio of 5:2.

[0041] Taking a quartz sand mine in Fengyang as the ore sample, its chemical composition is shown in Table 1:

[0042] Table 1

[0043]

[0044] The flotation reagent prepared above is used in the flotation separation of feldspar and quartz in a weakly acidic slurry environment. The flotation reagent is used to perform a coarse and fine flotation on the ore sample. The flotation process includes:

[0045] (1) Ore pretreatment: crush the ore sample by ball milling, so that the ore sample fineness is less than 0.074 mm, accounting for 15%. The raw ore after ball milling is screened to remove the fine sand with a fineness of less than 0.074 mm to obtain the raw ore for floating;

[0046] (2) Positive flotation enrichment: add 400g of the raw ore to the flotation tank, add 1200g of tap water to adjust the slurry, stir thoroughly, add sulfuric acid to adjust the slurry to pH 5, then add 400g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is feldspar concentrate, and the product in the flotation tank is quartz rough concentrate; add sulfuric acid to the quartz rough concentrate to adjust the pH to 5 again, then add 120g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is quartz middling ore, and the product in the flotation tank is quartz concentrate;

[0047] The total content of K2O and Na2O in the obtained feldspar concentrate is 7.92%, which meets the standard requirements for industrial preparation of ceramics; the SiO2 content in the obtained quartz concentrate is 96.33%, which does not meet the standard requirements for materials used in the photovoltaic glass industry.

[0048] Comparative Example 2

[0049] A method for preparing a flotation agent comprises the following steps:

[0050] 30 g of n-hexylsulfhydrazide and 70 g of hexadecanol polyoxyethylene ether were mixed evenly to obtain a flotation agent, and the flotation agent was dissolved in 2 L of deionized water to obtain a 5 wt % flotation agent aqueous solution.

[0051] Taking a kaolin mine in Yichun as the ore sample, its chemical composition is shown in Table 2:

[0052] Table 2

[0053]

[0054] The flotation reagent prepared above is used in the flotation separation of feldspar and quartz in a weakly acidic slurry environment. The flotation reagent is used to perform a coarse and fine flotation on the ore sample. The flotation process includes:

[0055] (1) Ore pretreatment: ball mill the ore sample to make the ore sample with a fineness less than 0.074 mm account for 16%, and screen the milled ore to remove fine sand with a fineness less than 0.074 mm to obtain the floating ore;

[0056] (2) Positive flotation enrichment: add 400g of raw ore to the flotation tank, add 1200g of tap water to adjust the slurry, stir thoroughly, add sulfuric acid to adjust the slurry to pH 5, then add 480g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is feldspar concentrate, and the product in the flotation tank is quartz rough concentrate; add sulfuric acid to the quartz rough concentrate to adjust the pH to 5 again, then add 180g / t of the above-prepared flotation agent aqueous solution, stir for 4min, and aerate for flotation. The obtained foam product is quartz middling ore, and the product in the flotation tank is quartz concentrate;

[0057] The total content of K2O and Na2O in the obtained feldspar concentrate is 8.56%, which meets the standard requirements for industrial preparation of ceramics; the SiO2 content in the obtained quartz concentrate is 97.43%, which does not meet the standard requirements for materials used in the photovoltaic glass industry.

[0058] In summary, the flotation agent provided by the present invention is used in the flotation separation of feldspar and quartz in a weakly acidic slurry environment. The flotation agent is used to perform coarse and fine positive flotation on the ore sample. The total content of K2O and Na2O in the obtained feldspar concentrate meets the standard requirements for industrial preparation of ceramics; the SiO2 content in the obtained quartz concentrate meets the standard requirements for materials used in the photovoltaic glass industry.

[0059] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A flotation reagent, characterized in that: The invention comprises the following raw materials in parts by weight: 3-6 parts of alkyl sulfhydrazide, 2-3 parts of fatty alcohol polyoxyethylene ether and 0.5-1 part of nonionic surfactant.

2. The flotation reagent according to claim 1, characterized in that: The alkyl sulfhydrazide is selected from one or more of n-hexyl sulfhydrazide and n-octyl sulfhydrazide.

3. The flotation reagent according to claim 1, characterized in that: The fatty alcohol polyoxyethylene ether is selected from one or more of lauryl alcohol polyoxyethylene ether and hexadecanol polyoxyethylene ether.

4. The flotation reagent according to claim 1, characterized in that: The nonionic surfactant includes dodecyl polyoxyethylene ether and octanol polyoxyethylene ether.

5. The flotation reagent according to claim 4, characterized in that: The mass ratio of the dodecyl polyoxyethylene ether and the octanol polyoxyethylene ether is (4-6): (1-3).

6. A method for preparing the flotation reagent according to any one of claims 1 to 5, characterized in that: The following steps are involved: Alkyl sulfhydrazide, fatty alcohol polyoxyethylene ether and nonionic surfactant are uniformly mixed to obtain a flotation agent.

7. The preparation method according to claim 6, characterized in that: The method for preparing the flotation reagent aqueous solution comprises adding deionized water into the flotation reagent to prepare the flotation reagent aqueous solution.

8. Use of the flotation agent according to any one of claims 1 to 5 or the flotation agent prepared by the preparation method according to any one of claims 6 to 7 in the flotation separation of feldspar and quartz in a weakly acidic pulp environment.

Citation Information

Patent Citations

  • Chemical mechanical polishing solution for gallium oxide and polishing method

    CN117720858A