Green light-imitating chromium treatment process for aluminum alloy base material

Through the green photochromium treatment process of aluminum alloy substrates, including cleaning treatment, UV spraying and PVD coating, the problems of high cost of electroplating CP of aluminum alloy substrates in the prior art, poor hexavalent chromium emission and corrosion resistance are solved, and the problem of high cost of electroplating CP in the existing technology is achieved. Low-cost, environmentally friendly imitation chrome products to meet functional testing requirements.

CN118892980APending Publication Date: 2024-11-05XIAMEN RUNNER IND CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110098.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The surface treatment process of existing aluminum alloy substrate electroplating CP has high cost and low yield. It involves hexavalent chromium emissions, affects the environment and human health, and has poor corrosion resistance and cannot meet the functional testing requirements.

Method used

A green imitation photochromium treatment process of aluminum alloy substrate, including surface cleaning treatment, spraying treatment agent stand-alone, UV primer spraying, PVD coating and UV topcoat spraying, omitting the water electroplating process, using silicone compound treatment agent and The aluminum wire coating has a cured ultraviolet wavelength of 300-420nm and the coating time is 5 minutes.

Benefits of technology

It has achieved the appearance, color and function of imitation chromium products to meet the requirements, reduce process costs, avoid hexavalent chromium emissions, reduce wastewater treatment costs, and improve corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892980A_ABST
    Figure CN118892980A_ABST
Patent Text Reader

Abstract

The invention discloses a green light-imitating chromium treatment process for an aluminum alloy base material. The green light-imitating chromium treatment process comprises the following steps: S1, cleaning the surface of a product to be sprayed; s2, spraying a treating agent on the cleaned surface, and standing for a certain time; s3, after standing is conducted, UV primer spraying is conducted on the surface; s4, PVD film coating is conducted on the surface sprayed with the primer; and S5, UV finish paint spraying is carried out on the film coating layer. By the adoption of the process, the light-imitating chromium product can meet the requirements for the appearance, color and function of a current electroplated CP product in the aspects of appearance, color and function, compared with the prior art, the water electroplating process is not needed, therefore, the process cost is reduced, discharge of heavy metal such as hexavalent chromium is not involved, and the process is more environmentally friendly and suitable for industrial production. In addition, the wastewater treatment cost is reduced, and in addition, the wastewater treatment agent also has relatively good corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electroplating, and in particular to a green imitation chromium treatment process for an aluminum alloy substrate. Background Art

[0002] At present, the surface treatment process of electroplating CP on aluminum alloy substrates is generally to perform water electroplating before polishing the blank. This process has high cost and low yield in the water electroplating process, and involves the emission of heavy metals such as hexavalent chromium in the electroplating process, which affects the environment and human health, and also increases the cost of wastewater treatment. In addition, the corrosion resistance is poor in the experimental function and cannot meet the corresponding functional test requirements. Summary of the invention

[0003] In view of the above problems, the purpose of the present invention is to provide a green imitation chrome treatment process for aluminum alloy substrates to improve the above problems.

[0004] The embodiment of the present invention provides a green imitation chrome treatment process for an aluminum alloy substrate, which comprises:

[0005] S1, cleaning the surface of the product to be sprayed;

[0006] S2, spraying a treatment agent on the cleaned surface and leaving it to stand for a certain period of time;

[0007] S3, after standing still, spraying UV primer on the surface;

[0008] S4, PVD coating is performed on the surface of the sprayed primer;

[0009] S5, spraying UV topcoat on the coating layer.

[0010] Preferably, in step S1, the cleaning process includes removing stains and dust from the surface of the product to be sprayed.

[0011] Preferably, in step S2, the treating agent is an organosilicon compound, and the standing time is 3-5 minutes.

[0012] Preferably, in step S3, the primer includes paint and thinner; paint: thinner = 5:0-2; the wavelength of ultraviolet rays used for primer curing is 300-420nm.

[0013] Preferably, in step S4, during PVD coating: the evaporation material is aluminum wire or aluminum alloy; the current is 10-40A;

[0014] The coating time is 5 minutes.

[0015] Preferably, in step S5, the primer includes paint and thinner; paint: thinner = 5:0-2; the wavelength of ultraviolet light used for curing the topcoat is 300-420nm.

[0016] Preferably, it also includes:

[0017] S6, performing functional tests on the product surface; the functional tests include corrosion resistance and wear resistance.

[0018] To sum up, in this embodiment, the above-mentioned process is adopted to make the imitation chrome product meet the appearance, color and function requirements of the current electroplated CP products in appearance, color and function. Compared with the prior art, this embodiment does not require a water electroplating process, thereby reducing the cost of the process, and does not involve the emission of heavy metals such as hexavalent chromium, which is more environmentally friendly and reduces the cost of wastewater treatment. In addition, this embodiment also has good corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solution of the present invention, the drawings required for use in the implementation mode will be briefly introduced below. Obviously, the drawings described below are only some implementation modes of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 The present invention provides a schematic flow chart of a green chromium-imitation treatment process for an aluminum alloy substrate. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] See also Figure 1 The embodiment of the present invention provides a green imitation chrome treatment process for aluminum alloy substrates. The application of the process enables the imitation chrome products to meet the appearance, color and function requirements of current electroplating CP products in terms of appearance, color and function, which includes:

[0023] S1, clean the surface of the product to be sprayed.

[0024] Specifically, in this embodiment, the product to be sprayed may be a metal part, especially an aluminum alloy substrate. The cleaning process includes removing stains and dust from the surface of the product to be sprayed, which may be cleaned by washing with water or other physical and chemical methods, and the present invention does not make specific limitations.

[0025] S2, spraying a treatment agent on the cleaned surface and leaving it to stand for a certain period of time.

[0026] In this embodiment, the treatment agent is an organic silicon compound (such as a silane metal treatment agent) that can enhance the bonding force, and the standing time is 3-5 minutes. The organic silicon compound can react chemically on the surface of the product to be sprayed and form a dense protective film, thereby improving the wear resistance and antifouling properties of the surface.

[0027] S3, after standing still, spraying UV primer on the surface.

[0028] The primer includes polyurethane UV paint and thinner; the ratio of the paint to the thinner is 5:0-2.

[0029] After the primer is sprayed, it needs to be cured with ultraviolet light. In this embodiment, the wavelength of the ultraviolet light for curing is 300-420nm.

[0030] S4, PVD coating is performed on the surface of the sprayed primer.

[0031] Among them, during PVD coating, the evaporation material is aluminum wire or aluminum alloy; the current is 10-40A; and the coating time is 5 minutes.

[0032] S5, spraying UV topcoat on the coating layer.

[0033] Likewise, the topcoat includes a polyurethane UV coating and a thinner; the ratio of the coating to the thinner is 5:0-2.

[0034] After the topcoat is sprayed, it needs to be cured with ultraviolet light. In this embodiment, the wavelength of ultraviolet light for curing the topcoat is 300-420nm.

[0035] In this embodiment, after the UV topcoat spraying is completed, the surface of the final product can be subjected to functional testing, for example, corrosion resistance and wear resistance testing, as shown in Table 1.

[0036] Table 1 Product functional test after imitation chrome treatment

[0037]

[0038]

[0039] In summary, compared with the prior art, this embodiment does not require a water electroplating process, thereby reducing the cost of the process, and does not involve the emission of heavy metals such as hexavalent chromium, is more environmentally friendly, and reduces wastewater treatment costs. In addition, this embodiment also has good corrosion resistance.

[0040] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A green imitation chrome treatment process for an aluminum alloy substrate, characterized in that: include: S1, cleaning the surface of the product to be sprayed; S2, spraying a treatment agent on the cleaned surface and leaving it to stand for a certain period of time; S3, after standing still, spraying UV primer on the surface; S4, PVD coating is performed on the surface of the sprayed primer; S5, spraying UV topcoat on the coating layer.

2. The green imitation chromium treatment process for aluminum alloy substrate according to claim 1, characterized in that: In step S1, the cleaning process includes removing stains and dust from the surface of the product to be sprayed.

3. The green imitation chromium treatment process for aluminum alloy substrate according to claim 1, characterized in that: In step S2, the treating agent is an organosilicon compound, and the standing time is 3-5 minutes.

4. The green imitation chromium treatment process for aluminum alloy substrate according to claim 1, characterized in that: In step S3, the primer includes a coating and a thinner; Paint: thinner = 5:0~2; the ultraviolet wavelength used for primer curing is 300-420nm.

5. The green imitation chromium treatment process for aluminum alloy substrate according to claim 1, characterized in that: In step S4, during PVD coating: the evaporation material is aluminum wire or aluminum alloy; the current is 10-40A; and the coating time is 5 minutes.

6. The green imitation chromium treatment process for aluminum alloy substrate according to claim 1, characterized in that: In step S5, the primer includes a coating and a thinner; Paint: thinner = 5:0~2; the ultraviolet wavelength used for topcoat curing is 300-420nm.

7. The green imitation chromium treatment process for aluminum alloy substrate according to claim 1, characterized in that: Also includes: S6, performing functional tests on the product surface; the functional tests include corrosion resistance and wear resistance.