Fiberboard without external adhesive and preparation method

Through the preparation method of fiberboard without external glue, the plant fibers are evenly mixed with eutectic solvent and water, which solves the odor and density problems of bio-based fiberboard during preparation, and achieves the preparation of fiberboard with high glue strength and environmental protection. Auto parts with complex structures.

CN118893683APending Publication Date: 2024-11-05CHERY NEW ENERGY AUTOMOBILE TECH CO LTD

Patent Information

Application Number
CN202411079417.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing bio-based fiberboards have problems such as large odor and large glue density during preparation, and the commonly used organic plywood is limited due to its odorability and non-recyclability, while inorganic plywood has insufficient performance due to its high density and uneven mixing.

Method used

Using the preparation method of fiberboard without external glue, the plant powder is added to dissolve the eutectic solvent and soaked in water to form the fiberboard, combined with the hot pressing process, and the hydrogen bond between the fibers is destroyed by using the eutectic solvent to make the cellulose and the matrix. Mix evenly to form fiberboard with high plywood strength.

Benefits of technology

It realizes the preparation of fiberboard without the need to add organic or inorganic adhesives, overcomes the problems of large odor and density, has good glue performance and environmental protection, is suitable for complex structures such as automotive parts, and has few raw materials and is recyclable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893683A_ABST
    Figure CN118893683A_ABST
Patent Text Reader

Abstract

The invention discloses a fiberboard without external glue and a preparation method, and belongs to the field of material preparation. According to the fiberboard provided by the invention, slurry and a base material are combined into a fiberboard structure through various processes and finally through a hot press molding process. According to the present invention, the variety of the raw materials of the product is less, various organic adhesives and inorganic adhesives do not need to be added, the used eutectic solvent destroys the hydrogen bonds between the fibers so as to dissolve the fibers, release more hydrogen bond interaction units, uniformly disperse the hydrogen bond interaction units, and achieve the good mixing effect with the matrix; after the base body and a large amount of water are added, the deep-eutectic solvent is separated from the water, cellulose and lignin in the deep-eutectic solvent act with fibers in the base body to play a role of an adhesive, and fiberboards with various bonding strengths can be obtained by controlling the ratio of slurry to the base body. The ecological plywood has the advantages of organic plywood, the problems that inorganic plywood is large in density and uneven in mixing are solved, and the ecological plywood is prepared with few materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and relates to a fiberboard without externally added glue and a preparation method thereof. Background Art

[0002] There are two major categories of bio-based materials that can be used in vehicles at present: a: bio-based polymers synthesized by extracting small molecules from plants, such as polylactic acid (PLA), polycaprolactone (PCL), bio-based nylon 56, etc.; b: bio-based reinforced composite materials reinforced with plant fibers and traditional polymerization, such as a Chinese patent for a modified hemp fiber reinforced unsaturated polyester composite material (Announcement No.: CN102702708B); For products of category a, small molecules need to be extracted from plants for polymerization, the production process is complicated, pollution is serious, and it cannot be recycled and reused due to performance problems. For category b, it is actually just the modification of bio-based fibers as additives, and the main polymer materials are still derived from fossil energy. Although the overall process is more convenient than category a and the performance is excellent, it has many problems such as severe odor, non-recyclability, and inability to be reused. These two categories of products have many adverse effects on production capacity, cost, scope of use, and have high selectivity requirements for plants. The proportion of plants used in all agricultural residues is small, and they still cannot solve the problem of other agricultural residue plants (such as waste straw, cauliflower straw, and nut shells). Therefore, fiberboards made of agricultural waste plants or powders as the main body and bonded with adhesives came into being.

[0003] At present, bio-based fiberboard can be divided into two categories according to the type of adhesive: the Chinese patent for organic plywood (Announcement No.: CN104802232B) and the Chinese patent application for inorganic plywood (Publication No.: CN109665803A). The commonly used organic plywood (common organic glue: urea-formaldehyde glue (UF), phenol-formaldehyde glue (PF) and melamine-formaldehyde glue (MF)) has been plagued by serious odor, especially the release of formaldehyde. Although inorganic plywood has excellent odor, due to the high density of inorganic glue and poor mixing uniformity, some of the performance properties of inorganic plywood (such as toughness and appearance) are slightly inferior to those of organic plywood. Although there is currently a Chinese patent for a low-odor bio-based organic adhesive (publication number: CN113249086B), its use is still affected by performance disadvantages such as low bonding strength, poor water resistance, poor mildew resistance, high viscosity, and poor processing performance. In addition, the synthesis process of organic adhesives is complicated and the environmental pollution is also relatively serious. In addition, both require the addition of various additives to improve performance, which increases the complexity and cost of the processing process. Summary of the invention

[0004] The purpose of the present invention is to solve the problem in the prior art that the existing organic fiberboard has a strong odor during preparation and the inorganic fiberboard has a high plywood density during preparation, resulting in uneven mixing, and to provide a fiberboard without externally added glue and a preparation method.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for preparing a fiberboard without externally added glue, comprising:

[0007] adding plant A powder into a deep eutectic solvent for dissolution to obtain a slurry;

[0008] The plant B powder is added into water and soaked to saturate the water, then beaten to obtain mud, and heated and kept warm to obtain a substrate;

[0009] The slurry, substrate and water are mixed, filtered, washed and heat-pressed to obtain a non-glue fiberboard;

[0010] Wherein, the plant A powder and the plant B powder are both woody plant or herbaceous plant powders.

[0011] Preferably, the particle size of the plant A powder is 10 to 500 meshes, and the mass ratio of the plant A powder to the low eutectic solvent is (1:5) to (1:40).

[0012] Preferably, in the step of adding the plant B powder into water to soak it to saturate it, beating it to obtain mud, and heating and heat-insulating it to obtain the substrate:

[0013] The length of plant B powder ranged from 1 to 10 cm;

[0014] The soaking temperature range is 10℃~40℃, and the soaking time is 10~240h;

[0015] The particle size of the pulp is 1 to 3000 mesh;

[0016] The heating temperature range is 60℃~120℃, and the insulation time range is 10~60min.

[0017] Preferably, in the step of mixing the slurry, substrate and water, filtering, washing and hot pressing to obtain the glue-free fiberboard:

[0018] The mass ratio of the slurry to the substrate is (10:1) to (1:10).

[0019] Preferably, during the hot pressing treatment, the vacuum pressure is -0.7 to -1.0 MPa; the hot pressing temperature is 100° C. to 200° C., and the hot pressing pressure is 1 MPa to 25 MPa.

[0020] Preferably, the plant A powder is a woody plant, and the plant B powder is a herbaceous plant powder.

[0021] Preferably, the deep eutectic solvent comprises a hydrogen bond donor solvent and a hydrogen bond acceptor solvent.

[0022] Preferably, the hydrogen bond donor solvent is one or more of an amine, an amide, a carboxylic acid, an amino acid, a sugar and an alcohol.

[0023] Preferably, the hydrogen bond acceptor solvent is one or more of quaternary ammonium salts, quaternary phosphonium salts, betaine, imidazoles and amino acids.

[0024] A fiberboard without externally added glue is prepared by a method for preparing a fiberboard without externally added glue.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention proposes a method for preparing a fiberboard without externally added glue, which uses slurry and substrate to be combined into a fiberboard structure through multiple processes and finally through a hot pressing process. The substrate serves as the main body and force-bearing part of the sample, and the slurry plays the role of an adhesive; the raw material types of the product of the present invention are relatively small, and there is no need to add various organic adhesives and inorganic adhesives. The low eutectic solvent used destroys the hydrogen bonds between the fibers and dissolves the fibers, releasing more hydrogen bonding units and dispersing them evenly, and having a better mixing effect with the matrix; after adding the matrix and a large amount of water, the low eutectic solvent is separated from the water, allowing the cellulose and lignin in the low eutectic solvent to act on the fibers in the matrix, playing the role of an adhesive, and various fiberboards with various bonding strengths can be obtained by controlling the ratio of slurry and matrix. It not only has the advantages of organic plywood, but also overcomes its shortcomings such as odor, non-recyclability, and inability to be reused, and also overcomes the problems of high density and uneven mixing of inorganic plywood, and uses less material to prepare ecological plywood. It can be used for automobile parts with simpler structures such as engine covers, door panels, trunk covers, seat guards, etc.

[0027] Furthermore, the hot pressing process can release more active units from cellulose, further strengthening the physical and chemical interactions between the various fiber components, making the fiberboard have very good gluing properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 The present invention is a flow chart of the method for preparing fiberboard without externally added glue. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0031] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0033] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0034] The present invention provides a method for preparing a fiberboard without externally added glue, comprising the following steps:

[0035] Step 1, adding plant A powder into a deep eutectic solvent for dissolution to obtain a slurry;

[0036] The particle size of the plant A powder is 10 to 500 meshes, and the mass ratio of the plant A powder to the low eutectic solvent is (1:5) to (1:40).

[0037] Step 2, adding the plant B powder into water to soak it to saturate it, beating it to obtain mud, and heating and heat preservation to obtain a base material;

[0038] The plant B powder is added to water and soaked to saturate it, then beaten to obtain mud, and heated and kept warm to obtain a substrate, specifically:

[0039] The length of plant B powder ranged from 1 to 10 cm;

[0040] The soaking temperature range is 10℃~40℃, and the soaking time is 10~240h;

[0041] The particle size of the pulp is 1 to 3000 mesh;

[0042] The heating temperature range is 60℃~120℃, and the insulation time range is 10~60min.

[0043] Step 3: Mix the slurry, substrate and water, filter, wash and heat-press to obtain a non-glue fiberboard.

[0044] The slurry, substrate and water are mixed, filtered, washed and hot-pressed to obtain a non-glue fiberboard, which is specifically:

[0045] The mass ratio of the slurry to the substrate is (10:1) to (1:10).

[0046] During the hot pressing treatment, the vacuum pressure is -0.7 to -1.0 MPa; the hot pressing temperature is 100°C to 200°C, and the hot pressing pressure is 1MPa to 25MPa.

[0047] The preparation method is described in detail below. Figure 1 As shown:

[0048] Step 1: The preparation steps of the slurry are as follows:

[0049] 1.1 Crushing: crush plant A into powder form by various machines (ball mill or sawdust crusher); preferably 10-500 mesh, preferably 50-100 mesh; ball milling at a speed of 500-600 rpm for 48h-50h;

[0050] 1.2 Dissolution: Add the powder prepared in 1.1 above into a deep eutectic solvent for dissolution;

[0051] Wherein, the mass ratio of the powder crushed in step 1.1 to the deep eutectic solvent is 1:5 to 1:40, preferably 1:10 to 1:20;

[0052] Plant A can be various plants, including various woody plants and herbaceous plants, preferably woody plants with high lignin content, including but not limited to coniferous wood, broad-leaved wood, poplar, etc.;

[0053] The low eutectic solvent is a mixed liquid, including hydrogen bond donors and hydrogen bond acceptors; hydrogen bond donors: generally composed of one or more of amines, amides, carboxylic acids, amino acids, sugars, alcohols or other polyols; hydrogen bond acceptors: generally composed of one or more of quaternary ammonium salts, quaternary phosphate salts, betaine, imidazole amino acids, etc.;

[0054] Step 2: The preparation steps of the substrate are as follows:

[0055] 2.1 Crushing: Use a crusher to crush the plant B into small pieces of a certain length, the length of which is 1 cm to 10 cm, preferably 2 cm to 4 cm;

[0056] 2.2 Soaking: Soak the plant B segment obtained in step 2.1 in water at a certain temperature for a certain period of time;

[0057] Temperature range: 10-50°C, preferably 20-30°C; Soaking time: 10-240h, preferably 60-100h;

[0058] 2.3 Grinding: Take out the saturated plant B segments soaked in step 2.2, and use a pulper to pulp them to obtain a slurry form;

[0059] The particle size is 1 to 3000 mesh; preferably: 10 to 1250 mesh; preferably 60 to 300 mesh;

[0060] 2.4 De-latency: Heat the slurry grinding liquid in step 2.3 to a certain temperature and keep it warm;

[0061] Furthermore, the heating temperature range is 60 to 120°C, preferably 80 to 100°C.

[0062] Furthermore, the holding time ranges from 10 to 60 minutes, preferably from 20 to 40 minutes.

[0063] Among them, plant B can be various plants, including various woody plants and herbaceous plants, preferably herbaceous plants with a high cellulose content: including but not limited to rice, wheat, soybeans, corn, etc.; water is clean water; to facilitate the subsequent recovery of the low eutectic solvent, the water is preferably distilled water or deionized water.

[0064] Step 3: subjecting the slurry and substrate to the following process to obtain a non-glue fiberboard:

[0065] 3.1 Mixing: Mix the slurry and base material and add water and stir.

[0066] The ratio of the slurry to the substrate is (10:1) to (1:10); preferably, (3:1) to (1:5); preferably, (1:1) to (1:3);

[0067] After adding water, the sum of the mass of the slurry and the base material mixed slurry accounts for 1% to 50% of the total mass; preferably, 5% to 30%;

[0068] The stirring time is preferably 1 to 6 hours, preferably 2 to 3 hours;

[0069] 3.2 Filtration: Filter the mixed solution in step 3.1 to obtain a mixed slurry (solid content 1% to 40%, preferably 5% to 20%);

[0070] 3.3 Washing: Wash the filtered mixed slurry in step 3.2 with clean water several times and filter it to wash out the excess low eutectic solvent; the low eutectic solvent can be recovered after evaporating the water;

[0071] 3.4 Ultrasound: The mixture cleaned in step 3.3 is subjected to ultrasonic treatment for a certain period of time to obtain a mixture with a more uniform surface structure;

[0072] Ultrasonic power: 200-3000W, preferably 600-1000W; ultrasonic treatment time: 10-60min, preferably 20-40min;

[0073] 3.5 Hot pressing: Place the product in step 3.4 into a mold with a dense mesh, first evacuate the air, then hot press to obtain the final fiberboard.

[0074] Vacuum pressure -0.7~-1.0MPa, preferably: -0.8~-1.0MPa; vacuum until no water appears;

[0075] The hot pressing temperature is 100-200° C., preferably 130-170° C.; the hot pressing pressure is 1-25 MPa, preferably 2-8 MPa.

[0076] The following is an analysis based on examples

[0077] Example 1

[0078] For example, plant A is poplar and plant B is rape straw

[0079] 1. Preparation of slurry:

[0080] 1.1 Crushing: The poplar wood was ball-milled at a speed of 500 rpm for 48 hours to be crushed into powder form, and then sieved to obtain wood powder with a mesh number of 60;

[0081] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:15;

[0082] Further, the deep eutectic solvent is prepared by mixing choline chloride (C5H14CINO) and oxalic acid (H2C2O4●2H2O) in a molar ratio of 1:1 and heating and melting at 80°C until a uniform and transparent liquid is obtained;

[0083] 2. Preparation of substrate:

[0084] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 2 cm;

[0085] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 20℃ room temperature water for 72h;

[0086] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to beat it to obtain a slurry with an average particle size of 100 meshes;

[0087] 2.4 De-latching: Heat the above slurry grinding liquid to 90℃ and keep it warm for 30min;

[0088] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0089] 3.1 Mixing:

[0090] Further, the slurry and the substrate are mixed in a ratio of 1:1 and stirred;

[0091] Further, distilled water (mixture proportion 10%) was added to the above mixture and stirred for 2 h;

[0092] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to remove the liquid and obtain a mixed slurry with a solid content of 20%;

[0093] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0094] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (800 W) treatment for 20 min to obtain a more uniform mixture;

[0095] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.9 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing process at a temperature of 150°C and a pressure of 6.5 MPa.

[0096] Example 2

[0097] For example, plant A is coniferous wood and plant B is corn stalks.

[0098] 1. Preparation of slurry:

[0099] 1.1 Crushing: The coniferous wood was ball-milled at 550 rpm for 48 hours to be crushed into powder form, and then sieved to obtain wood powder with a mesh size of 50;

[0100] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:10;

[0101] Further, the deep eutectic solvent is obtained by mixing choline chloride (C5H14CINO) and urea in a molar ratio of 1:2 and heating and melting at 302°C until a uniform and transparent liquid is obtained;

[0102] 2. Preparation of substrate:

[0103] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 4 cm;

[0104] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 10℃ room temperature water for 60h;

[0105] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to beat it to obtain a slurry with an average particle size of 300 meshes;

[0106] 2.4 De-latency: Heat the above slurry grinding liquid to 100℃ and keep it warm for 40min;

[0107] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0108] 3.1 Mixing:

[0109] Further, the slurry and the substrate are mixed and stirred in a ratio of 1:3;

[0110] Further, distilled water (mixture proportion is 50%) was added to the above mixture and stirred for 3 h;

[0111] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to remove the liquid and obtain a mixed slurry with a solid content of 30%;

[0112] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0113] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (600 W) treatment for 40 min to obtain a more uniform mixture;

[0114] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.7 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 170°C and a pressure of 8 MPa.

[0115] Example 3

[0116] For example, plant A is a broadleaf tree and plant B is wheat straw.

[0117] 1. Preparation of slurry:

[0118] 1.1 Crushing: The hardwood was ball milled at 600 rpm for 50 hours to form a powder, which was then sieved to obtain wood powder with a mesh size of 100;

[0119] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:20;

[0120] Further, the deep eutectic solvent is obtained by mixing choline chloride (C5H14CINO) and imidazole in a molar ratio of 3:7 and heating and melting at 140°C until a uniform and transparent liquid is obtained;

[0121] 2. Preparation of substrate:

[0122] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 10 cm;

[0123] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 30℃ room temperature water for 100h;

[0124] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to pulp it to obtain a slurry with an average particle size of 60 meshes;

[0125] 2.4 De-latching: Heat the above slurry grinding liquid to 80℃ and keep it warm for 20min;

[0126] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0127] 3.1 Mixing:

[0128] Further, the slurry and the substrate are mixed and stirred in a ratio of 3:1;

[0129] Further, distilled water (5% of the mixture) was added to the above mixture and stirred for 6 h;

[0130] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to remove the liquid and obtain a mixed slurry with a solid content of 40%;

[0131] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0132] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (1000 W) treatment for 60 min to obtain a more uniform mixture;

[0133] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.8 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 200°C and a pressure of 25 MPa.

[0134] Example 4

[0135] For example, plant A is poplar and plant B is rice straw.

[0136] 1. Preparation of slurry:

[0137] 1.1 Crushing: The poplar wood was ball milled at a speed of 580 rpm for 49 hours to be crushed into powder form, and then sieved to obtain wood powder with a mesh number of 500;

[0138] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:40;

[0139] Further, the deep eutectic solvent is prepared by mixing choline chloride (C5H14CINO) and ammonium thiocyanate in a molar ratio of 1:1 and heating and melting at 100°C until a uniform transparent liquid is obtained;

[0140] 2. Preparation of substrate:

[0141] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 1 cm;

[0142] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 50℃ room temperature water for 200h;

[0143] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to pulp it to obtain a slurry with an average particle size of 3000 meshes;

[0144] 2.4 De-latching: Heat the above slurry grinding liquid to 90℃ and keep it warm for 50min;

[0145] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0146] 3.1 Mixing:

[0147] Further, the slurry and the substrate are mixed and stirred in a ratio of 1:5;

[0148] Further, distilled water (30% of the mixture) was added to the above mixture and stirred for 1 h;

[0149] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to obtain a mixed slurry with a solid content of 5%;

[0150] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0151] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (2500W) treatment for 60 min to obtain a more uniform mixture;

[0152] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-1.0 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 100°C and a pressure of 5 MPa.

[0153] Example 5

[0154] For example, plant A is coniferous wood and plant B is corn stalks.

[0155] 1. Preparation of slurry:

[0156] 1.1 Crushing: The coniferous wood was ball-milled at a speed of 500 rpm for 48 hours to be crushed into powder form, and then sieved to obtain wood powder with a mesh size of 10;

[0157] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:5;

[0158] Further, the deep eutectic solvent is prepared by mixing choline chloride (C5H14CINO) and caprolactam in a molar ratio of 1:1 and heating and melting at 120°C until a uniform and transparent liquid is obtained;

[0159] 2. Preparation of substrate:

[0160] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 5 cm;

[0161] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 50℃ room temperature water for 240h;

[0162] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to pulp it to obtain a slurry with an average particle size of 1250 meshes;

[0163] 2.4 De-latency: Heat the above slurry grinding liquid to 120℃ and keep it warm for 60min;

[0164] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0165] 3.1 Mixing:

[0166] Further, the slurry and the substrate are mixed and stirred in a ratio of 1:10;

[0167] Further, distilled water (mixture proportion is 20%) was added to the above mixture and stirred for 5 h;

[0168] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to obtain a mixed slurry with a solid content of 10%;

[0169] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0170] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (2500W) treatment for 50 min to obtain a more uniform mixture;

[0171] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.8 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 130°C and a pressure of 7 MPa.

[0172] Example 6

[0173] For example, plant A is a hardwood and plant B is soybean straw

[0174] 1. Preparation of slurry:

[0175] 1.1 Crushing: The hardwood was ball milled at 580 rpm for 48 hours to form a powder, which was then sieved to obtain 80-mesh wood powder;

[0176] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:15;

[0177] Further, the deep eutectic solvent is prepared by mixing choline chloride (C5H14CINO) and hexanamide in a molar ratio of 1:2 and heating and melting at 140°C until a uniform and transparent liquid is obtained;

[0178] 2. Preparation of substrate:

[0179] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 3 cm;

[0180] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 40℃ room temperature water for 10 hours;

[0181] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to pulp it to obtain a slurry with an average particle size of 10 meshes;

[0182] 2.4 De-latency: Heat the above slurry grinding liquid to 60℃ and keep it warm for 10min;

[0183] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0184] 3.1 Mixing:

[0185] Further, the slurry and the substrate were mixed and stirred in a ratio of 10:1;

[0186] Further, distilled water (1% of the mixture) was added to the above mixture and stirred for 2 h;

[0187] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to remove the liquid and obtain a mixed slurry with a solid content of 1%;

[0188] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0189] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (3000W) treatment for 10 min to obtain a more uniform mixture;

[0190] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.8 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 190°C and a pressure of 2 MPa.

[0191] Example 7

[0192] For example, plant A is coniferous wood and plant B is corn stalks.

[0193] 1. Preparation of slurry:

[0194] 1.1 Crushing: The coniferous wood was ball-milled at a speed of 500 rpm for 48 hours to be crushed into powder form, and then sieved to obtain wood powder with a mesh size of 80;

[0195] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:18;

[0196] Further, the deep eutectic solvent is prepared by mixing benzyltrimethylammonium chloride and lactic acid in a molar ratio of 1:1 and heating and melting at 140° C. until a uniform and transparent liquid is obtained;

[0197] 2. Preparation of substrate:

[0198] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 8 cm;

[0199] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 25℃ room temperature water for 80h;

[0200] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to pulp it to obtain a slurry with an average particle size of 1 mesh;

[0201] 2.4 De-latching: Heat the above slurry grinding liquid to 85℃ and keep it warm for 25min;

[0202] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0203] 3.1 Mixing:

[0204] Further, the slurry and the substrate are mixed and stirred in a ratio of 1:2;

[0205] Further, distilled water (10% of the mixture) was added to the above mixture and stirred for 4 h;

[0206] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to remove the liquid and obtain a mixed slurry with a solid content of 30%;

[0207] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0208] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (200 W) treatment for 20 min to obtain a more uniform mixture;

[0209] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.8 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 160°C and a pressure of 1 MPa.

[0210] Example 8

[0211] For example, plant A is poplar and plant B is rape straw

[0212] 1. Preparation of slurry:

[0213] 1.1 Crushing: The poplar wood was ball-milled at 600 rpm for 50 hours to be crushed into powder form, and then sieved to obtain wood powder with a mesh size of 70;

[0214] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:35;

[0215] Further, the deep eutectic solvent is prepared by mixing benzyltriethylammonium chloride (BTEAC) / lactic acid (LA) in a molar ratio of 1:1 and heating and melting at 140° C. until a uniform transparent liquid is obtained;

[0216] 2. Preparation of substrate:

[0217] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 7 cm;

[0218] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 45°C room temperature water for 200 hours;

[0219] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to beat it to obtain a slurry with an average particle size of 2400 meshes;

[0220] 2.4 De-latching: Heat the above slurry grinding liquid to 110℃ and keep it warm for 50min;

[0221] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0222] 3.1 Mixing:

[0223] Further, the slurry and the substrate are mixed in a ratio of 1:1 and stirred;

[0224] Further, distilled water (40% of the mixture) was added to the above mixture and stirred for 4 h;

[0225] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to obtain a mixed slurry with a solid content of 35%;

[0226] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0227] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (300 W) treatment for 30 min to obtain a more uniform mixture;

[0228] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-1.0 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 180°C and a pressure of 18 MPa.

[0229] Example 9

[0230] For example, plant A is a broadleaf tree and plant B is wheat straw.

[0231] 1. Preparation of slurry:

[0232] 1.1 Crushing: The hardwood was ball milled at 570 rpm for 47 hours to form a powder, which was then sieved to obtain wood powder with a mesh size of 400;

[0233] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:25;

[0234] Further, the deep eutectic solvent is prepared by mixing choline chloride (C5H14CINO) and oxalic acid (H2C2O4●2H2O) in a molar ratio of 1:2 and heating and melting at 130°C until a uniform and transparent liquid is obtained;

[0235] 2. Preparation of substrate:

[0236] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 3 cm;

[0237] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 25℃ room temperature water for 80h;

[0238] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to beat it to obtain a slurry with an average particle size of 500 meshes;

[0239] 2.4 De-latency: Heat the above slurry grinding liquid to 100℃ and keep it warm for 40min;

[0240] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0241] 3.1 Mixing:

[0242] Further, the slurry and the substrate are mixed and stirred in a ratio of 3:1;

[0243] Further, distilled water (mixture proportion is 20%) was added to the above mixture and stirred for 5 h;

[0244] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to remove the liquid and obtain a mixed slurry with a solid content of 15%;

[0245] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0246] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (400 W) treatment for 30 min to obtain a more uniform mixture;

[0247] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.7 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 200°C and a pressure of 15 MPa.

[0248] Example 10

[0249] For example, plant A is poplar and plant B is soybean straw

[0250] 1. Preparation of slurry:

[0251] 1.1 Crushing: The poplar wood was ball-milled at a speed of 500 rpm for 49 hours to be crushed into powder form, and then sieved to obtain wood powder with a mesh number of 300;

[0252] 1.2 Dissolution: Add the above wood powder into the deep eutectic solvent at a mass ratio of 1:20;

[0253] Further, the deep eutectic solvent is prepared by mixing choline chloride (C5H14CINO) and oxalic acid (H2C2O4●2H2O) in a molar ratio of 1:1 and heating and melting at 150°C until a uniform and transparent liquid is obtained;

[0254] 2. Preparation of substrate:

[0255] 2.1 Crushing: Use a straw crusher to crush the straw into small pieces with a length of 8 cm;

[0256] 2.2 Soaking: Soak the above-mentioned small pieces of straw raw materials in 30℃ room temperature water for 200h;

[0257] 2.3 Grinding: Take out the soaked saturated straw and use a pulping machine to beat it to obtain a slurry with an average particle size of 500 meshes;

[0258] 2.4 De-latency: Heat the above slurry grinding liquid to 90℃ and keep it warm for 10 minutes;

[0259] 3. Mix the above slurry and substrate to prepare the fiberboard without external additives:

[0260] 3.1 Mixing:

[0261] Further, the slurry and the substrate were mixed and stirred in a ratio of 10:1;

[0262] Further, distilled water (8% of the mixture) was added to the above mixture and stirred for 4 h;

[0263] 3.2 Filtration: The mixed solution was filtered under vacuum (-0.9 MPa) to remove the liquid and obtain a mixed slurry with a solid content of 15%;

[0264] 3.3 Washing: Wash the mixed slurry with distilled water and filter it according to step 3.2; after filtering the recovered filtrate, evaporate the water to recover the low eutectic solvent;

[0265] 3.4 Ultrasound: The mixture cleaned in step 3.3 was subjected to ultrasound (1800 W) treatment for 15 min to obtain a more uniform mixture;

[0266] 3.5 Hot pressing: Place the product of step 3.4 into a mold with a dense mesh, first evacuate (-0.9 MPa) until no water appears, and then obtain the final fiberboard under a hot pressing molding process at a temperature of 140°C and a pressure of 6 MPa.

[0267] The fiberboard without externally added glue proposed by the present invention uses plants, low eutectic solvents and water as raw materials. Due to the generation and dissociation of various components of plant fibers and the synergistic effect (mainly hydrogen bonding) with the low eutectic solvent, a plywood with the advantages of high bonding strength, stable performance, green environmental protection, non-toxicity, harmlessness, recyclability, utilization and degradability is made, which meets the requirements of ecological plywood; the raw materials of the present invention are only: plants, low eutectic solvents, water, and the types of raw materials are relatively small, and there is no need to add various organic adhesives and inorganic adhesives; the plants of the present invention have a wide range of applications, and all agricultural waste plants can be used as plant A or plant B; the low eutectic solvent used in the present invention destroys the hydrogen bonds between fibers to dissolve the fibers, releasing The low eutectic solvent is separated from the water after being added to the matrix and a large amount of water, so that the cellulose and lignin in the low eutectic solvent react with the fibers in the matrix to play the role of an adhesive, and fiberboards with various bonding strengths can be obtained by controlling the ratio of the slurry and the matrix; the low eutectic solvent and water of the present invention can be recycled and reused; the hot pressing process of the present invention can release more action units from cellulose, further strengthen the physical and chemical effects between the various components of the fiber, and make the fiberboard have very good bonding properties; the present invention has excellent modification potential, and various performance requirements, such as electrical conductivity, can be achieved through various additives.

[0268] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a fiberboard without externally added glue, It is characterized in that include: adding plant A powder into a deep eutectic solvent for dissolution to obtain a slurry; The plant B powder is added into water and soaked to saturate the water, then beaten to obtain mud, and heated and kept warm to obtain a substrate; The slurry, substrate and water are mixed, filtered, washed and heat-pressed to obtain a non-glue fiberboard; Wherein, the plant A powder and the plant B powder are both woody plant or herbaceous plant powders.

2. The method for preparing a fiberboard without externally added glue according to claim 1, It is characterized in that The particle size of the plant A powder is 10 to 500 meshes, and the mass ratio of the plant A powder to the low eutectic solvent is (1:5) to (1:40).

3. The method for preparing a fiberboard without externally added glue according to claim 1, It is characterized in that In the step of adding the plant B powder into water and soaking it to saturate it, beating it to obtain mud, and heating and heat preservation to obtain the substrate: The length of plant B powder ranged from 1 to 10 cm; The soaking temperature range is 10℃~40℃, and the soaking time is 10~240h; The particle size of the pulp is 1 to 3000 mesh; The heating temperature range is 60℃~120℃, and the insulation time range is 10~60min.

4. The method for preparing fiberboard without externally added glue according to claim 1, It is characterized in that In the step of mixing the slurry, substrate and water, filtering, washing and hot pressing to obtain the glue-free fiberboard: The mass ratio of the slurry to the substrate is (10:1) to (1:10).

5. The method for preparing the fiberboard without external addition of glue according to claim 1, It is characterized in that During the hot pressing treatment, the vacuum pressure is -0.7 to -1.0 MPa; the hot pressing temperature is 100°C to 200°C, and the hot pressing pressure is 1MPa to 25MPa.

6. The method for preparing the fiberboard without external additives according to claim 1, It is characterized in that The plant A powder is a woody plant, and the plant B powder is a herbaceous plant powder.

7. The method for preparing the fiberboard without external addition of glue according to claim 1, It is characterized in that The deep eutectic solvent includes a hydrogen bond donor solvent and a hydrogen bond acceptor solvent.

8. The method for preparing the fiberboard without externally added glue according to claim 7, It is characterized in that The hydrogen bond donor solvent is one or more of amines, amides, carboxylic acids, amino acids, sugars and alcohols.

9. The method for preparing the fiberboard without externally added glue according to claim 7, It is characterized in that The hydrogen bond acceptor solvent is one or more of quaternary ammonium salts, quaternary phosphonium salts, betaine, imidazoles and amino acids.

10. A fiberboard without external glue, It is characterized in that The fiberboard is prepared by the method for preparing a fiberboard without externally added glue as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Gluing-free middle and high-density fiber board preparation method

    CN101086150A

  • Novel pulping process for obtaining high performance fiber at high yield from plants

    CN102337687A

  • Method for rapidly separating main components of woody biomass by using eutectic solvent

    CN114108350A

  • Method for gluing plates without glue

    CN114536487A

  • Multifunctional polyurethane fiber as well as preparation method and application thereof

    CN114892294A

Cited By

  • Wood fiber structural material as well as preparation method and application thereof

    CN121200173A

  • Forming method for physical consolidation of fiber material

    CN122610288A

  • A forming method for the physical consolidation of fibrous materials

    CN122610288B