Production process of annular wearable part and intelligent ring

By using supercritical carbon dioxide to replace air and control temperature pressure in ring wearable products, a low viscosity plastic mixture is formed, which solves the problem of uneven bubbles and filling, improves the waterproof performance and structural strength of ring wearable products, and improves the Production quality.

CN118893790AActive Publication Date: 2024-11-05JUNSON SHENZHEN CHUANJINDAIYIN TECH CO LTD

Patent Information

Application Number
CN202411315396.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-05
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Annular wearable products are prone to bubbles during the injection and curing of plastic materials, resulting in reduced waterproofing performance and insufficient structural strength, and it is difficult for the material to fill the internal space evenly, affecting production quality and yield.

Method used

Supercritical carbon dioxide is used to replace air to form a low viscosity plastic mixture, and it is deposited and solidified in the annular cavity by precise control of temperature and pressure. The compensation cavity structure is used to supplement the volume reduction caused by precipitation, ensuring uniform distribution and filling of the material.

Benefits of technology

It effectively avoids bubble formation, ensures uniform distribution and filling of materials, improves waterproof performance and structural strength, reduces the risk of thermal shock of electronic components, and improves production quality and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893790A_ABST
    Figure CN118893790A_ABST
Patent Text Reader

Abstract

The invention discloses a production process of an annular wearable part and an intelligent ring, and the production process comprises the steps: providing an annular element and a mold, and placing the annular element in a cavity; supercritical carbon dioxide for replacement is injected into the annular cavity and the compensation cavity; mixing a pre-prepared plastic material with supercritical carbon dioxide for mixing to form a low-viscosity plastic mixture; the low-viscosity plastic mixture is injected into the annular cavity and the compensation cavity, and the pressure is kept higher than the critical pressure of the supercritical carbon dioxide in the injection process; controlling the temperature and the pressure, so that the supercritical carbon dioxide is gradually separated out from the low-viscosity plastic mixture, and meanwhile, the plastic material in the low-viscosity plastic mixture is gradually deposited and cured in the annular cavity; and after the plastic material in the annular cavity is completely cured, taking out the annular element from the mold, cooling the annular element to room temperature, and packaging the annular element. According to the technical scheme, bubbles can be prevented from existing in the cured plastic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of production of annular wearable parts, and in particular to a production process of annular wearable parts and a smart ring. Background Art

[0002] With the rapid development of wearable technology, smart devices are gradually evolving towards miniaturization, portability and multifunctionality. Under this trend, ring-shaped wearable products such as smart rings, earrings and bracelets have emerged, which combine the beauty of traditional accessories with advanced electronic technology to provide users with multiple functions such as health monitoring and identity authentication. To achieve these functions, various electronic components such as optical sensors, processors and batteries need to be integrated into the inner cavity of wearable products.

[0003] In order to protect these delicate electronic components and ensure the normal operation of wearable products, it is necessary to fill the inner cavity of the product with plastic materials. After the plastic materials are solidified and formed, the outer shell and electronic components of the product can be effectively connected together to achieve protection functions such as fixing electronic components, waterproofing, dustproofing and shock resistance. However, traditional filling methods face many challenges. During the injection and curing process of plastic materials, bubbles often form inside, which not only affects the appearance of the product, but also may reduce its waterproof performance and structural strength. Due to the complex internal structure of ring-shaped wearable devices, traditional methods make it difficult to ensure that plastic materials are evenly distributed in all spaces, especially in some tiny corners and gaps. In addition, some plastic materials will shrink during the curing process, resulting in incomplete filling or internal stress. These problems have seriously affected the production quality and yield of ring-shaped wearable devices, and a new production process is urgently needed to solve them. Summary of the invention

[0004] The main purpose of the present invention is to solve the technical problems in the existing production process of annular wearable products, such as bubbles existing inside the plastic material and the material being unable to effectively fill the internal space of the annular wearable product.

[0005] A first aspect of the present invention provides a production process for an annular wearable component, the production process for the annular wearable component comprising: S1, providing an annular element and a mold, wherein an annular cavity is formed in the annular element, an injection port connected to the annular cavity is opened on the annular element, a cavity matching the annular element and a compensation cavity connected to the cavity are provided in the mold; S2, placing the annular element in the cavity, wherein the outer wall surface of the annular element fits the inner wall surface of the cavity, and the annular cavity is connected with the compensation cavity through the injection port; S3, injecting supercritical carbon dioxide for replacement into the annular cavity and the compensation cavity to replace all the air in the annular cavity and the compensation cavity; S4, mixing the pre-prepared plastic material with supercritical carbon dioxide for mixing to form a low-viscosity plastic mixture; injecting the low-viscosity plastic mixture into the annular cavity and the compensation cavity, and maintaining a pressure higher than the critical pressure of the supercritical carbon dioxide during the injection process; S5, controlling the temperature and pressure to gradually precipitate the supercritical carbon dioxide from the low-viscosity plastic mixture, and at the same time gradually depositing and solidifying the plastic material in the low-viscosity plastic mixture in the annular cavity; in this process, the low-viscosity plastic mixture in the compensation cavity is used to supplement the volume reduction of the low-viscosity plastic mixture in the annular cavity caused by the precipitation of the supercritical carbon dioxide; S6, after the plastic material in the annular cavity is completely solidified, the annular element is taken out from the mold, cooled to room temperature and packaged.

[0006] Optionally, the annular element comprises an outer annular wall and an inner annular wall which are arranged opposite to each other, and the injection port is formed between the outer annular wall and the inner annular wall; The mold comprises an annular outer side wall and an annular inner side wall which are arranged opposite to each other, wherein the compensation cavity and a fluid passage communicating with the compensation cavity are formed between the annular outer side wall and the annular inner side wall; The distance between the annular outer side wall and the annular inner side wall is smaller than the distance between the outer annular wall and the inner annular wall; wherein, After the annular element is placed in the mold cavity, the inner wall surface of the annular outer wall and the inner wall surface of the annular inner wall are both located between the outer annular wall and the inner annular wall, and the low-viscosity plastic mixture flows into the compensation cavity through the fluid port and flows into the annular cavity under the guidance of the inner wall surface of the annular outer wall or the inner wall surface of the annular inner wall.

[0007] Optionally, an outer annular abutting wall is convexly provided on the outer annular wall, and an inner annular abutting wall is convexly provided on the inner annular wall; wherein, After the annular element is placed in the cavity, the annular outer side wall is moved to abut the end thereof against the outer annular abutting wall, and the annular inner side wall is moved to abut the end thereof against the inner annular abutting wall.

[0008] Optionally, S3 includes: S3.1, placing the mold with the annular element in a high pressure reactor, wherein the high pressure reactor includes an inlet valve and an exhaust valve; S3.2, sealing the autoclave and adjusting the internal temperature of the autoclave to 35-40° C.; S3.3, open the exhaust valve, and inject supercritical carbon dioxide for replacement into the high-pressure reactor through the inlet valve, with an initial injection pressure of 80-100 bar; S3.4, after continuously injecting supercritical carbon dioxide for replacement for 15-20 minutes, close the exhaust valve and the inlet valve to maintain the pressure of the high-pressure reactor.

[0009] Optionally, the S4 includes: S4.1, mixing the pre-prepared plastic material with supercritical carbon dioxide for mixing in a high-pressure mixer for 5-10 minutes to form a low-viscosity plastic mixture; S4.2, controlling the temperature of the high-pressure mixer to 40-50° C. and the pressure to 100-120 bar; S4.3, opening the injection valve on the high-pressure reactor connected to the mold, injecting the low-viscosity plastic mixture into the annular cavity and the compensation cavity, and controlling the injection rate to be 0.1-0.5 ml / s; S4.4, during the injection process, the pressure in the annular cavity and the compensation cavity is maintained at 110-130 bar; S4.5, after the injection is completed, close the injection valve to ensure that the low-viscosity plastic mixture fills the annular cavity and the compensation cavity.

[0010] Optionally, the S5 includes: S5.1, controlling the temperature of the autoclave to 45-55°C for 30 minutes; S5.2, slowly reducing the pressure in the autoclave at a rate of 0.5-1 bar / min, so that supercritical carbon dioxide gradually precipitates from the low-viscosity plastic mixture; S5.3, gradually increasing the temperature of the autoclave to 60-70°C at a rate of 0.5°C / min, and maintaining the temperature for 60 minutes; S5.4, continue to reduce the pressure in the autoclave, and slow down the reduction rate to 0.3-0.5 bar / min; S5.5, raising the temperature of the autoclave to 70-80°C and maintaining it for 90 minutes; S5.6, slowly reducing the pressure in the autoclave to atmospheric pressure at a rate of 0.1-0.2 bar / min; S5.7, by means of a pressure sensor disposed in the high-pressure reactor, the pressure change in the annular cavity is monitored to ensure that the low-viscosity plastic mixture in the compensation cavity can flow naturally into the annular cavity to compensate for the volume reduction caused by the precipitation of supercritical carbon dioxide until the plastic material in the annular cavity is completely solidified.

[0011] A second aspect of the present invention provides a smart ring, comprising: An annular element, the annular element comprising an outer annular shell, an inner annular shell, a dough ring and a dough cover, the outer annular shell and the inner annular shell are arranged opposite to each other, the bottom periphery of the outer annular shell is connected to the bottom periphery of the inner annular shell, the top periphery of the outer annular shell is connected to the dough ring, the outer annular shell, the inner annular shell and the dough ring jointly define an annular cavity, an injection port communicating with the annular cavity is formed between the dough ring and the top periphery of the inner annular shell, and the dough cover is arranged on the injection port; An electronic component, wherein the electronic component is disposed in the annular cavity; The filler is formed by solidifying a plastic material and is filled in the annular cavity.

[0012] Optionally, the inner annular shell is made of plastic or titanium; and / or, The outer annular shell is made of at least one of titanium, gold, K gold, pure silver or jade; and / or, The material of the face ring is at least one of titanium, gold, K gold, pure silver or jade; and / or, The material of the face cover is at least one of titanium, gold, K gold, pure silver or jade.

[0013] Optionally, the electronic components include a circuit board and a battery; The circuit board is electrically connected to the battery; The circuit board and the battery are respectively arranged at two positions 180 degrees apart in the circumferential direction in the annular cavity, so that the weight distribution of the smart ring is balanced.

[0014] Optionally, a charging interface is provided on the inner annular shell, and the electronic component includes a charging component which is arranged in the annular cavity and is electrically connected to the battery and the circuit board respectively, and the charging component is exposed through the charging interface.

[0015] The technical solution provided by the embodiments of the present application has at least the following advantages: First, the process effectively displaces all air by injecting supercritical carbon dioxide for displacement into the annular cavity and the compensation cavity, thus avoiding the formation of bubbles at the source. Supercritical carbon dioxide has the characteristics of low viscosity like gas and high density like liquid, which can penetrate into every tiny space in the annular cavity and ensure the complete exclusion of air. Secondly, the pre-formulated plastic material is mixed with supercritical carbon dioxide for mixing to form a low-viscosity plastic mixture, which significantly reduces the viscosity of the material and improves its fluidity. This low-viscosity mixture can evenly fill all corners of the annular cavity during the injection process, solving the problem of uneven filling in traditional methods. At the same time, maintaining a pressure higher than the critical pressure of supercritical carbon dioxide during the injection process further ensures the uniform distribution of the material and the effective suppression of bubbles.

[0016] The process of the present invention achieves the slow precipitation of supercritical carbon dioxide and the gradual deposition and solidification of the plastic material by precisely controlling the temperature and pressure. Although the final solidification temperature of the plastic material is similar to that of the traditional method, the present solution significantly improves the solidification process by slowly increasing the temperature and precisely controlling the pressure. This progressive temperature control helps to reduce thermal shock and reduces the risk of damage to electronic components. In particular, the present invention cleverly designs a compensation cavity structure, utilizing the natural flow of the low-viscosity plastic mixture in the compensation cavity to timely replenish the portion of the mixture volume reduction in the annular cavity caused by the precipitation of supercritical carbon dioxide. This design effectively solves the problem of incomplete filling caused by material shrinkage and ensures the accuracy and integrity of the molded product. In addition, the use of supercritical carbon dioxide improves the thermal conductivity of the material, helps to disperse heat more evenly during the solidification process, and reduces local overheating. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0018] Figure 1 is a flow chart of the production process of the annular wearable component of the present invention; Figure 2 It is a cross-sectional schematic diagram of an embodiment of a smart ring of the present invention.

[0019] Description of Figure Numbers: 1. Ring element; 11. Outer ring shell; 12. Inner ring shell; 121. Charging port; 122. Inner ring wall; 123. Inner ring abutting wall; 13. Face ring; 131. Outer ring wall; 132. Outer ring abutting wall; 14. Face cover; 15. Ring cavity; 16. Injection molding port; 2. Electronic component; 21. Circuit board; 22. Battery; 23. Charging component; 3. Filler.

[0020] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0023] In addition, the descriptions of "first", "second", etc. in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, "and / or" in the full text includes three solutions. Taking A and / or B as an example, it includes technical solution A, technical solution B, and technical solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, which must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0024] An embodiment of the present application provides a production process for a ring-shaped wearable component. Figure 1 A flow chart of a production process of a ring-shaped wearable component provided in one embodiment of the present application.

[0025] See also Figure 1S1, providing an annular element 1 and a mold, wherein an annular cavity 15 is formed in the annular element 1, an injection port 16 connected to the annular cavity 15 is opened on the annular element 1, and a cavity matching the annular element 1 and a compensation cavity connected to the cavity are provided in the mold; Specifically, in this embodiment, the annular element 1 includes an outer annular shell 11, an inner annular shell 12 and a face ring 13. The outer annular shell 11 and the inner annular shell 12 can be made of different materials. For example, the outer annular shell 11 can be made of materials such as titanium, gold, K gold, pure silver or jade, which not only have good strength and durability, but also meet the aesthetic needs of the wearer. The inner annular shell 12 is usually made of plastic material, because plastic has good processing performance and electrical insulation, which is conducive to the installation and protection of the electronic component 2. In addition, the inner annular shell 12 can also be made of titanium metal material, which is insulated through process technology to support the hardness and non-deformation advantages of the filler 3. An annular cavity 15 is formed between the outer annular shell 11 and the inner annular shell 12, and the annular cavity 15 is used to accommodate the electronic component 2. The electronic component 2 includes but is not limited to an optical sensor, a circuit board 21, a charging component 23 and a battery 22. Among them, the optical sensor is a key component for realizing the health monitoring function, and is usually installed near the inner annular shell 12. In order to ensure that the optical sensor can accurately detect the wearer's physiological signals, a light-transmitting window corresponding to the position of the optical sensor needs to be provided on the inner annular shell 12. This light-transmitting window is usually made of transparent materials, such as optical grade plastic or glass, to ensure that the light signal can pass through without obstacles. In the actual manufacturing process, the inner annular shell 12 can first be made into a basic shape by injection molding, and then a light-transmitting window is opened at the corresponding position, and finally the transparent material is fixed at the window position.

[0026] The assembly of the ring element 1 requires precise craftsmanship, please refer to Figure 2 Specifically, first, the circuit board 21, the charging component 23 and the battery 22 are wound inside the inner annular shell 12, and then the insulating tape is wrapped around to fix the circuit board 21 and the battery 22 inside the cavity of the inner annular shell 12, and then the bottom periphery of the inner annular shell 12 and the bottom periphery of the outer annular shell 11 are bonded and fixed with glue, and finally, the top periphery of the outer annular shell 11 and the dough ring 13 are fixed together by interference fit, and a proper amount of sealant is added to strengthen the fixation. The above-mentioned injection port 16 is formed between the dough ring 13 and the top periphery of the inner annular shell 12.

[0027] The mold mainly consists of two core parts: the male mold and the female mold. Their precise matching forms the key structure for molding ring-shaped wearable parts.

[0028] The main body of the male mold includes an inner arc wall corresponding to the outer surface of the outer annular shell 11, and the inner arc wall accurately replicates the outer contour of the outer annular shell 11. At the top of the inner arc wall, the male mold extends upward to form an outer retaining wall. This outer retaining wall is an upright structure. The male mold is made of high-strength tool steel, such as H13 or P20 steel, which has excellent heat resistance and wear resistance and can maintain stable size and shape in high temperature and high pressure injection molding environments. The female mold includes an outer arc wall corresponding to the inner surface of the inner annular shell 12, and the outer arc wall accurately matches the inner contour of the inner annular shell 12. Similar to the male mold, the female mold also extends upward at the top of the outer arc wall to form an inner retaining wall. The inner retaining wall is also an upright structure and is arranged opposite to the outer retaining wall of the male mold. The material selection of the female mold is the same as that of the male mold, and high-quality tool steel is also used to ensure stability and durability during the injection molding process.

[0029] When the male and female molds are closed, the two arcuate walls (inner arcuate wall and outer arcuate wall) are precisely butted together to form a ring-shaped cavity. This cavity precisely envelops the annular element 1. The space between the outer retaining wall of the male mold and the inner retaining wall of the female mold forms a compensation cavity connected to the injection port 16. The design of the compensation cavity allows additional material to flow into the annular cavity 15 during the injection and curing process to compensate for the volume shrinkage caused by the precipitation of supercritical carbon dioxide. The volume of the compensation cavity is usually designed to be 5% to 15% of the volume of the annular cavity 15. This ratio is accurately calculated based on the characteristics of the plastic material (epoxy resin) used and the amount of supercritical carbon dioxide used.

[0030] The height and spacing of the outer and inner baffles need to be carefully designed to ensure that the volume of the compensation cavity is appropriate and that the material flow can be effectively guided. The surfaces of the two baffles require high-precision machining and surface treatment to reduce the friction resistance of the material during the flow process. Usually, the surfaces of the baffles (outer and inner baffles) are mirror polished.

[0031] Please continue reading Figure 1 , S2, placing the annular element 1 in the cavity, wherein the outer wall surface of the annular element 1 is in contact with the inner wall surface of the cavity, and the annular cavity 15 is connected with the compensation cavity through the injection port 16; In one embodiment of the present invention, the annular element 1 comprises an outer annular wall 131 and an inner annular wall 122 which are arranged opposite to each other, and the injection port 16 is formed between the outer annular wall 131 and the inner annular wall 122; The mold comprises an annular outer side wall and an annular inner side wall which are arranged opposite to each other, wherein the compensation cavity and a fluid passage communicating with the compensation cavity are formed between the annular outer side wall and the annular inner side wall; The distance between the annular outer side wall and the annular inner side wall is smaller than the distance between the outer annular wall 131 and the inner annular wall 122; wherein, After the annular element 1 is placed in the mold cavity, the inner wall surface of the annular outer wall and the inner wall surface of the annular inner wall are both located between the outer annular wall 131 and the inner annular wall 122, and the low-viscosity plastic mixture flows into the compensation cavity through the fluid port, and flows into the annular cavity 15 under the guidance of the inner wall surface of the annular outer wall or the inner wall surface of the annular inner wall.

[0032] Specifically, see Figure 2 The outer annular wall 131 is actually the side wall of the face ring 13 facing the inner annular shell 12, while the inner annular wall 122 is the top periphery of the inner annular shell 12.

[0033] The annular outer side wall is formed by the structure of the outer retaining wall mentioned above, and the annular inner side wall is formed by the structure of the inner retaining wall mentioned above.

[0034] The spacing between the annular outer side wall and the annular inner side wall of the mold is designed to be smaller than the spacing between the outer annular wall 131 and the inner annular wall 122 of the annular element 1. This design has the following advantages: it ensures that during the injection molding process, the material is prevented from flowing to the top of the dough ring 13 and the top of the inner annular shell 12. It helps to control the flow direction and speed of the material. For example, for an injection port 16 with a spacing of 3 mm, the corresponding spacing in the mold may be designed to be 2.8 mm. This 0.2 mm difference seems small, but it plays a key role in controlling the flow of the material.

[0035] In the actual injection molding process, the low-viscosity plastic mixture first flows into the compensation cavity through the fluid port. Subsequently, under the guidance of the inner wall surface of the annular outer wall or the inner wall surface of the annular inner wall, the material further flows into the annular cavity 15. This guided flow design effectively prevents material turbulence and reduces the formation of bubbles. For example, by designing micron-level guide lines on the mold wall, the flow path of the material can be further optimized. The depth of these lines is usually between 10 and 50 microns and the width is between 50 and 200 microns.

[0036] In one embodiment of the present invention, an outer annular abutting wall 132 is convexly formed on the outer annular wall 131, and an inner annular abutting wall 123 is convexly formed on the inner annular wall 122; wherein, After the annular element 1 is placed in the cavity, the annular outer side wall is moved to make its end abut against the outer annular abutting wall 132 , and the annular inner side wall is moved to make its end abut against the inner annular abutting wall 123 .

[0037] Specifically, the outer and inner walls in the mold each consist of two key parts: a fixed part and a moving part. The moving part of the outer wall is the annular outer wall, while the moving part of the inner wall constitutes the annular inner wall. The core purpose of this design is to achieve precise sealing and positioning during the injection molding process.

[0038] The outer annular wall 131 of the annular element 1 is provided with an outer annular abutting wall 132, and the inner annular wall 122 is provided with an inner annular abutting wall 123. When the annular element 1 is placed in the cavity, the outer annular wall (i.e., the moving part of the outer retaining wall) moves up and down until its end is tightly abutted against the outer annular abutting wall 132. Similarly, the inner annular wall (i.e., the moving part of the inner retaining wall) also moves up and down until it is precisely in contact with the inner annular abutting wall 123. This two-way abutment mechanism creates a highly sealed injection molding environment.

[0039] The main purpose of this design is to prevent plastic material from penetrating into the tiny gap between the outer wall of the annular element 1 and the inner wall of the cavity during the injection process. Without this sealing mechanism, even a gap of 0.01 mm may cause material leakage, thereby affecting the precision and appearance quality of the product. Through the precise abutment of the outer annular wall and the inner annular wall, an almost perfect sealing environment is created, ensuring that the injected material can only flow along the preset path and fill the designated annular cavity 15.

[0040] Please continue reading Figure 1 , S3, injecting supercritical carbon dioxide for replacement into the annular cavity 15 and the compensation cavity to replace all the air in the annular cavity 15 and the compensation cavity; In one embodiment of the present invention, the S3 includes: S3.1, placing the mold with the annular element 1 in a high-pressure reactor, wherein the high-pressure reactor includes an inlet valve and an exhaust valve; S3.2, sealing the autoclave and adjusting the internal temperature of the autoclave to 35-40° C.; S3.3, open the exhaust valve, and inject supercritical carbon dioxide for replacement into the high-pressure reactor through the inlet valve, with an initial injection pressure of 80-100 bar; S3.4, after continuously injecting supercritical carbon dioxide for replacement for 15-20 minutes, close the exhaust valve and the inlet valve to maintain the pressure of the high-pressure reactor.

[0041] Specifically, first, the mold with the ring element 1 is carefully placed in the autoclave. This autoclave is a specially designed device, usually made of high-strength alloy steel, capable of withstanding pressures up to 200 bar. The autoclave is equipped with an inlet valve and an exhaust valve, which play a vital role in the entire process. The inlet valve is used to control the injection of supercritical carbon dioxide, while the exhaust valve is used to exhaust the air in the autoclave and control the internal pressure.

[0042] After the mold is placed, the next step is to seal the autoclave. Usually, the autoclave is sealed with high-performance O-rings or metal gaskets, which can maintain good sealing performance under high pressure and high temperature environments. After the sealing is completed, the internal temperature of the autoclave is adjusted. The temperature adjustment to the range of 35-40℃ is carefully calculated because this temperature is slightly higher than the critical temperature of carbon dioxide (31.1℃), which is conducive to maintaining the supercritical state of carbon dioxide. Temperature control is usually achieved through external heating elements on the outer wall of the reactor or built-in internal heating elements, and multiple temperature sensors are used to ensure the uniformity of the temperature throughout the reactor.

[0043] When the temperature reaches the set range, open the exhaust valve. The purpose of this step is to create a flow path for the supercritical carbon dioxide to be injected. Then, start injecting supercritical carbon dioxide for replacement through the inlet valve. The initial injection pressure is set at 80-100bar. This pressure range is much higher than the critical pressure of carbon dioxide (73.8bar), ensuring that the carbon dioxide always remains in a supercritical state. Precise control of pressure is usually achieved through high-precision pressure sensors and electronic control valves. For example, for a 50-liter high-pressure reactor, the initial injection rate may be set at 2-3 liters per minute (volume under standard conditions). This rate can ensure rapid replacement without causing a sudden change in temperature in the reactor due to too fast injection.

[0044] The injection of supercritical carbon dioxide lasts for 15-20 minutes, which is the optimal time determined after repeated tests. In this process, supercritical carbon dioxide can quickly penetrate into every corner of the mold and effectively replace all the air with its unique physical properties (low viscosity like gas and high density like liquid). In this process, the gas discharged through the exhaust valve will gradually change from air to pure carbon dioxide. This change can be monitored by an online gas analyzer. When the concentration of carbon dioxide in the exhaust gas reaches more than 99.9%, it can be considered that the replacement is basically completed.

[0045] After the 15-20 minute injection process, the operator will first close the exhaust valve and then the inlet valve. This order is very important to ensure that sufficient pressure is maintained in the autoclave. At this point, the pressure in the autoclave is usually stable at around 90-110 bar, which is enough to ensure that the carbon dioxide remains in a supercritical state, creating ideal conditions for the subsequent injection molding process.

[0046] This process of air displacement using supercritical carbon dioxide has several significant advantages. First, it can completely remove the air from the mold and the annular cavity 15, which is crucial to preventing bubbles from appearing in the final product. Second, supercritical carbon dioxide has excellent permeability and can enter tiny spaces that are difficult to reach with traditional methods, ensuring the integrity of the displacement. Furthermore, this process is carried out at relatively mild temperatures and will not cause thermal damage to the sensitive electronic components 2 within the annular element 1. Finally, by precisely controlling temperature and pressure, this process creates an ideal environment for subsequent injection molding, which is conducive to obtaining high-quality molding results.

[0047] Please continue reading Figure 1 S4, mixing the pre-prepared plastic material with the supercritical carbon dioxide for mixing to form a low-viscosity plastic mixture; injecting the low-viscosity plastic mixture into the annular cavity 15 and the compensation cavity, and maintaining the pressure higher than the critical pressure of the supercritical carbon dioxide during the injection process; In one embodiment of the present invention, the S4 comprises: S4.1, mixing the pre-prepared plastic material with supercritical carbon dioxide for mixing in a high-pressure mixer for 5-10 minutes to form a low-viscosity plastic mixture; S4.2, controlling the temperature of the high-pressure mixer to 40-50° C. and the pressure to 100-120 bar; S4.3, opening the injection valve on the high-pressure reactor connected to the mold, injecting the low-viscosity plastic mixture into the annular cavity 15 and the compensation cavity, and controlling the injection rate to be 0.1-0.5 ml / s; S4.4, during the injection process, the pressure in the annular cavity 15 and the compensation cavity is maintained at 110-130 bar; S4.5, after the injection is completed, close the injection valve to ensure that the low-viscosity plastic mixture fills the annular cavity 15 and the compensation cavity.

[0048] Specifically, in the embodiments of the present application, the plastic material is preferably epoxy resin. Of course, in other embodiments, it may also be one or a combination of phenolic resin, polyurethane resin, unsaturated polyester resin, silicone resin, melamine formaldehyde resin, and alkyd resin. These materials exhibit good fluidity and plasticity during the injection and molding stages, and can accurately fill tiny spaces. After curing, they have excellent mechanical strength, weather resistance and electrical insulation.

[0049] The mixing process lasts for 5-10 minutes. This time length is the optimal value determined through repeated experiments. It can ensure sufficient mixing without causing changes in material properties due to excessive time. During the mixing process, the temperature of the high-pressure mixer is precisely controlled within the range of 40-50°C. This temperature range has been carefully selected to ensure that the plastic material maintains good fluidity without triggering the cross-linking reaction of the material. At the same time, the pressure in the mixer is maintained at 100-120bar. This pressure range ensures that carbon dioxide is always in a supercritical state and can be fully dissolved in the plastic material. For example, for a high-pressure mixer with a volume of 5 liters, the temperature control accuracy is usually required to reach ±0.5°C, and the pressure control accuracy needs to reach ±1bar. This precision control is achieved through high-performance temperature sensors, pressure sensors and PID control systems.

[0050] After mixing, the low-viscosity plastic mixture has unique rheological properties, and its viscosity may be 50% or more lower than that of the original plastic material. This low viscosity property is crucial for subsequent precision injection, because it ensures that the material can fill every corner of the annular cavity 15 and the compensation cavity, especially some tiny structural features.

[0051] Next, open the injection valve connected to the mold on the autoclave and start injecting the low-viscosity plastic mixture into the annular cavity 15 and the compensation cavity. The injection rate is controlled in the range of 0.1-0.5 ml / s. The selection of this rate range is the result of weighing multiple factors. A slower injection rate helps to avoid material turbulence and reduce the formation of bubbles. For a typical smart ring, the total volume of the annular cavity 15 and the compensation cavity is about 2-3 ml. At this injection rate, the entire injection process will last 4-30 seconds.

[0052] During the entire injection process, the pressure in the annular cavity 15 and the compensation cavity is strictly controlled within the range of 110-130bar. This pressure range is higher than the pressure in the mixer, in order to ensure that the low-viscosity plastic mixture does not cause the dissolved carbon dioxide to precipitate prematurely due to a sudden drop in pressure after entering the cavity. Pressure control is achieved through a high-precision pressure sensor set on the mold and a feedback control loop connected to the injection system. This precise pressure control not only helps to maintain the low viscosity state of the material, but also promotes uniform distribution of the material and reduces the occurrence of defects such as shrinkage and warpage.

[0053] When the low-viscosity plastic mixture completely fills the annular cavity 15 and the compensation cavity, the injection valve is immediately closed. This closing action needs to be fast and accurate, and can be achieved by using a high-response solenoid valve or pneumatic valve, and the response time can be controlled within 10 milliseconds. The purpose of quickly closing the valve is to prevent the material from flowing back and ensure that the cavity remains full. After closing the valve, the system will immediately perform a quick pressure check to confirm that the pressure in the annular cavity 15 and the compensation cavity is maintained within the set range.

[0054] The advantage of this whole process is that it can achieve precise control of the material state and the filling process. By using supercritical carbon dioxide, the viscosity of the plastic material is significantly reduced, allowing the material to be injected at relatively low temperature and pressure, which not only reduces the thermal stress on the electronic components 2 in the annular element 1, but also reduces the wear of the mold. The precisely controlled injection rate and pressure ensure that the material can be evenly filled into the complex cavity structure, greatly reducing the generation of defects such as bubbles and shrinkage marks. In addition, the design of the compensation cavity provides sufficient material reserves for subsequent material shrinkage compensation, which is crucial to improving the dimensional accuracy and surface quality of the product.

[0055] Please continue reading Figure 1 S5, controlling the temperature and pressure to gradually precipitate the supercritical carbon dioxide from the low-viscosity plastic mixture, and at the same time gradually depositing and solidifying the plastic material in the low-viscosity plastic mixture in the annular cavity 15; in this process, the low-viscosity plastic mixture in the compensation cavity is used to supplement the volume reduction of the low-viscosity plastic mixture in the annular cavity 15 caused by the precipitation of supercritical carbon dioxide; In one embodiment of the present invention, the S5 comprises: S5.1, controlling the temperature of the autoclave to 45-55°C for 30 minutes; S5.2, slowly reducing the pressure in the autoclave at a rate of 0.5-1 bar / min, so that supercritical carbon dioxide gradually precipitates from the low-viscosity plastic mixture; S5.3, gradually increasing the temperature of the autoclave to 60-70°C at a rate of 0.5°C / min, and maintaining the temperature for 60 minutes; S5.4, continue to reduce the pressure in the autoclave, and slow down the reduction rate to 0.3-0.5 bar / min; S5.5, raising the temperature of the autoclave to 70-80°C and maintaining it for 90 minutes; S5.6, slowly reducing the pressure in the autoclave to atmospheric pressure at a rate of 0.1-0.2 bar / min; S5.7, by means of a pressure sensor arranged in the high-pressure reactor, the pressure change in the annular cavity 15 is monitored to ensure that the low-viscosity plastic mixture in the compensation cavity can flow naturally into the annular cavity 15 to compensate for the volume reduction caused by the precipitation of supercritical carbon dioxide until the plastic material in the annular cavity 15 is completely solidified.

[0056] Specifically, controlling the curing process of the plastic material is a key step in ensuring product quality. This process begins with precisely controlling the temperature of the autoclave within the range of 45-55°C and maintaining this temperature for 30 minutes. This initial temperature range is carefully selected to be above the glass transition temperature of the epoxy resin system but below the rapid curing temperature, creating ideal starting conditions for the subsequent slow curing process. During these 30 minutes, the molecules in the low-viscosity plastic mixture begin to slowly move and align, preparing for the subsequent cross-linking reaction.

[0057] Next, the pressure in the autoclave is slowly reduced at a rate of 0.5-1 bar / min. This carefully controlled decompression process allows the supercritical carbon dioxide dissolved in the low-viscosity plastic mixture to gradually precipitate. The slow reduction of pressure is crucial to controlling the precipitation rate of carbon dioxide, because too fast precipitation will cause a large number of tiny bubbles to form in the material, affecting the mechanical properties and appearance quality of the product. For example, for a system with an initial pressure of 120 bar, it takes 2-4 hours to complete this decompression process, and this time span provides a sufficient time window for the initial curing of the material.

[0058] As the pressure decreases, the temperature of the autoclave begins to gradually increase to 60-70°C at a rate of 0.5°C / min and is maintained in this temperature range for 60 minutes. The setting of this heating process and the holding time is determined based on the curing kinetics of the epoxy resin system. The slow heating rate ensures the uniformity of the temperature distribution in the entire annular cavity 15 and avoids stress concentration caused by local overheating. At this stage, the cross-linking reaction between the epoxy resin molecules begins to accelerate, the network structure gradually forms, and the strength and modulus of the material begin to increase significantly.

[0059] After the 60-minute holding period, the pressure in the autoclave continued to decrease, but the rate of decrease (the rate of reducing the pressure in the autoclave) slowed down to 0.3-0.5 bar / min. This slower rate of decompression matches the increase in the degree of curing of the material, which can effectively prevent the formation of defects caused by the rapid precipitation of carbon dioxide when the viscosity of the material increases significantly. At the same time, the temperature of the autoclave was further increased to 70-80°C and maintained in this temperature range for 90 minutes. This higher temperature promotes complete cross-linking between epoxy resin molecules, ensuring that the material achieves the expected mechanical properties and thermal stability.

[0060] In the final stage of the entire curing process, the pressure in the autoclave is slowly reduced to atmospheric pressure, and the reduction rate is controlled at 0.1-0.2 bar / min. This extremely slow decompression process gives the material sufficient time to adapt to the pressure change and minimizes the accumulation of internal stress. At the same time, the pressure changes in the annular cavity 15 are continuously monitored by a high-precision pressure sensor set in the autoclave. This real-time monitoring is essential to ensure that the low-viscosity plastic mixture in the compensation cavity can flow naturally into the annular cavity 15, which supplements the volume reduction caused by the precipitation of supercritical carbon dioxide until the plastic material in the annular cavity 15 is completely cured.

[0061] This precisely controlled curing process has several significant advantages. First, through the precise control of temperature and pressure, uniform curing of plastic materials is achieved, avoiding the problems of local overheating or incomplete curing common in traditional processes. Second, the slow pressure release process effectively prevents the formation and growth of bubbles, significantly improving the internal quality and surface finish of the product. Furthermore, the design of the compensation cavity and the coordination of the pressure monitoring system ensure that the material can be replenished in time during the material shrinkage process, minimizing shrinkage stress and warpage deformation.

[0062] For example, for a smart ring with a diameter of 20mm, the entire curing process may last 6-8 hours. Although this time is relatively long, it ensures the high quality and consistency of the product. During this process, the pressure in the annular cavity 15 may gradually decrease from the initial 120bar to atmospheric pressure, while the temperature increases from 45°C to the final 75°C. Through this carefully designed temperature and pressure curve, the dimensional accuracy of the final product can be controlled within ±0.02mm, and the surface roughness can reach Ra0.4μm or better, which are far beyond the level of traditional injection molding process.

[0063] Please continue reading Figure 1 , S6, after the plastic material in the annular cavity 15 is completely solidified, the annular element 1 is taken out of the mold, cooled to room temperature and packaged.

[0064] Specifically, first, the autoclave is slowly cooled down to near room temperature, which usually takes 2-3 hours to ensure that stress is not generated inside the annular element 1 due to the rapid temperature change. Then, the autoclave is carefully opened and the mold is taken out. Next, the male and female molds of the mold are slowly separated by a precise mechanical device, such as a hydraulic or pneumatic system, to avoid any damage to the annular element 1.

[0065] After the annular element 1 is removed from the mold, the plastic material remaining at the injection port 16 is immediately and carefully cleaned. This cleaning process usually uses precision cutting tools or laser trimming equipment to ensure the accuracy of cleaning and the smoothness of the surface. For example, for a smart ring with a diameter of 20 mm, the cleaning accuracy of the residue at the injection port 16 usually needs to be controlled within 0.05 mm to ensure the sealing of the subsequent packaging.

[0066] After cleaning, the ring element 1 is placed in a thermostat with a temperature control precision of ±0.5°C and slowly cooled until it reaches room temperature. This slow cooling process usually takes 1-2 hours to further release internal stress and improve the dimensional stability of the product. After cooling, the ring element 1 is fully inspected using a high-precision three-dimensional coordinate measuring machine to ensure that its size and shape meet the design requirements.

[0067] Finally, the packaging process is performed, and the carefully designed cover 14 is placed at the injection port 16. The bottom of the cover 14 is precisely abutted against the inner annular abutting wall 123 and the outer annular abutting wall 132. This design can not only ensure the aesthetics of the packaging, but also improve the sealing effect. Glue is used to seal the connection between the cover 14 and the annular element 1.

[0068] Another embodiment of the present application further provides a smart ring, which is manufactured by the production process of the ring-shaped wearable component provided in the above embodiment. Figure 2 It is a cross-sectional schematic diagram of an embodiment of a smart ring.

[0069] The smart ring comprises: An annular element 1, the annular element 1 comprises an outer annular shell 11, an inner annular shell 12, a dough ring 13 and a dough cover 14, the outer annular shell 11 and the inner annular shell 12 are arranged opposite to each other, the bottom periphery of the outer annular shell 11 is connected to the bottom periphery of the inner annular shell 12, the top periphery of the outer annular shell 11 is connected to the dough ring 13, the outer annular shell 11, the inner annular shell 12 and the dough ring 13 jointly define an annular cavity 15, an injection port 16 communicating with the annular cavity 15 is formed between the dough ring 13 and the top periphery of the inner annular shell 12, and the dough cover 14 is covered on the injection port 16; An electronic component 2, wherein the electronic component 2 is disposed in the annular cavity 15; The filler 3 is formed by solidifying a plastic material, and the filler 3 is filled in the annular cavity 15 .

[0070] Specifically, the smart ring formed by a combination of multiple structures allows for more flexible material selection and a more sophisticated manufacturing process. Compared with the ring with an integrated physical structure, the smart ring of the present invention has significantly improved material compatibility. Precious metals are used on the outside to improve the appearance and durability, and plastics are used on the inside to optimize the working environment of the electronic components 2. Secondly, manufacturing flexibility is greatly enhanced, and each component can be manufactured and optimized separately. At the same time, the split structure makes it easier to repair or upgrade when necessary without replacing the entire ring. In addition, this design provides more possibilities for personalized customization, and users can more easily replace the outer ring shell 11 of different materials or colors.

[0071] In general, this design takes into account functionality, reliability and aesthetics, providing more possibilities for mass production and personalized customization of smart rings, enabling smart rings to reach a higher level in performance, appearance and user experience.

[0072] In a specific implementation, the material of the inner annular shell 12 is plastic or titanium. The material of the outer annular shell 11 is at least one of titanium, gold, K gold, pure silver or jade. The material of the face ring 13 is at least one of titanium, gold, K gold, pure silver or jade. The material of the face cover 14 is at least one of titanium, gold, K gold, pure silver or jade.

[0073] Optionally, the electronic component 2 includes a circuit board 21 and a battery 22; The circuit board 21 is electrically connected to the battery 22; The circuit board 21 and the battery 22 are respectively arranged at two positions 180 degrees apart in the circumferential direction in the annular cavity 15 so that the weight distribution of the smart ring is balanced.

[0074] Specifically, the circuit board 21 and the battery 22 are arranged at two relative positions in the annular cavity 15, with an angle of 180 degrees between them. This means that if the smart ring is placed flat and viewed from above, the circuit board 21 and the battery 22 are located at the two ends of a diameter.

[0075] The purpose of this design is mainly reflected in two aspects: weight distribution and wearing direction. First, from the perspective of weight distribution, the circuit board 21 and the battery 22 are usually the two heaviest components inside the smart ring. Placing them in relative positions can make the weight distribution more balanced, avoiding discomfort caused by one side of the ring being too heavy when worn. This balanced weight distribution can improve wearing comfort, so that users will not feel excessive pressure on one side of the finger when wearing it for a long time.

[0076] Secondly, in terms of wearing orientation, this design allows users to wear the smart ring at any angle without affecting its functionality or comfort. No matter how the ring is rotated, the weight distribution always remains balanced. This feature is particularly important because it eliminates the need for users to consider a specific wearing orientation, increasing the convenience of the product.

[0077] Optionally, a charging interface 121 is provided on the inner annular shell 12, and the electronic component 2 includes a charging component 23 disposed in the annular cavity 15 and electrically connected to the battery 22 and the circuit board 21, respectively, and the charging component 23 is exposed through the charging interface 121. Providing the charging interface 121 on the inner annular shell 12 instead of the outer annular shell 11 can ensure the charging function without affecting the appearance design of the ring, so that the product remains beautiful and neat in the non-charging state.

[0078] The charging component 23 is exposed through the charging interface 121, which means that the user can directly connect the charging cable to the charging interface 121 and charge the ring without disassembling or opening it. This design greatly improves the convenience of daily use of the product, and the user can easily charge the smart ring without complicated operations.

[0079] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A production process for an annular wearable component, characterized in that: include: S1, providing an annular element and a mold, wherein an annular cavity is formed in the annular element, an injection port connected to the annular cavity is opened on the annular element, a cavity matching the annular element and a compensation cavity connected to the cavity are provided in the mold; S2, placing the annular element in the cavity, wherein the outer wall surface of the annular element fits the inner wall surface of the cavity, and the annular cavity is connected with the compensation cavity through the injection port; S3, injecting supercritical carbon dioxide for replacement into the annular cavity and the compensation cavity to replace all the air in the annular cavity and the compensation cavity; S4, mixing the pre-prepared plastic material with supercritical carbon dioxide for mixing to form a low-viscosity plastic mixture; injecting the low-viscosity plastic mixture into the annular cavity and the compensation cavity, and maintaining a pressure higher than the critical pressure of the supercritical carbon dioxide during the injection process; S5, controlling the temperature and pressure to gradually precipitate the supercritical carbon dioxide from the low-viscosity plastic mixture, and at the same time gradually depositing and solidifying the plastic material in the low-viscosity plastic mixture in the annular cavity; in this process, the low-viscosity plastic mixture in the compensation cavity is used to supplement the volume reduction of the low-viscosity plastic mixture in the annular cavity caused by the precipitation of the supercritical carbon dioxide; S6, after the plastic material in the annular cavity is completely solidified, the annular element is taken out from the mold, cooled to room temperature and packaged.

2. The production process of the annular wearable component according to claim 1, characterized in that: The annular element comprises an outer annular wall and an inner annular wall which are arranged opposite to each other, and the injection port is formed between the outer annular wall and the inner annular wall; The mold comprises an annular outer side wall and an annular inner side wall which are arranged opposite to each other, wherein the compensation cavity and a fluid passage communicating with the compensation cavity are formed between the annular outer side wall and the annular inner side wall; The distance between the annular outer side wall and the annular inner side wall is smaller than the distance between the outer annular wall and the inner annular wall; wherein, After the annular element is placed in the mold cavity, the inner wall surface of the annular outer wall and the inner wall surface of the annular inner wall are both located between the outer annular wall and the inner annular wall, and the low-viscosity plastic mixture flows into the compensation cavity through the fluid port and flows into the annular cavity under the guidance of the inner wall surface of the annular outer wall or the inner wall surface of the annular inner wall.

3. The production process of the annular wearable component according to claim 2, characterized in that: An outer annular abutting wall is convexly provided on the outer annular wall, and an inner annular abutting wall is convexly provided on the inner annular wall; wherein, After the annular element is placed in the cavity, the annular outer side wall is moved to abut the end thereof against the outer annular abutting wall, and the annular inner side wall is moved to abut the end thereof against the inner annular abutting wall.

4. The production process of the annular wearable component according to claim 1, characterized in that: The S3 includes: S3.1, placing the mold with the annular element in a high pressure reactor, wherein the high pressure reactor includes an inlet valve and an exhaust valve; S3.2, sealing the autoclave and adjusting the internal temperature of the autoclave to 35-40° C.; S3.3, open the exhaust valve, and inject supercritical carbon dioxide for replacement into the high-pressure reactor through the inlet valve, with an initial injection pressure of 80-100 bar; S3.4, after continuously injecting supercritical carbon dioxide for replacement for 15-20 minutes, close the exhaust valve and the inlet valve to maintain the pressure of the high-pressure reactor.

5. The production process of the annular wearable component according to claim 4, characterized in that: The S4 comprises: S4.1, mixing the pre-prepared plastic material with supercritical carbon dioxide for mixing in a high-pressure mixer for 5-10 minutes to form a low-viscosity plastic mixture; S4.2, controlling the temperature of the high-pressure mixer to 40-50° C. and the pressure to 100-120 bar; S4.3, opening the injection valve on the high-pressure reactor connected to the mold, injecting the low-viscosity plastic mixture into the annular cavity and the compensation cavity, and controlling the injection rate to be 0.1-0.5 ml / s; S4.4, during the injection process, the pressure in the annular cavity and the compensation cavity is maintained at 110-130 bar; S4.5, after the injection is completed, close the injection valve to ensure that the low-viscosity plastic mixture fills the annular cavity and the compensation cavity.

6. The production process of the annular wearable component according to claim 5, characterized in that: The S5 comprises: S5.1, controlling the temperature of the autoclave to 45-55°C for 30 minutes; S5.2, slowly reducing the pressure in the autoclave at a rate of 0.5-1 bar / min, so that supercritical carbon dioxide gradually precipitates from the low-viscosity plastic mixture; S5.3, gradually increasing the temperature of the autoclave to 60-70°C at a rate of 0.5°C / min, and maintaining the temperature for 60 minutes; S5.4, continue to reduce the pressure in the autoclave, and slow down the reduction rate to 0.3-0.5 bar / min; S5.5, raising the temperature of the autoclave to 70-80°C and maintaining it for 90 minutes; S5.6, slowly reducing the pressure in the autoclave to atmospheric pressure at a rate of 0.1-0.2 bar / min; S5.7, by means of a pressure sensor disposed in the high-pressure reactor, the pressure change in the annular cavity is monitored to ensure that the low-viscosity plastic mixture in the compensation cavity can flow naturally into the annular cavity to compensate for the volume reduction caused by the precipitation of supercritical carbon dioxide until the plastic material in the annular cavity is completely solidified.

7. A smart ring, characterized in that: The smart ring is manufactured by the production process of the ring-shaped wearable component according to any one of claims 1 to 6, and the smart ring comprises: An annular element (1), the annular element (1) comprising an outer annular shell (11), an inner annular shell (12), a face ring (13) and a face cover (14), the outer annular shell (11) and the inner annular shell (12) being arranged opposite to each other, the bottom periphery of the outer annular shell (11) being connected to the bottom periphery of the inner annular shell (12), the top periphery of the outer annular shell (11) being connected to the face ring (13), the outer annular shell (11), the inner annular shell (12) and the face ring (13) jointly defining an annular cavity (15), an injection port (16) being formed between the face ring (13) and the top periphery of the inner annular shell (12) and communicating with the annular cavity (15), and the face cover (14) being arranged to cover the injection port (16); An electronic component (2), wherein the electronic component (2) is arranged in the annular cavity (15); A filler (3), wherein the filler (3) is formed by solidifying a plastic material, and the filler (3) is filled in the annular cavity (15).

8. The smart ring according to claim 7, characterized in that: The inner annular shell (12) is made of plastic or titanium; and / or, The outer annular shell (11) is made of at least one of titanium, gold, K gold, pure silver or jade; and / or, The material of the face ring (13) is at least one of titanium, gold, K gold, pure silver or jade; and / or, The material of the face cover (14) is at least one of titanium, gold, K gold, pure silver or jade.

9. The smart ring according to claim 7, characterized in that: The electronic component (2) comprises a circuit board (21) and a battery (22); The circuit board (21) is electrically connected to the battery (22); The circuit board (21) and the battery (22) are respectively arranged at two positions 180 degrees apart in the circumferential direction in the annular cavity (15) so that the weight distribution of the smart ring is balanced.

10. The smart ring according to claim 9, characterized in that: The inner annular shell (12) is provided with a charging interface (121), and the electronic component (2) includes a charging component (23) which is arranged in the annular cavity (15) and is electrically connected to the battery (22) and the circuit board (21) respectively, and the charging component (23) is exposed through the charging interface (121).

Citation Information

Patent Citations

  • Method of injection molding using ribs and apparatus therefor

    CN108136636A

  • Polymer micro-foaming device and process based on foaming-injection-molding blank making

    CN113001864A

  • Injection molding process of micro-adjustment type dust collector shell

    CN117698048A

  • Carbon dioxide injection device used for injection molding of thermoplastic resin

    JP2006327133A

  • Molding process of thermoplastic resin foam, and molding system

    JP2009090557A

Cited By

  • Production process of annular wearable part and intelligent ring

    CN118893791A

  • Production process for annular wearable article, and smart ring

    WO2026061555A1