Titanium magnesium phosphate solid electrolyte material, preparation method thereof and magnesium ion battery
By combining nano-scale raw materials with flux for solid phase sintering and crushing treatment, the problems of impurity generation and efficiency in the synthesis of traditional titanium phosphate electrolyte materials are solved, and the performance of magnesium ion batteries is significantly improved.
Patent Information
- Application Number
- CN202410825537.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-05
AI Technical Summary
There are problems of impurity generation and low efficiency in the synthesis of traditional titanium phosphate solid electrolyte materials, which affects its application in magnesium ion batteries.
The nano-scale magnesium source, titanium source, and phosphorus source are mixed with flux evenly and then solid phase sintering is performed, and then pulverized to improve purity and reaction efficiency. The flux promotes liquid phase reaction to replace solid phase reaction.
The purity and reaction efficiency of titanium magnesium phosphate solid electrolyte materials are improved, and the performance of magnesium ion batteries is enhanced.
Smart Images

Figure CN118894510A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium ion batteries, and in particular to a magnesium titanium phosphate solid electrolyte material and a preparation method thereof, and a magnesium ion battery. Background Art
[0002] At present, in the battery industry, the most comprehensive and widely used electrolyte materials are based on organic solvents. However, these organic electrolytes are very easy to generate heat during the conduction process, and even spontaneously combust and explode. As more and more news reports of spontaneous combustion accidents of new energy vehicles are reported, people are paying more and more attention to the safety of batteries. Solid electrolytes, as a new type of electrolyte material, have good chemical stability and are extremely safe. Therefore, the development of solid electrolytes is of great practical significance.
[0003] Lithium-ion batteries are one of the most widely used batteries at present. However, the reserves of lithium resources on the earth are limited, enough for humans to develop and utilize for only a few decades. Therefore, the development of the next generation of rechargeable ion batteries is urgent.
[0004] Magnesium-ion batteries have a higher volumetric energy density, magnesium is abundant on Earth, and its price is less than one-tenth of lithium. Therefore, many people believe that magnesium-ion batteries have the greatest potential to replace lithium-ion batteries.
[0005] Magnesium titanium phosphate is a solid electrolyte material. Nano-scale magnesium titanium phosphate can be directly used for coating battery separators, expanding the application of magnesium ion batteries in solid-state batteries. However, in the traditional method of synthesizing magnesium titanium phosphate, either the mixing is uneven, which easily generates impurities; or the synthesis efficiency is low, which is not conducive to wide application. Therefore, the development of a new process is of great practical significance for the synthesis of magnesium titanium phosphate solid electrolyte materials. Summary of the invention
[0006] Based on this, it is necessary to provide a magnesium titanium phosphate solid electrolyte material and a preparation method thereof and a magnesium ion battery in order to improve the reaction efficiency and purity.
[0007] A method for preparing a magnesium titanium phosphate solid electrolyte material comprises the following steps:
[0008] Providing nano-scale magnesium source, nano-scale titanium source and nano-scale phosphorus source;
[0009] Evenly mixing the nano-scale magnesium source, the nano-scale titanium source, the nano-scale phosphorus source and a flux to obtain a mixed material;
[0010] The mixed material is subjected to solid phase sintering treatment to obtain titanium magnesium phosphate powder; and
[0011] The magnesium titanium phosphate powder is pulverized to obtain the pulverized magnesium titanium phosphate, which is the magnesium titanium phosphate solid electrolyte material.
[0012] The preparation method of the above-mentioned magnesium titanium phosphate solid electrolyte material is simple to operate, and the particle size of the nano-scale magnesium source, nano-scale titanium source and nano-scale phosphorus source is small, which increases the specific surface area of the raw material powder, helps to improve the reaction activity, and thus improves the reaction efficiency; the flux makes the reaction between the raw materials of the present invention a liquid phase reaction, replacing the traditional solid phase reaction, greatly improving the sintering efficiency; further, it has been verified by experiments that the magnesium titanium phosphate solid electrolyte material obtained by the above-mentioned preparation method has a high purity.
[0013] In a feasible implementation, the nanoscale magnesium source, the nanoscale titanium source and the nanoscale phosphorus source are obtained by respectively subjecting the magnesium source, the titanium source and the phosphorus source to air flow milling treatment.
[0014] In a feasible implementation, the molar ratio of the magnesium element in the nanoscale magnesium source, the titanium element in the nanoscale titanium source, and the phosphorus element in the nanoscale phosphorus source is (1.02-1.05):4:6.
[0015] In a feasible implementation, the nanoscale magnesium source is selected from at least one of magnesium oxide, magnesium hydroxide and magnesium carbonate;
[0016] The nano-scale titanium source is titanium dioxide;
[0017] The nanoscale phosphorus source is selected from at least one of white phosphorus, red phosphorus, phosphorus pentoxide and ammonium dihydrogen phosphate.
[0018] In a feasible implementation, the flux is selected from at least one of lithium carbonate, lithium fluoride, sodium carbonate and potassium carbonate.
[0019] In a feasible implementation, the mass of the flux accounts for 3wt% to 10wt% of the total mass of the nanoscale magnesium source, the nanoscale titanium source and the nanoscale phosphorus source.
[0020] In a feasible implementation, the temperature of solid phase sintering is 900° C. to 1500° C., and the time of solid phase sintering is 2 h to 20 h.
[0021] In a feasible implementation, the magnesium titanium phosphate powder is crushed to obtain the crushed magnesium titanium phosphate by:
[0022] The magnesium titanium phosphate powder is placed in a jaw crusher for crushing to obtain magnesium titanium phosphate powder with a particle size of 0.1 cm to 1 cm;
[0023] The titanium magnesium phosphate powder with a particle size of 0.1 cm to 1 cm is placed in a ball mill for ball milling, the speed of the ball mill is 100 rpm to 400 rpm, and the ball milling time is 1 h to 10 h to obtain a titanium magnesium phosphate powder with a particle size of 5 μm to 50 μm; and
[0024] The magnesium titanium phosphate powder with a particle size of 5 μm to 50 μm is subjected to a jet mill to obtain pulverized magnesium titanium phosphate with a particle size of 0.3 μm to 0.9 μm.
[0025] A magnesium titanium phosphate solid electrolyte material is prepared by any of the above methods for preparing magnesium titanium phosphate solid electrolyte materials.
[0026] It has been verified through experiments that the magnesium titanium phosphate solid electrolyte material obtained by the above preparation method has a high purity.
[0027] A magnesium ion battery comprises the above-mentioned magnesium titanium phosphate solid electrolyte material.
[0028] Compared with the conventional magnesium ion battery using magnesium titanium phosphate solid electrolyte material containing impurities, the magnesium ion battery of the technical solution of the present invention has better performance due to the higher purity of the magnesium titanium phosphate solid electrolyte material. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a flow chart of a method for preparing a magnesium titanium phosphate solid electrolyte material according to one embodiment of the present invention;
[0030] Figure 2 The X-ray diffraction pattern of the magnesium titanium phosphate solid electrolyte material prepared in Example 1;
[0031] Figure 3 The X-ray diffraction pattern of the magnesium titanium phosphate solid electrolyte material prepared in Example 2;
[0032] Figure 4 This is an X-ray diffraction pattern of the magnesium titanium phosphate solid electrolyte material prepared in Example 3;
[0033] Figure 5 This is an X-ray diffraction pattern of the magnesium titanium phosphate solid electrolyte material prepared in Comparative Example 1;
[0034] Figure 6 This is the X-ray diffraction pattern of the magnesium titanium phosphate solid electrolyte material prepared in Comparative Example 2. DETAILED DESCRIPTION
[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0037] See also Figure 1 A method for preparing a magnesium titanium phosphate solid electrolyte material according to an embodiment of the present invention comprises the following steps:
[0038] S10. Provide a nano-scale magnesium source and a nano-scale titanium source.
[0039] Among them, nano-scale magnesium source refers to a magnesium source with a particle size of nanometers, preferably a particle size of 100nm to 1000nm; nano-scale titanium source refers to a magnesium and titanium particle size of nanometers, preferably a particle size of 100nm to 1000nm. This uniform and fine particle distribution can increase the specific surface area of the raw material powder, help to improve the reaction activity, and can effectively reduce the insulation time during subsequent sintering, thereby improving the reaction efficiency.
[0040] In a feasible implementation, the nano-scale magnesium source and the nano-scale titanium source are obtained by respectively treating the magnesium source and the titanium source with air flow milling. Generally, the particle size of the magnesium source and the titanium source directly purchased is 10 μm to 100 μm. After air flow milling, nano-scale powder raw materials can be obtained. Of course, nano-scale magnesium source, titanium source and phosphorus source can also be purchased.
[0041] In a feasible implementation, the molar ratio of the magnesium element in the nanoscale magnesium source, the titanium element in the nanoscale titanium source, and the phosphorus element in the phosphorus source is (1.02-1.05):4:6.
[0042] In a feasible implementation, the nanoscale magnesium source is selected from at least one of magnesium oxide, magnesium hydroxide and magnesium carbonate.
[0043] In a feasible implementation, the nano-scale titanium source is titanium dioxide.
[0044] In a feasible implementation, the nanoscale phosphorus source is selected from at least one of phosphorus pentoxide, ammonium dihydrogen phosphate and diammonium hydrogen phosphate.
[0045] S20, uniformly mixing the nano-scale magnesium source, nano-scale titanium source, nano-scale phosphorus source and flux in step S10 to obtain a mixed material.
[0046] In step S20, the order of mixing the nano-magnesium source, the nano-titanium source, the nano-phosphorus source and the flux is not limited. In addition, the mixing method can be electric stirring and mixing by a mixer, which can fully mix the materials.
[0047] In a feasible implementation, the flux is selected from at least one of lithium carbonate, lithium fluoride, sodium carbonate and potassium carbonate.
[0048] In a feasible implementation, the weight of the flux accounts for 3 wt% to 10 wt% of the total weight of the nano-scale magnesium source, the nano-scale titanium source and the nano-scale phosphorus source.
[0049] S30, subjecting the mixed material obtained in step S20 to solid phase sintering to obtain magnesium titanium phosphate powder.
[0050] In step S30, when the temperature of the reaction system rises to the temperature of solid phase sintering, the flux melts into liquid, and the original solid phase sintering environment is changed into a liquid phase environment, which is conducive to the dispersion of the mixed materials, and accelerates the reaction between the raw materials, greatly improving the sintering efficiency. During the solid phase sintering process, the flux can be gradually volatilized to avoid affecting the purity of the product. Based on this, in the preparation method of the magnesium titanium phosphate solid electrolyte material of the present invention, the melting point of the flux needs to be lower than the temperature of solid phase sintering.
[0051] In a feasible implementation, the solid phase sintering temperature is 900°C to 1500°C, and the solid phase sintering time is 2h to 20h. At this time, the raw materials can be fully reacted, and the flux can be fully volatilized, which reduces energy consumption and avoids the agglomeration of magnesium titanium phosphate, which is not conducive to subsequent crushing.
[0052] S40, crushing the magnesium titanium phosphate powder obtained in step S30 to obtain crushed magnesium titanium phosphate, which is the magnesium titanium phosphate solid electrolyte material.
[0053] In a feasible implementation, the magnesium titanium phosphate powder is crushed to obtain the crushed magnesium titanium phosphate by:
[0054] S41, putting the titanium magnesium phosphate powder into a jaw crusher for crushing to obtain titanium magnesium phosphate powder with a particle size of 0.1 cm to 1 cm.
[0055] S42, putting titanium magnesium phosphate powder with a particle size of 0.1 cm to 1 cm into a ball mill for ball milling, the rotation speed of the ball mill is 100 rpm to 400 rpm, the ball milling time is 1 h to 10 h, and obtaining titanium magnesium phosphate powder with a particle size of 5 μm to 50 μm.
[0056] S43, passing magnesium titanium phosphate powder with a particle size of 5 μm to 50 μm through a jet mill to obtain pulverized magnesium titanium phosphate with a particle size of 0.3 μm to 0.9 μm.
[0057] After the above-mentioned pulverization treatment, the obtained magnesium titanium phosphate powder has a small particle size, high dispersibility, and is not easy to agglomerate, which is beneficial to improving the ionic conductivity of the magnesium titanium phosphate solid electrolyte material and expanding the application of magnesium ions in solid-state batteries.
[0058] The preparation method of the above-mentioned magnesium titanium phosphate solid electrolyte material is simple to operate, and the particle size of the nano-scale magnesium source, nano-scale titanium source and nano-scale phosphorus source is small, which increases the specific surface area of the raw material powder, helps to improve the reaction activity, and thus improves the reaction efficiency; the flux makes the reaction between the raw materials of the present invention a liquid phase reaction, replacing the traditional solid phase reaction, greatly improving the sintering efficiency; further, it has been verified by experiments that the magnesium titanium phosphate solid electrolyte material obtained by the above-mentioned preparation method has a high purity.
[0059] The magnesium titanium phosphate solid electrolyte material of one embodiment is prepared by any of the above-mentioned methods for preparing the magnesium titanium phosphate solid electrolyte material.
[0060] It has been verified through experiments that the magnesium titanium phosphate solid electrolyte material obtained by the above preparation method has a high purity.
[0061] A magnesium ion battery according to one embodiment comprises the above-mentioned magnesium titanium phosphate solid electrolyte material. The magnesium titanium phosphate solid electrolyte material according to the technical solution of the present invention can be used in aspects such as electrode coating slurry, battery pole pieces and electrolyte of magnesium ion batteries.
[0062] Compared with the conventional magnesium ion battery using magnesium titanium phosphate solid electrolyte material containing impurities, the magnesium ion battery of the technical solution of the present invention has better performance due to the higher purity of the magnesium titanium phosphate solid electrolyte material.
[0063] With reference to the above implementation contents, in order to make the technical solution of the present application more specific, clear and easy to understand, the technical solution of the present application is now exemplified. However, it should be noted that the contents to be protected by the present application are not limited to the following embodiments.
[0064] Example 1
[0065] The raw materials were provided with a particle size distribution as shown in Table 1.
[0066] Table 1 Particle size distribution of each raw material
[0067] raw material D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Magnesium Oxide 1.170 2.730 6.267 13.412 Titanium oxide 0.254 0.589 1.494 10.196
[0068] 1 kg of magnesium oxide and 1 kg of titanium oxide are respectively subjected to air flow milling to obtain nano-magnesium oxide and nano-titanium oxide with particle sizes of 100 nm to 1000 nm and 100 nm to 1000 nm respectively.
[0069] 105.6 g of nano-magnesium oxide, 812 g of nano-titanium oxide and 80 g of lithium carbonate were added into a mixer and stirred electrically for 1 hour. Then 1090 g of phosphorus pentoxide was added and mixed for 10 minutes and then poured out to obtain a mixed material.
[0070] The mixed material is placed in a high-temperature box furnace, the sintering temperature is adjusted to 1000° C., the sintering time is 10 h, and a magnesium titanium phosphate sintered block is obtained by high-temperature calcination.
[0071] The magnesium titanium phosphate powder is placed in a jaw crusher for crushing to obtain magnesium titanium phosphate particles with a particle size of 0.1 cm to 1 cm.
[0072] Titanium phosphate magnesium powder with a particle size of 0.1 cm to 1 cm is placed in a ball mill for ball milling. The speed of the ball mill is 300 rpm. The ball milling time is 5 hours to obtain titanium phosphate magnesium powder with a particle size of 5 μm to 50 μm.
[0073] The titanium magnesium phosphate powder with a particle size of 5 μm to 50 μm was subjected to a jet mill to obtain a crushed titanium magnesium phosphate with a particle size of 300 nm to 900 nm, namely the material of Example 1, and its particle size distribution is shown in Table 2.
[0074] Table 2 Particle size distribution of nano-magnesium titanium phosphate powder
[0075] substance D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Magnesium Titanium Phosphate 0.392 0.479 0.712 0.896
[0076] The material obtained in Example 1 was subjected to X-ray diffraction to obtain Figure 2 .Depend on Figure 2 It can be seen that the diffraction peaks of the substance prepared in Example 1 all correspond to the standard card PDF#82-0297 one by one, and no impurity peaks appear, indicating that the synthesized substance is high-purity magnesium titanium phosphate.
[0077] Example 2
[0078] Provide the raw materials with particle size distribution as shown in Table 3.
[0079] Table 3 Particle size distribution of each raw material
[0080] raw material D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Magnesium Oxide 1.170 2.730 6.267 13.412 Titanium oxide 0.254 0.589 1.494 10.196
[0081] 1 kg of magnesium oxide and 1 kg of titanium oxide are respectively subjected to air flow milling to obtain nano-magnesium oxide and nano-titanium oxide with particle sizes of 100 nm to 1000 nm and 100 nm to 1000 nm respectively.
[0082] 105.6 g of nano-magnesium oxide, 812 g of nano-titanium oxide and 80 g of lithium fluoride were added into a mixer and stirred electrically for 1 hour. Then 1090 g of phosphorus pentoxide was added and mixed for 10 minutes and then poured out to obtain a mixed material.
[0083] The mixed material is placed in a high-temperature box furnace, the sintering temperature is adjusted to 1000° C., the sintering time is 10 h, and a magnesium titanium phosphate sintered block is obtained by high-temperature calcination.
[0084] The magnesium titanium phosphate powder is placed in a jaw crusher for crushing to obtain magnesium titanium phosphate particles with a particle size of 0.1 cm to 1 cm.
[0085] Titanium phosphate magnesium powder with a particle size of 0.1cm to 1cmxx is placed in a ball mill for ball milling. The speed of the ball mill is 300rmp. The ball milling time is 5h to obtain titanium phosphate magnesium powder with a particle size of 5-50umxx.
[0086] The titanium magnesium phosphate powder with a particle size of 5 μm to 50 μm was subjected to a jet mill to obtain a crushed titanium magnesium phosphate with a particle size of 300 nm to 900 nm, namely the material of Example 2, and its particle size distribution is shown in Table 4.
[0087] Table 4 Particle size distribution of nano-magnesium titanium phosphate powder
[0088] substance D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Magnesium Titanium Phosphate 0.354 0.491 0.753 0.874
[0089] The material obtained in Example 2 was subjected to X-ray diffraction to obtain Figure 3 .Depend on Figure 3 It can be seen that the diffraction peaks of the substance prepared in Example 2 all correspond to the standard card PDF#82-0297 one by one, and no impurity peaks appear, indicating that the synthesized substance is high-purity magnesium titanium phosphate.
[0090] Example 3
[0091] Provide the raw materials with particle size distribution as shown in Table 5.
[0092] Table 5 Particle size distribution of each raw material
[0093] raw material D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Magnesium Oxide 1.170 2.730 6.267 13.412 Titanium oxide 0.254 0.589 1.494 10.196
[0094] 1 kg of magnesium oxide and 1 kg of titanium oxide are respectively passed through air flow mills to obtain nano-magnesium oxide and nano-titanium oxide with particle sizes of 100 nm to 1000 nm and 100 nm to 1000 nm, respectively.
[0095] 105.6 g of nano-magnesium oxide, 812 g of nano-titanium oxide and 80 g of sodium carbonate were added into a mixer and stirred electrically for 1 hour. Then 1090 g of phosphorus pentoxide was added and mixed for 10 minutes and then poured out to obtain a mixed material.
[0096] The mixed material is placed in a high-temperature box furnace, the sintering temperature is adjusted to 1000° C., the sintering time is 10 h, and a magnesium titanium phosphate sintered block is obtained by high-temperature calcination.
[0097] The magnesium titanium phosphate powder is placed in a jaw crusher for crushing to obtain magnesium titanium phosphate particles with a particle size of 0.1 cm to 1 cm.
[0098] Titanium phosphate magnesium powder with a particle size of 0.1 cm to 1 cm is placed in a ball mill for ball milling. The speed of the ball mill is 300 rpm. The ball milling time is 5 hours to obtain titanium phosphate magnesium powder with a particle size of 5 μm to 50 μm.
[0099] The titanium magnesium phosphate powder with a particle size of 5 μm-50 μm was jet milled to obtain a crushed titanium magnesium phosphate with a particle size of 300 nm to 900 nm, namely the material of Example 3, and its particle size distribution is shown in Table 6.
[0100] Table 6 Particle size distribution of nano-magnesium titanium phosphate powder
[0101] substance D10(micrometer) D50(micrometer) D90(micrometer) D100(micrometer) Magnesium Titanium Phosphate 0.310 0.483 0.766 0.882
[0102] The material obtained in Example 3 was subjected to X-ray diffraction to obtain Figure 4 .Depend on Figure 4 It can be seen that the diffraction peaks of the substance prepared in Example 3 all correspond to the standard card PDF#82-0297 one by one, and no impurity peaks appear, indicating that the synthesized substance is high-purity magnesium titanium phosphate.
[0103] Comparative Example 1
[0104] This comparative example is a comparative example of Example 1, and provides a magnesium titanium phosphate solid electrolyte material and a preparation method thereof. The preparation method is substantially the same as that of Example 1, and the only difference from the preparation method of Example 1 is that the raw materials used are not subjected to airflow mill nano-processing.
[0105] The material obtained in Comparative Example 1 was subjected to X-ray diffraction to obtain Figure 5 .Depend on Figure 5It can be seen that the diffraction peaks of the substance prepared in Comparative Example 1 are significantly different from those of the standard card PDF#82-0297, and there are obvious impurity peaks on both sides of the main peak, indicating that the synthesized substance has other impurities in addition to magnesium titanium phosphate.
[0106] Comparative Example 2
[0107] This comparative example is a comparative example of Example 2, and provides a magnesium titanium phosphate solid electrolyte material and a preparation method thereof. The preparation method is substantially the same as that of Example 1, and the only difference from the preparation method of Example 2 is that no flux is added and the sintering time is 20 hours.
[0108] The material obtained in Comparative Example 2 was subjected to X-ray diffraction to obtain Figure 6 .Depend on Figure 6 It can be seen that the diffraction peaks of the substance prepared in Comparative Example 2 are significantly different from those of the standard card PDF#82-0297, and there are obvious impurity peaks on both sides of the main peak, indicating that the synthesized substance contains other impurities in addition to magnesium titanium phosphate.
[0109] From the above, it can be seen that compared with the magnesium titanium phosphate solid electrolyte materials of Comparative Examples 1 and 2, the reaction efficiency and purity of the magnesium titanium phosphate solid electrolyte materials of Examples 1 to 3 of the present invention are higher, indicating that the preparation method of the magnesium titanium phosphate solid electrolyte material of the present invention can improve the reaction efficiency and the purity of the magnesium titanium phosphate solid electrolyte material.
[0110] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0111] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a magnesium titanium phosphate solid electrolyte material, It is characterized in that The steps include: Providing nano-scale magnesium source, nano-scale titanium source and nano-scale phosphorus source; Evenly mixing the nano-scale magnesium source, the nano-scale titanium source, the nano-scale phosphorus source and a flux to obtain a mixed material; The mixed material is subjected to solid phase sintering treatment to obtain titanium magnesium phosphate powder; as well as The magnesium titanium phosphate powder is pulverized to obtain the pulverized magnesium titanium phosphate, which is the magnesium titanium phosphate solid electrolyte material.
2. The method for preparing the magnesium titanium phosphate solid electrolyte material according to claim 1, It is characterized in that The nano-scale magnesium source, the nano-scale titanium source and the nano-scale phosphorus source are obtained by respectively treating the magnesium source, the titanium source and the phosphorus source by air flow milling.
3. The method for preparing the magnesium titanium phosphate solid electrolyte material according to claim 1, It is characterized in that The molar ratio of the magnesium element in the nanoscale magnesium source, the titanium element in the nanoscale titanium source and the phosphorus element in the nanoscale phosphorus source is (1.02-1.05):4:
6.
4. The method for preparing the magnesium titanium phosphate solid electrolyte material according to claim 1, It is characterized in that The nano-scale magnesium source is selected from at least one of magnesium oxide, magnesium hydroxide and magnesium carbonate; The nano-scale titanium source is titanium dioxide; The nanoscale phosphorus source is selected from at least one of phosphorus pentoxide, ammonium dihydrogen phosphate and diammonium hydrogen phosphate.
5. The method for preparing the magnesium titanium phosphate solid electrolyte material according to claim 1, It is characterized in that The flux is selected from at least one of lithium carbonate, lithium fluoride, sodium carbonate and potassium carbonate.
6. The method for preparing the magnesium titanium phosphate solid electrolyte material according to claim 1, It is characterized in that The weight of the flux accounts for 3wt% to 10wt% of the total weight of the nanoscale magnesium source, the nanoscale titanium source and the nanoscale phosphorus source.
7. The method for preparing the magnesium titanium phosphate solid electrolyte material according to claim 1, It is characterized in that The temperature of solid phase sintering is 900°C to 1500°C, and the time of solid phase sintering is 2h to 20h.
8. The method for preparing the magnesium titanium phosphate solid electrolyte material according to claim 1, It is characterized in that The magnesium titanium phosphate powder is crushed to obtain the crushed magnesium titanium phosphate by: The magnesium titanium phosphate powder is placed in a jaw crusher for crushing to obtain magnesium titanium phosphate particles with a particle size of 0.1 cm to 1 cm; The titanium magnesium phosphate powder with a particle size of 0.1 cm to 1 cm is placed in a ball mill for ball milling, the speed of the ball mill is 100 rpm to 400 rpm, and the ball milling time is 1 h to 10 h to obtain a titanium magnesium phosphate powder with a particle size of 5 μm to 50 μm; and The magnesium titanium phosphate powder with a particle size of 5 μm to 50 μm is subjected to a jet mill to obtain pulverized magnesium titanium phosphate with a particle size of 0.3 μm to 0.9 μm.
9. A magnesium titanium phosphate solid electrolyte material, It is characterized in that The magnesium titanium phosphate solid electrolyte material is prepared by the preparation method of any one of claims 1 to 8.
10. A magnesium ion battery, It is characterized in that It includes the magnesium titanium phosphate solid electrolyte material as described in claim 9.