Method for eliminating flocculent carbon in lithium iron phosphate material
By introducing carbon dioxide gas into the high-temperature sintering step of lithium iron phosphate material, the reaction between floc carbon and carbon dioxide is used to solve the problem of removing floc carbon in lithium iron phosphate material, and the safety and electrochemical properties of the material are improved. A green and low-cost removal process is achieved.
Patent Information
- Application Number
- CN202410942942.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The prior art is difficult to effectively eliminate flocculent carbon in lithium iron phosphate materials, affecting the conductivity and safety performance of the material, and conventional methods may lose carbon content or affect electrical performance.
In the cooling stage of the high-temperature sintering step of lithium iron phosphate material, an appropriate amount of carbon dioxide gas is introduced, and the specific reaction between carbon dioxide gas and floc carbon is used to selectively eliminate floc carbon with high reactivity, and control the concentration and circulation of carbon dioxide gas. Input time to avoid affecting the graphitized carbon coating.
Effectively reduce flocculent carbon in lithium iron phosphate materials, improve safety performance and electrochemical properties, and do not affect the carbon coating of the material, achieving a green, low-cost and controllable removal process.
Smart Images

Figure CN118894512A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium iron phosphate preparation, and more specifically, to a method for eliminating flocculent carbon in lithium iron phosphate materials. Background Art
[0002] During the production process of lithium iron phosphate materials, due to their poor electrical conductivity, it is necessary to add an organic carbon source and sinter it with the precursor to carbon-coat the surface of the material, improve the overall electrical conductivity of the material, and increase the charge and discharge capacity. However, the organic carbon source decomposes a large amount of gas during the thermal decomposition process to form carbon bubbles, which then produce free carbon outside the near-surface of the lithium iron phosphate particles. These free carbons adhere to the surface of the lithium iron phosphate material to form flocs called flocculent carbon. These flocculent carbons have poor electrical and thermal conductivity and cannot improve the electrical conductivity of the lithium iron phosphate material. They also affect the overall safety performance of the lithium iron phosphate material and increase the risk of spontaneous combustion after forming a battery. Therefore, in order to solve this problem, researchers have used some methods to eliminate the flocculent carbon.
[0003] For example, Chinese patent CN112768688A discloses a lithium iron phosphate material, a preparation method thereof and a lithium ion battery, wherein reaction raw materials containing lithium, iron and phosphorus, a carbon source and a binder are dispersed and mixed in a solvent to obtain a mixture; the mixture is then granulated to obtain a precursor; the precursor is pre-fired in an oxidizing atmosphere to obtain a pre-fired product, and the pre-fired product is sintered in a protective atmosphere to obtain the lithium iron phosphate material; wherein before sintering, the binder is removed by pre-fired in an oxidizing atmosphere, thereby avoiding the generation of flocculent carbon residues after the binder is decomposed during high-temperature sintering in a protective atmosphere, promoting the crystal growth of primary particles inside secondary particles, and improving the cyclic stability of the material; the invention removes the flocculent carbon by oxidative decomposition, and the essence of the removal is the binder rather than the carbon source, the oxidizing atmosphere is air, and the flocculent carbon generated by the carbon source is not accurately removed.
[0004] For another example, Japanese patent CN1893154A discloses a silicon composite material, a manufacturing method and a negative electrode material for a non-aqueous electrolyte battery, which is prepared by heating the powder at a temperature of 600°C to 1400°C in an oxidizing atmosphere to remove the excess free carbon layer on the surface by oxidative decomposition, so that the free carbon content reaches 5% by weight; this invention also removes the surface free carbon by oxidative decomposition of carbon in the air, and its material is silicon carbide, not lithium iron phosphate material. The carbon bonding methods of the two are different, so they cannot be simply combined and applied to lithium iron phosphate.
[0005] In addition, in common knowledge, we know that carbon and carbon dioxide gas can react to generate carbon monoxide, and this principle can be used to remove flocculent carbon. For example, patent CN104925864A also discloses that after the carbonization process of the reaction is completed, carbon dioxide gas is continuously introduced and kept warm for 0.5 to 2 hours to remove excess free carbon, but the amount of carbon dioxide gas introduced is not explored, and the non-free carbon in the invention is connected by chemical bonds, while the free carbon only exists on the surface of the material by physical adsorption force. The reaction difficulty of the two is different. Therefore, since the carbon in the lithium iron phosphate material is combined with the material by physical adsorption force, this method cannot be simply applied to the lithium iron phosphate material, and it is easy to lose carbon content, affecting the conductive properties of the lithium iron phosphate.
[0006] Existing technologies also reduce the flocculent carbon in the material by adjusting parameters such as the type and amount of carbon source, sintering temperature and time, but these cannot effectively eliminate the flocculent carbon in the material and may affect the carbon coating on the surface of the lithium iron phosphate crystal, resulting in a decrease in electrical performance. Therefore, how to effectively and accurately eliminate the flocculent carbon in the material without affecting the established conditions of the material sintering process and without generating new polluting waste is an important challenge facing current technology. Summary of the invention
[0007] In view of the above, the present invention provides a method for eliminating flocculent carbon in lithium iron phosphate materials. By utilizing the specific reaction of carbon dioxide gas and carbon element, an appropriate amount of carbon dioxide gas is introduced into the cooling stage in the high-temperature sintering step of the process for preparing lithium iron phosphate materials, and the flocculent carbon with greater reaction activity in the lithium iron phosphate material is selectively eliminated, thereby effectively reducing the flocculent carbon in the lithium iron phosphate material without affecting the carbon coating on the surface of the lithium iron phosphate crystals, thereby ensuring the safety performance and electrochemical performance of the material.
[0008] The present invention provides a method for eliminating flocculent carbon in lithium iron phosphate material, comprising grinding, spray drying and high-temperature sintering raw materials in sequence to obtain lithium iron phosphate positive electrode material, wherein carbon dioxide gas with a concentration of 1000 to 5000 ppm is introduced in the cooling stage of high-temperature sintering for 4 to 6 hours, the initial temperature of the cooling stage is 500°C, and the end temperature is 200°C.
[0009] The carbon in lithium iron phosphate positive electrode materials can be roughly divided into two categories: One type is graphitized carbon, which is formed by carbon atoms into a uniform and stable carbon hexagonal structure and extends into a lamellar structure. Due to the sp2 hybridization of carbon atoms, there is an unpaired electron in the outer layer. The unpaired electrons on the same layer of carbon atoms can migrate freely on the graphite layer structure due to the conjugation effect, making the graphite have good conductivity. Therefore, the graphitized carbon coated on the surface of lithium iron phosphate particles is a key substance to improve the electronic conductivity of lithium iron phosphate and exert the material's capacitance. It is composed of stable and uniform crystals, has relatively stable chemical properties, and is not easily oxidized. The other type is amorphous carbon, also known as flocculent carbon, in which the connections between carbon atoms are disordered and irregular, with both sp2 hybridization and sp3 hybridization, and cannot form a regular crystal structure. Its microscopic morphology shows a flocculent distribution. Flocculent carbon accounts for a small proportion of the surface of lithium iron phosphate particles, but its conductivity is poor, its reaction activity is high, and it is prone to redox reactions. It is an important component of the risk of thermal runaway of battery materials.
[0010] Therefore, in view of the above, the present invention utilizes the difference in the reactivity of graphitized carbon and flocculent carbon to specifically eliminate flocculent carbon in the coexistence system of graphitized carbon and flocculent carbon on the surface of lithium iron phosphate material in a low concentration CO2 atmosphere.
[0011] Although the chemical properties of graphitized carbon are stable, it is not connected to lithium iron phosphate by chemical bonds and is essentially a type of carbon single substance. In a high-temperature, high-concentration CO2 atmosphere, it will react to generate CO, which will be consumed. The loss of graphitized carbon will lead to a decrease in the electronic conductivity of the lithium iron phosphate material, hindering its capacity. Therefore, the present invention strictly controls the concentration and time of carbon dioxide gas introduction during the cooling stage, thereby avoiding the reaction of carbon dioxide gas with the graphitized carbon coated on the surface of the lithium iron phosphate material and damaging the coated carbon layer on the surface of the material, thereby achieving the purpose of eliminating flocculent carbon without affecting the performance of the material.
[0012] The raw materials include glucose, and the mass ratio of glucose to carbon dioxide gas is about 1:0.092. Glucose is the carbon source raw material for preparing lithium iron phosphate materials, and flocculent carbon is produced from it. Under the same process conditions, the more glucose is added, the more flocculent carbon the material finally contains, and the amount of flocculent carbon determines the amount of carbon dioxide gas added. Therefore, the mass ratio of glucose to carbon dioxide gas is strictly controlled, and the concentration, temperature and time of the carbon dioxide gas are combined to achieve the purpose of better eliminating flocculent carbon. The carbon of the carbon coating layer of the lithium iron phosphate material will not be lost due to excessive addition of carbon dioxide gas, thereby avoiding the impact on the performance of the lithium iron phosphate material.
[0013] During the cooling stage of high-temperature sintering, carbon dioxide gas with a concentration of 3000 ppm is introduced.
[0014] The beneficial effects of the present invention are: (1) The present invention introduces carbon dioxide gas during the cooling stage of the high-temperature sintering step in the process of preparing lithium iron phosphate materials, which neither affects the established conditions of the material production process, such as the type and amount of carbon source, sintering temperature, and sintering time, nor generates new waste gas pollution, and has no risk of damaging the sintering equipment. Moreover, the treatment is completed during the material cooling process, without additional time-consuming treatment, thereby achieving efficient, green, controllable, and low-cost removal of flocculent carbon; (2) The present invention strictly controls the concentration of carbon dioxide gas and the mass ratio of glucose to carbon dioxide gas, which not only effectively reduces the flocculent carbon in the lithium iron phosphate material, but also avoids the problem of excessive addition of carbon dioxide gas, high concentration of carbon dioxide gas, too long introduction time, or too high reaction temperature causing it to react with the graphitized carbon coated on the surface of the material, thereby damaging the carbon coated on the surface of the material, thereby achieving the purpose of eliminating flocculent carbon without seriously affecting the electrochemical properties of the material, and the introduction of carbon dioxide gas at an appropriate concentration can also improve its electrochemical properties to a certain extent; (3) The present invention utilizes the reaction between flocculent carbon and carbon dioxide gas to specifically eliminate flocculent carbon on the surface of the material, thereby reducing the risk of thermal runaway of the battery and improving its safety performance in use. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a SEM image of the lithium iron phosphate material of Example 1.
[0016] Figure 2 This is a SEM image of the lithium iron phosphate material of Example 2.
[0017] Figure 3 This is a SEM image of the lithium iron phosphate material of Example 3.
[0018] Figure 4 This is a SEM image of the lithium iron phosphate material of Example 4.
[0019] Figure 5 This is a SEM image of the lithium iron phosphate material of Example 5.
[0020] Figure 6 This is a SEM image of the lithium iron phosphate material of Example 6.
[0021] Figure 7 This is a SEM image of the lithium iron phosphate material of Example 7. DETAILED DESCRIPTION
[0022] The embodiments of the present application will be described in more detail below. The application can be implemented in various forms, and should not be construed as being limited to the embodiments set forth herein, but rather these embodiments are provided to provide a more thorough and complete understanding of the present application. It should be understood that the embodiments of the present application are only for exemplary purposes and are not intended to limit the scope of protection of the present application.
[0023] The embodiments of the present invention are implemented with the following technical solutions: (1) preparing raw materials: mixing iron phosphate, lithium carbonate, glucose, and pure water in a mass ratio of 8:2:1:7 to obtain a mixture; (2) Grinding and drying: the mixed material is put into a grinding tank, and after grinding, it is spray-dried to obtain a dry material; (3) High temperature sintering: The dried material is fed into a box furnace and sintered in a 100% N2 atmosphere. The constant temperature zone of the sintering is set at 800°C and the sintering time is 23h. (4) Eliminating flocculent carbon: After the sintering is completed at the constant temperature stage, when the sintered material enters the cooling stage at 500°C, carbon dioxide gas with a concentration of 1000-5000 ppm is introduced to make the atmosphere a mixed gas of carbon dioxide gas and nitrogen. The introduction time is 4-6 hours until the temperature drops to 200°C to obtain lithium iron phosphate material, in which the mass ratio of glucose to carbon dioxide gas is 1:0.092.
[0024] Table 1 shows the specific implementation conditions and electrochemical performance test results of the embodiments of the present invention. Figures 1 to 7 3 is a SEM image of the lithium iron phosphate material prepared in the embodiment of the present invention. The filamentous substance in the SEM image is flocculent carbon.
[0025] Figure 1 This is a lithium iron phosphate material without the introduction of carbon dioxide gas. It can be seen that there are a lot of flocculent carbon on its surface. Figures 2 to 7 It is the lithium iron phosphate material after the treatment of carbon dioxide gas. It can be seen that with the increase of the amount of carbon dioxide gas introduced, the flocculent carbon on its surface is further reduced, which proves that carbon dioxide gas can effectively eliminate flocculent carbon. However, the higher the concentration of carbon dioxide gas, the better. The higher the concentration of carbon dioxide gas, the more carbon loss will occur in the carbon coating layer of the lithium iron phosphate material, thus affecting the electrochemical properties of the material.
[0026] It can be seen from Table 1 that the concentration of carbon dioxide gas affects the electrochemical properties of lithium iron phosphate materials. As the concentration of carbon dioxide gas increases, the electrochemical properties show a trend of first increasing and then decreasing. In Example 3, the carbon dioxide gas concentration is 3000ppm, the introduction time is 5h, and the prepared lithium iron phosphate has the best electrochemical performance. Compared with the lithium iron phosphate material in Example 1 in which carbon dioxide gas is not introduced to eliminate flocculent carbon, its electrochemical performance is improved; in Examples 6 and 7, the carbon dioxide gas concentration is 3000ppm, the introduction time is 4h and 6h, and the prepared Compared with the material in Example 3, the electrochemical performance of the lithium iron phosphate prepared by the present invention is reduced, but the difference is not large; the concentration of carbon dioxide gas in Example 4 is 5000ppm, and the introduction time is 5h, and the electrochemical performance of the lithium iron phosphate prepared is significantly reduced. When the concentration is further increased, the electrochemical performance of the lithium iron phosphate prepared is further reduced, indicating that the concentration of carbon dioxide gas has a certain influence on the electrochemical performance of the prepared lithium iron phosphate, but it will not have a significant impact on the electrochemical performance of the lithium iron phosphate within the carbon dioxide concentration range of the present invention; therefore, in combination with the attached Figures 1 to 7 The experiments shown in Table 1 show that the introduction of a certain amount of carbon dioxide gas during the cooling stage of the high-temperature sintering step in the preparation of lithium iron phosphate can effectively eliminate the flocculent carbon on the surface of the lithium iron phosphate, and the concentration of the introduced carbon dioxide gas can be controlled, which can effectively eliminate the flocculent carbon on the surface of the lithium iron phosphate without seriously affecting the electrochemical properties of the lithium iron phosphate material, thereby ensuring the safety and electrochemical properties of the lithium iron phosphate material during use. At the same time, the introduction time is controlled to avoid too short a time, which cannot fully react, and too long a time, which not only results in high energy consumption and uneven reaction, but also may react with graphitized carbon to reduce the electrochemical properties of the material. In addition, the introduction of carbon dioxide gas of appropriate concentration and time can also improve the electrochemical properties of the material to a certain extent.
[0027] Table 1 Specific implementation conditions of the embodiment and electrochemical performance test of the prepared lithium iron phosphate.
[0028] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in this application, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for eliminating flocculent carbon in lithium iron phosphate material, comprising grinding, spray drying and high-temperature sintering the raw materials in sequence to obtain a lithium iron phosphate positive electrode material, characterized in that: During the cooling stage of the high-temperature sintering, carbon dioxide gas with a concentration of 1000-5000 ppm is introduced for 4-6 hours. The initial temperature of the cooling stage is 500°C and the end temperature is 200°C.
2. The method for eliminating flocculent carbon in lithium iron phosphate material according to claim 1, characterized in that: The raw materials include iron phosphate, lithium carbonate and glucose, wherein the mass ratio of glucose to carbon dioxide gas is 1:0.
092.
3. The method for eliminating flocculent carbon in lithium iron phosphate material according to claim 1, characterized in that: During the cooling stage of high-temperature sintering, carbon dioxide gas with a concentration of 3000 ppm is introduced.
Citation Information
Patent Citations
Preparation method for nano chromium carbide powder
CN104925864A
Lithium iron phosphate material, preparation method thereof and lithium ion battery
CN112768688A
Silicon composite, making method, and non-aqueous electrolyte secondary cell negative electrode material
CN1893154A
Preparation method of high-compactness high-capacity lithium iron phosphate
CN109867268A
Selective oxidation-reduction regeneration method of waste lithium iron phosphate, regenerated lithium iron phosphate and lithium ion battery
CN113036253A