Method for preparing and recycling high-purity copper sulfate from waste copper sulfate electrolyte
By using copper oxide powder and hydrogen peroxide in waste copper sulfate electrolyte for redox reaction, combined with heating, pH adjustment and multiple filtration, the problems of low copper recovery and secondary pollution are solved, and efficient Copper recycling and waste disposal reduce environmental and health risks.
Patent Information
- Application Number
- CN202411165560.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art copper recovery rate in waste copper sulfate electrolyte treatment is low and is prone to secondary pollution, leading to environmental and human health risks.
By adding copper oxide powder and hydrogen peroxide to the waste electrolyte for redox reaction, the copper ions are reduced to copper element, and the copper ions are precipitated by heating and pH adjustment, combined with multiple filtration and centrifugation, and finally dried by vacuum and cement sealing treatment of arsenic iron slag.
It significantly improves the copper recovery rate and processing efficiency, reduces environmental and health risks, and ensures high purity and stability of the product.
Smart Images

Figure CN118894548A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste treatment, in particular to a method for preparing high-purity copper sulfate from waste copper sulfate electrolyte for reuse. Background Art
[0002] Waste copper sulfate electrolyte refers to the waste liquid containing copper and sulfuric acid produced during the copper electrolytic refining process. In the copper electrolytic refining process, crude copper is used as the anode, pure copper sheets are used as the cathode, and a mixed solution of sulfuric acid and copper sulfate is used as the electrolyte. When power is turned on, copper dissolves from the anode into copper ions and moves to the cathode, where it obtains electrons and precipitates as pure copper. In this process, some metals that are more active than copper, such as iron and zinc, will also dissolve, but since their ions are not easy to precipitate on the cathode, their reactions can be controlled by adjusting the potential difference. Inactive impurities such as gold and silver are deposited at the bottom of the electrolytic cell. As the electrolytic process proceeds, the concentration of copper ions in the electrolyte continues to rise, the concentration of sulfuric acid gradually decreases, and impurities continue to accumulate. In order to maintain the stability of the components in the electrolyte, it is necessary to regularly extract part of the waste electrolyte and replenish water and sulfuric acid. The extracted waste electrolyte usually contains high concentrations of copper and sulfuric acid, as well as various impurities, including iron, arsenic, etc. If this waste electrolyte is directly discharged without treatment, it will not only waste resources, but also cause serious pollution to the environment.
[0003] In the existing treatment process of waste copper sulfate electrolyte, due to improper operating conditions or technical limitations, the copper recovery rate may be lower than expected. At the same time, during the treatment process, some by-products will produce secondary pollution and cause new pollution to the environment. Summary of the invention
[0004] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a method for preparing high-purity copper sulfate for reuse from waste copper sulfate electrolyte, which has the advantages of firstly oxidizing copper ions in the waste electrolyte to reduce the copper ions to single copper, using hydrogen peroxide to improve the reaction efficiency, thereby significantly improving the recovery rate of copper, then heating and precipitating the copper ions in the form of copper hydroxide or copper salt to improve the recovery rate of copper, and finally treating the arsenic iron slag to not only improve the efficiency of waste treatment, but also effectively reduce the risks to the environment and human health, etc., thereby solving the problems of low copper recovery rate and easy secondary pollution in the treatment process.
[0005] (II) Technical solution To achieve the above object, the present invention provides a technical solution: a method for preparing high-purity copper sulfate for reuse from waste copper sulfate electrolyte, comprising the following steps: Step 1, filtration: using a filter to remove solid impurities in the electrolyte to obtain spent electrolyte; Step 2: Mixing: adding copper oxide powder and hydrogen peroxide to the waste electrolyte and stirring to form a solution; Step 3, heating: heating the solution in step 2; Step 4, adjusting the pH value: adding sodium hydroxide or sodium carbonate aqueous solution to the heated solution to adjust the pH value and then letting it stand; Step 5, secondary filtration: secondary filtration of the solution after adjusting the pH value to separate the arsenic iron slag and the copper sulfate purified liquid; Step 6: Centrifugal separation: Place the copper sulfate purified liquid into a centrifuge to separate the copper sulfate from the liquid by centrifugal force; Step 7, three-time filtration: filter the liquid three times through a 0.2 micron filter membrane device to extract fine particles of copper sulfate in the liquid; Step 8, washing: washing the fine particles of copper sulfate extracted in step 7 and the copper sulfate in step 6; Step 9, drying: Place the washed copper sulfate in a vacuum dryer for drying.
[0006] Preferably, the filter in step 1 uses a 5 μm ceramic filter membrane to remove solid impurities in the electrolyte to obtain the spent electrolyte.
[0007] Preferably, in the step 2, the mass ratio of copper oxide powder to waste electrolyte is 1:10-1:20, and the volume ratio of hydrogen peroxide to waste electrolyte is 1:10-1:20, wherein the concentration of hydrogen peroxide is usually 50%, and the waste electrolyte, copper oxide powder, and hydrogen peroxide with the mass ratio and volume ratio are placed in a mechanical stirrer at 200-400 rpm and stirred for 1 hour to obtain a solution.
[0008] Preferably, in step three, the mechanical stirrer is heated at a temperature of 60°C-70°C for 45 minutes to ensure complete reaction.
[0009] Preferably, the specific operation method of step 4 is: S1.1, prepare in advance 0.1M or 1M sodium hydroxide aqueous solution and sodium carbonate aqueous solution; S1.2. Use a pH meter or pH test paper to measure the current pH value of the heated solution; S1.3. According to the tested pH value, add sodium hydroxide aqueous solution or sodium carbonate aqueous solution into the solution one by one, stir it with a mechanical stirrer for 5 minutes, and then test the pH value of the solution again until the pH value is adjusted to 3-4.
[0010] Preferably, in step five, a 5 μm ceramic filter membrane is used to perform secondary filtration on the solution after adjusting the pH value to separate the arsenic iron slag and the copper sulfate purified solution.
[0011] Preferably, in step 5, the separated arsenic iron slag is treated as follows: S2.1, put the separated arsenic iron slag into a drying furnace for drying, the drying furnace temperature is 80 ° C-100 ° C, and the drying time is 5h; S2.2, put the dried arsenic iron slag into a grinder at 2000-3000 rpm and grind for 1 hour; S2.3, the ground arsenic iron slag powder is placed in a 50kW magnetic roller magnetic separator, the magnetic roller magnetic separator is set to 80 rpm, and the iron component is separated by the magnetic roller magnetic separator; S2.4, put the remaining arsenic iron slag into an acid corrosion resistant container, pour sulfuric acid in a mass ratio of 1:1 to the arsenic iron slag, and acid-leach the arsenic iron slag for 2 hours, with a sulfuric acid concentration of 1-2 mol / L; S2.5, using a filter press with 40 filter plates with a pore size of 60 microns and a speed of 1000-1500 rpm, a pressure of 0.6-1.0 MPa, to perform a primary filtration on the arsenic-iron slag after acid leaching to separate the arsenic-containing acid solution and the undissolved iron slag; S2.6, storing the undissolved iron slag and the iron components separated from S1.3 for future use; S2.7, put sodium hydroxide in a volume ratio of 1:1 with the arsenic acid solution into a mechanical stirrer at 100-500 rpm, stir for 30 minutes and then let it stand for 2 hours; S2.8, placing the arsenic-containing acid solution after static separation into a 600-1000W vacuum filter with a vacuum pressure of 0.05-0.1MPa, and filtering the acid solution with a 10μm chemical corrosion-resistant filter membrane to separate the liquid and the precipitate; S2.9, mix arsenic precipitate with cement to form a stable solid and reduce its environmental impact; S2.10. Place cement in a weight ratio of 1:2 to arsenic precipitate into a mechanical stirrer at a speed of 100-2000 rpm and stir for 30 minutes to allow the arsenic precipitate and cement to be mixed and then naturally dried to form a stable solid, thereby reducing its environmental impact.
[0012] Preferably, in step six, a centrifuge at 5000-10000 rpm is used at room temperature of 20°C-25°C for 30 min to separate copper sulfate from the liquid.
[0013] Preferably, the specific operation method of step eight is: S3.1. Place deionized water and copper sulfate in a volume ratio of 1:5 into a mechanical stirrer at 500-1000 rpm, stir for 30 min, and then let stand naturally for 2 h. S3.2. Use a 0.45 μm filter membrane and a vacuum filter with a vacuum pressure of 0.1-0.6 MPa to filter the copper sulfate and liquid in S3.1.
[0014] Preferably, in step nine, the temperature of the vacuum dryer is 60°C to 80°C, and the drying time is 4-5h.
[0015] Compared with the prior art, the present invention provides a method for preparing high-purity copper sulfate for reuse from waste copper sulfate electrolyte, which has the following beneficial effects: 1. The present invention adds copper oxide powder and hydrogen peroxide to the waste electrolyte, converts copper ions into precipitable copper compounds through redox reaction, the copper oxide powder acts as an oxidant, reacts with the copper ions in the waste electrolyte, and reduces the copper ions to single copper, and the hydrogen peroxide provides the necessary oxidant for the oxidation reaction, improves the reaction efficiency, and thus significantly improves the recovery rate of copper, and then heats the solution to 60°C-70°C and keeps it for 45 minutes, which can promote the chemical reaction, ensure the completeness of the reaction, optimize the physical properties of the solution, reduce the occurrence of side reactions, and improve the yield of the product and purity, while helping to remove gases and impurities, improve operational stability, and optimize subsequent processing steps. In the pH range of 3-4, copper ions are precipitated in the form of copper hydroxide or copper salts, thereby increasing the copper recovery rate and ensuring the stability of the reaction. At the same time, the precipitate generated by the reaction is more stable and easy to separate from the solution. Adjusting the pH value can allow the reaction product to precipitate in solid form, thereby improving the separation efficiency. By adding sodium hydroxide or sodium carbonate aqueous solution, the pH value of the solution can be adjusted to optimize the particle size and quality of the precipitate, thereby improving the efficiency of filtration and subsequent processing.
[0016] 2. The present invention can effectively separate and remove harmful components such as arsenic by treating arsenic iron slag and convert it into a stable solid form. The drying and crushing steps improve the material processing efficiency. The magnetic separation and acid leaching processes improve the separation and recovery of arsenic. Filtration and sodium hydroxide treatment further remove arsenic and neutralize acidity. The final solidification treatment seals the arsenic precipitate with cement, reducing the impact on the environment. This not only improves the efficiency of waste treatment, but also effectively reduces the risks to the environment and human health. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the process steps of the present invention; DETAILED DESCRIPTION
[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] See also Figure 1 A method for preparing high-purity copper sulfate for reuse from waste copper sulfate electrolyte comprises the following steps: Step 1, filtration: using a 5 μm ceramic filter membrane to remove solid impurities in the electrolyte to obtain spent electrolyte; Step 2, mixing: adding copper oxide powder and hydrogen peroxide to the waste electrolyte, stirring and mixing to form a solution, specifically: the mass ratio of copper oxide powder to waste electrolyte is 1:10-1:20, the volume ratio of hydrogen peroxide to waste electrolyte is 1:10-1:20, wherein the concentration of hydrogen peroxide is generally 50%, and the waste electrolyte, copper oxide powder, and hydrogen peroxide of the mass ratio and volume ratio are placed in a mechanical stirrer at 200-400 rpm, and stirred for 1 hour to obtain a solution; Copper oxide powder and hydrogen peroxide are added to the waste electrolyte, and copper ions are converted into precipitable copper compounds through redox reaction. The copper oxide powder acts as an oxidant to react with the copper ions in the waste electrolyte, so that the copper ions can be reduced to single copper. The hydrogen peroxide provides the necessary oxidant for the oxidation reaction, thereby improving the reaction efficiency, thereby significantly improving the recovery rate of copper. The copper ions in the waste liquid are converted into a form that can be further processed, thereby reducing the loss of copper. Step 3, heating: heating the solution in step 2 at 60°C-70°C for 45 min to ensure complete reaction; Heating the solution to 60°C-70°C and maintaining it for 45 minutes can promote the chemical reaction, ensure the completeness of the reaction, optimize the physical properties of the solution, reduce the occurrence of side reactions, increase the yield and purity of the product, and help remove gases and impurities, improve the stability of the operation, and optimize subsequent processing steps; Step 4: Adjust the pH value: Add sodium hydroxide or sodium carbonate aqueous solution to the heated solution to adjust the pH value and then let it stand. The specific operation method is as follows: S1.1, prepare in advance 0.1M or 1M sodium hydroxide aqueous solution and sodium carbonate aqueous solution; S1.2. Use a pH meter or pH test paper to measure the current pH value of the heated solution; S1.3. According to the tested pH value, add sodium hydroxide aqueous solution or sodium carbonate aqueous solution into the solution one by one, stir it with a mechanical stirrer for 5 minutes, and then test the pH value of the solution again until the pH value is adjusted to 3-4; In the pH range of 3-4, copper ions are precipitated in the form of copper hydroxide or copper salt, thereby improving the recovery rate of copper and ensuring the stability of the reaction. At the same time, the precipitate generated by the reaction is more stable and easy to separate from the solution. Adjusting the pH value can make the reaction product precipitate in solid form, improving the separation efficiency. By adding sodium hydroxide or sodium carbonate aqueous solution, the pH of the solution can be adjusted to optimize the particle size and quality of the precipitate, thereby improving the efficiency of filtration and subsequent treatment; Step 5, secondary filtration: Use a 5μm ceramic filter membrane to perform secondary filtration on the solution after adjusting the pH value to separate the arsenic iron slag and the copper sulfate purification solution. The separated arsenic iron slag is treated as follows: S2.1, put the separated arsenic iron slag into a drying furnace for drying, the drying furnace temperature is 80 ° C-100 ° C, and the drying time is 5h; S2.2, put the dried arsenic iron slag into a grinder at 2000-3000 rpm and grind for 1 hour; S2.3, the ground arsenic iron slag powder is placed in a 50kW magnetic roller magnetic separator, the magnetic roller magnetic separator is set to 80 rpm, and the iron component is separated by the magnetic roller magnetic separator; S2.4, put the remaining arsenic iron slag into an acid corrosion resistant container, pour sulfuric acid in a mass ratio of 1:1 to the arsenic iron slag, and acid-leach the arsenic iron slag for 2 hours, with a sulfuric acid concentration of 1-2 mol / L; S2.5, using a filter press with 40 filter plates with a pore size of 60 microns and a speed of 1000-1500 rpm, a pressure of 0.6-1.0 MPa, to perform a primary filtration on the arsenic-iron slag after acid leaching to separate the arsenic-containing acid solution and the undissolved iron slag; S2.6, storing the undissolved iron slag and the iron components separated from S1.3 for future use; S2.7, put sodium hydroxide in a volume ratio of 1:1 with the arsenic acid solution into a mechanical stirrer at 100-500 rpm, stir for 30 minutes and then let it stand for 2 hours; S2.8, placing the arsenic-containing acid solution after static separation into a 600-1000W vacuum filter with a vacuum pressure of 0.05-0.1MPa, and filtering the acid solution with a 10μm chemical corrosion-resistant filter membrane to separate the liquid and the precipitate; S2.9, mix arsenic precipitate with cement to form a stable solid and reduce its environmental impact; S2.10, placing cement in a weight ratio of 1:2 to arsenic precipitate into a mechanical stirrer at a speed of 100-2000 rpm for 30 min, so that the arsenic precipitate and cement are mixed and naturally dried to form a stable solid, thereby reducing its environmental impact; The use of a 5μm ceramic filter membrane for secondary filtration can effectively remove arsenic iron slag and other solid impurities in the solution, ensure product quality, and reduce possible impurity interference in the subsequent treatment process. At the same time, the treatment of arsenic iron slag can effectively separate and remove harmful components such as arsenic and convert them into a stable solid form. The drying and crushing steps improve the material processing efficiency. The magnetic separation and acid leaching process improves the separation and recovery of arsenic. Filtration and sodium hydroxide treatment further remove arsenic and neutralize acidity. The final solidification treatment seals the arsenic precipitate with cement, reducing the impact on the environment, thereby not only improving the efficiency of waste treatment, but also effectively reducing the risks to the environment and human health. Step 6: Centrifugal separation: Use a centrifuge at 5000-10000 rpm at room temperature of 20°C-25°C for 30 minutes to separate the copper sulfate from the liquid; Step 7, three-time filtration: filter the liquid three times through a 0.2 micron filter membrane device to extract fine particles of copper sulfate in the liquid; Step 8, washing: washing the fine particles of copper sulfate extracted in step 7 and the copper sulfate in step 6. The specific operation method of step 8 is: S3.1. Place deionized water and copper sulfate in a volume ratio of 1:5 into a mechanical stirrer at 500-1000 rpm, stir for 30 min, and then let stand naturally for 2 h. S3.2, filter the copper sulfate and liquid in S3.1 using a 0.45 μm filter membrane and a vacuum filter with a vacuum pressure of 0.1-0.6 MPa; Step 9, drying: put the washed copper sulfate into a vacuum dryer for drying. It is worth noting that the temperature of the vacuum dryer is 60°C to 80°C and the drying time is 4-5h.
[0020] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing high-purity copper sulfate from waste copper sulfate electrolyte for reuse, It is characterized in that The following steps are involved: Step 1, filtration: using a filter to remove solid impurities in the electrolyte to obtain spent electrolyte; Step 2: Mixing: adding copper oxide powder and hydrogen peroxide to the waste electrolyte and stirring to form a solution; Step 3, heating: heating the solution in step 2; Step 4, adjusting the pH value: adding sodium hydroxide or sodium carbonate aqueous solution to the heated solution to adjust the pH value and then letting it stand; Step 5, secondary filtration: secondary filtration of the solution after adjusting the pH value to separate the arsenic iron slag and the copper sulfate purified liquid; Step 6: Centrifugal separation: Place the copper sulfate purified liquid into a centrifuge to separate the copper sulfate from the liquid by centrifugal force; Step 7, three-time filtration: filter the liquid three times through a 0.2 micron filter membrane device to extract fine particles of copper sulfate in the liquid; Step 8, washing: washing the fine particles of copper sulfate extracted in step 7 and the copper sulfate in step 6; Step 9, drying: Place the washed copper sulfate in a vacuum dryer for drying.
2. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: The filter in step 1 uses a 5 μm ceramic filter membrane to remove solid impurities in the electrolyte to obtain waste electrolyte.
3. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: In the step 2, the mass ratio of copper oxide powder to waste electrolyte is 1:10-1:20, and the volume ratio of hydrogen peroxide to waste electrolyte is 1:10-1:20, wherein the concentration of hydrogen peroxide is usually 50%, and the waste electrolyte, copper oxide powder, and hydrogen peroxide with the mass ratio and volume ratio are placed in a mechanical stirrer at 200-400 rpm, and stirred for 1 hour to obtain a solution.
4. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: In the step 3, the mechanical stirrer is heated at a temperature of 60°C-70°C for 45 minutes.
5. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: The specific operation method of step 4 is: S1.1, prepare in advance 0.1M or 1M sodium hydroxide aqueous solution and sodium carbonate aqueous solution; S1.
2. Use a pH meter or pH test paper to measure the current pH value of the heated solution; S1.
3. According to the tested pH value, add sodium hydroxide aqueous solution or sodium carbonate aqueous solution into the solution one by one, stir it with a mechanical stirrer for 5 minutes, and then test the pH value of the solution again until the pH value is adjusted to 3-4.
6. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: In the step 5, the solution after adjusting the pH value is filtered twice using a 5 μm ceramic filter membrane to separate the arsenic iron slag and the copper sulfate purified solution.
7. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: In step 5, the separated arsenic iron slag is treated as follows: S2.1, put the separated arsenic iron slag into a drying furnace for drying, the drying furnace temperature is 80 ° C-100 ° C, and the drying time is 5h; S2.2, put the dried arsenic iron slag into a grinder at 2000-3000 rpm and grind for 1 hour; S2.3, the ground arsenic iron slag powder is placed in a 50kW magnetic roller magnetic separator, the magnetic roller magnetic separator is set to 80 rpm, and the iron component is separated by the magnetic roller magnetic separator; S2.4, put the remaining arsenic iron slag into an acid corrosion resistant container, pour sulfuric acid in a mass ratio of 1:1 to the arsenic iron slag, and acid-leach the arsenic iron slag for 2 hours, with a sulfuric acid concentration of 1-2 mol / L; S2.5, using a filter press with 40 filter plates with a pore size of 60 microns and a speed of 1000-1500 rpm, a pressure of 0.6-1.0 MPa, to perform a primary filtration on the arsenic-iron slag after acid leaching to separate the arsenic-containing acid solution and the undissolved iron slag; S2.6, storing the undissolved iron slag and the iron components separated from S1.3 for future use; S2.7, put sodium hydroxide in a volume ratio of 1:1 with the arsenic acid solution into a mechanical stirrer at 100-500 rpm, stir for 30 minutes and then let it stand for 2 hours; S2.8, placing the arsenic-containing acid solution after static separation into a 600-1000W vacuum filter with a vacuum pressure of 0.05-0.1MPa, and filtering the acid solution with a 10μm chemical corrosion-resistant filter membrane to separate the liquid and the precipitate; S2.9, mix arsenic precipitate with cement to form a stable solid and reduce its environmental impact; S2.
10. Place cement in a weight ratio of 1:2 to arsenic precipitate into a mechanical stirrer at a speed of 100-2000 rpm and stir for 30 minutes to allow the arsenic precipitate and cement to be mixed and then naturally dried to form a stable solid, thereby reducing its environmental impact.
8. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: In the step six, a centrifuge at 5000-10000 rpm is used at a room temperature of 20° C. to 25° C. for 30 min to separate the copper sulfate from the liquid.
9. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: The specific operation method of step eight is: S3.
1. Place deionized water and copper sulfate in a volume ratio of 1:5 into a mechanical stirrer at 500-1000 rpm, stir for 30 min, and then let stand naturally for 2 h. S3.
2. Use a 0.45 μm filter membrane and a vacuum filter with a vacuum pressure of 0.1-0.6 MPa to filter the copper sulfate and liquid in S3.
1.
10. The method for preparing high-purity copper sulfate from waste copper sulfate electrolyte according to claim 1, Features: In the step nine, the temperature of the vacuum dryer is 60°C to 80°C, and the drying time is 4-5h.