Method for preparing high-purity quartz from silicon granules and high-purity quartz

By removing impurities, grinding, oxidizing, and calcining silicon particles, the problems of environmental pollution, high energy consumption, and high cost in the preparation of high-purity quartz have been solved, realizing the industrial production and resource recycling of high-purity quartz.

CN118894638APending Publication Date: 2024-11-05HANGZHOU JINGBAO NEW ENERGY TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411155975.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing technologies for preparing high-purity quartz suffer from problems such as significant environmental pollution, high energy consumption, high cost, low purity, and difficulty in industrial production.

Method used

High-purity quartz is prepared by using silicon particles as raw material and through impurity removal, grinding oxidation and calcination. The process includes steps such as water washing, acid washing, ball milling and high-temperature calcination to remove impurities and convert silicon particles into silicon dioxide, which is then further purified by calcination.

Benefits of technology

This method enables the low-cost and efficient preparation of high-purity quartz, reduces production energy consumption, improves product purity, and promotes industrial production and resource recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894638A_ABST
    Figure CN118894638A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing high-purity quartz by using silicon granules, which comprises the following steps: removing impurities from initial silicon granules to obtain intermediate silicon granules; mixing, grinding and stirring the intermediate silicon granules and an oxidizing agent to obtain initial silicon dioxide powder; and carrying out impurity removal treatment on the initial silicon dioxide powder, and calcining to obtain the high-purity quartz. The invention also discloses the high-purity quartz. According to the method, the industrial cut silicon waste can be recycled, the raw material cost is greatly reduced, the value of the industrial waste is exerted, the cyclic utilization of resources is promoted, meanwhile, the preparation process of the high-purity quartz is simple and efficient, and the production cost is also greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of high-purity quartz, in particular to high-purity quartz and a method for preparing the high-purity quartz by using silicon granules. Background Art

[0002] High-purity quartz generally refers to quartz materials with SiO2 content higher than 99.99%, and is the main raw material for quartz tubes, quartz crucibles, quartz utensils, etc. At present, my country's photovoltaic quartz crucible inner quartz sand mainly relies on imports of high-purity quartz from the United States because the domestic quartz purity cannot meet its purity requirements.

[0003] Artificial synthesis of high-purity quartz is not limited by natural resources and has become a hot topic in recent years. The methods for artificial synthesis of high-purity quartz mainly include the following: (1) Gas phase synthesis method, using organic silicon or related derivatives as raw materials, gasifying them and mixing them with hydrogen and oxygen, hydrolyzing them at high temperature to form mist-like SiO2, and finally obtaining quartz products through gas-solid separation such as cooling, separation, and deacidification. This method is easy to obtain quartz materials with high purity, but it has high energy consumption and high cost. (2) Chemical precipitation method, using sodium silicate and carbon dioxide or acid solution as raw materials, mixing and reacting at a certain synthesis temperature to obtain metasilicic acid precipitate, and then preparing quartz materials through filtering, washing, drying, and calcining processes. This method has the advantages of easy operation, simple production process, easy availability of raw materials, low energy consumption and investment, but the purity of the obtained product is low, and it is difficult to obtain high-purity quartz materials with purity that meets the standard. (3) The sol-gel method uses silicon-containing inorganic salts or hydrolyzable silicon sources as raw materials, adds acid or alkaline solutions as catalysts, and performs hydrolysis and polycondensation to form SiO2 gel. The organic solvent in the gel is filtered and washed, and then dried and calcined to obtain quartz material. This method has a simple production process, easy-to-control synthesis conditions, and is not strict on equipment and materials. However, the cost is high, the production cycle is long, and the industrial value is not great.

[0004] In summary, the existing technologies have the problems of serious environmental pollution, high energy consumption, low product purity and yield, inability to achieve industrialized production and high cost.

[0005] Therefore, finding a method for preparing high-purity quartz with low cost, low energy consumption, high product purity and easy industrial production is an urgent problem to be solved. Summary of the invention

[0006] The present invention aims to solve one of the technical problems in the related art to a certain extent. To this end, the present invention provides a method for preparing high-purity quartz using silicon granules and a high-purity quartz.

[0007] As a first aspect of the present invention, a method for preparing high-purity quartz using silicon granules is provided, comprising:

[0008] removing impurities from the initial silicon granules to obtain intermediate silicon granules;

[0009] The intermediate silicon particles and the oxidant are mixed, ground and stirred to obtain initial silicon dioxide powder;

[0010] The initial silicon dioxide powder is subjected to impurity removal treatment and then calcined to obtain high-purity quartz.

[0011] Furthermore, the impurity removal of the initial silicon granules comprises:

[0012] Removing organic impurities from the initial silicon granules to obtain first silicon granules;

[0013] The metal impurities in the first silicon granules are removed to obtain the intermediate silicon granules.

[0014] Furthermore, removing organic impurities in the initial silicon granule material includes at least one of water washing and filtration, organic solvent washing and filtration, and alkali washing and filtration.

[0015] Furthermore, removing metal impurities in the first silicon granules includes: acid washing and filtering.

[0016] Furthermore, the oxidant is water-soluble, and the impurity removal treatment of the initial silicon dioxide powder includes: at least one of water washing and filtration and acid washing and filtration.

[0017] Furthermore, the oxidant includes at least one of hydrogen peroxide, percarbonic acid and its salts, peracetic acid and its derivatives, dichloroisocyanuric acid and its salts, trichloroisocyanuric acid and its salts, chloric acid and its salts, hypochlorous acid and its salts, perchloric acid and its salts, and chlorous acid and its salts.

[0018] Furthermore, in the step of calcining the initial silica powder after removing impurities, the calcination temperature is between 500°C and 1300°C, the calcination time is between 20min and 300min, and the calcination atmosphere includes at least one of compressed air, nitrogen, argon, oxygen, chlorine, and hydrogen chloride gas.

[0019] Furthermore, the molar ratio of the oxidant to the intermediate silicon particles is between 1:1 and 10:1.

[0020] Furthermore, the grinding and stirring includes: at least one of normal temperature ball milling and heated ball milling.

[0021] As a second aspect of the present invention, a high-purity quartz is provided, wherein the high-purity quartz is prepared by the above method.

[0022] The object of the present invention is to provide a method for preparing high-purity quartz using silicon granules, by cleaning, removing impurities, grinding and oxidizing the silicon granules to make them into silicon dioxide powder. The silicon granules are firstly purified by impurities removal, and then the silicon element in the silicon granules is combined with oxygen by an oxidation method and retained in the silicon dioxide phase, so that other impurity elements are separated from the silicon granules, thereby purifying the silicon granules and obtaining silicon dioxide powder with higher purity. Finally, the silicon dioxide powder is further purified by calcination to prepare industrially usable high-purity quartz, which can recycle industrial cutting silicon waste, greatly reduce the raw material cost, give full play to the value of industrial waste, promote the recycling of resources, and at the same time, the preparation process is simple and efficient, and the production cost is greatly reduced.

[0023] The features and advantages of the present invention will be disclosed in detail in the following specific embodiments and drawings. The best embodiments or means of the present invention will be described in detail in conjunction with the drawings, but they are not intended to limit the technical solutions of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0025] Figure 1 It is a flow chart of an implementation method of the method for preparing high-purity quartz using silicon granules provided by the present invention;

[0026] Figure 2 It is the X-ray diffraction test data of Example 1 of the present invention. DETAILED DESCRIPTION

[0027] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.

[0028] References to "one embodiment" or "example" or "example" in this specification mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment disclosed herein. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.

[0029] The inventors have found that the cutting of silicon wafers in the semiconductor and solar energy industries produces a large amount of cutting waste, which contains a large amount of silicon particles. These silicon particles are mixed with impurities such as cutting fluid and diamond wire wear, and these impurities are attached to the surface of silicon particles or suspended in the cutting fluid. Silicon particles with higher purity can be obtained through a variety of impurity removal methods. Recycling these silicon particles has resource value and environmental significance. On the one hand, the current resource utilization of silicon particles is mainly focused on the preparation of high-purity silicon, silicon-containing alloys or ceramics, silicon-containing nitrides, silicon-containing nanomaterials, and silicon-containing electrode materials. There are a few reports on the preparation of silicon dioxide materials using silicon particles, but the production method is complicated, the temperature is high, and the cost is high. There is no report on the preparation of high-purity quartz by silicon particles. High-purity quartz generally refers to silicon dioxide with a silicon dioxide content higher than 99.99%.

[0030] On the other hand, the main methods for recycling and reusing silicon granules are: acid leaching, smelting, thermal plasma, aerosol reaction, physical method, etc. The purification methods have the problems of high environmental pollution, high production cost, low purity, low yield, and difficulty in industrial production.

[0031] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing high-purity quartz using silicon granules, wherein the preparation method comprises:

[0032] In step S110, the initial silicon granules are cleaned to obtain intermediate silicon granules;

[0033] In step S120, the intermediate silicon granules and the oxidant are mixed, ground and stirred to obtain initial silicon dioxide powder;

[0034] In step S130, the initial silicon dioxide powder is subjected to impurity removal treatment and then calcined to obtain high-purity quartz.

[0035] In step S110, the present invention does not specifically limit how to obtain the initial silicon particles. For example, the initial silicon particles can be obtained by purchasing them from outside. For another example, the initial silicon particles can be obtained by directly cutting silicon wafers using diamond wires.

[0036] The present invention does not impose any restrictions on the impurity removal method, and it is only necessary to remove impurities from the initial silicon granules. For example, impurities can be removed by chemical acid leaching. For another example, impurities can be removed by physical screening and filtration. For another example, impurities can be removed by high-temperature heat treatment followed by acid washing, filtration and drying. For another example, impurities can be removed by alcohol washing, acid washing, water washing, solid-liquid separation and vacuum drying.

[0037] The main component of the initial silicon granules is silicon, and the impurities include the cutting fluid (which is a mixture of various organic substances) used in the cutting process and the metal impurities worn off the diamond wire.

[0038] The present invention does not impose any restrictions on the method for removing organic impurities, and it only needs to meet the requirements of removing organic impurities in the initial silicon granules. For example, some impurities that are easily soluble in water can be removed by washing with water and filtering. For another example, organic impurities can be removed by washing with alkali or washing with an organic solvent and then filtering. For another example, impurities can be removed by flotation.

[0039] The present invention does not impose any limitation on the method for removing metal impurities. For example, metal impurities can be removed by acid washing and filtration. For another example, metal impurities can be separated by magnetic separation.

[0040] In step S120, the intermediate silicon granule material is mixed with the oxidant for grinding and stirring. During the grinding process, the silicon particles in the intermediate silicon granule material are continuously rubbed and collided, so that the particle size of the silicon particles continues to decrease. When the silicon particles exist in the form of silicon powder with a finer particle size, the silicon in powder form has a larger surface area, which is easier to contact and react with the oxidant. The oxidant can react with it more fully, thereby increasing the oxidation degree of the silicon particles, further oxidizing more unoxidized silicon particles into silicon dioxide, and accelerating the oxidation reaction rate. At the same time, since a large amount of heat is generated during the collision and friction process, the temperature increase will promote further oxidation, and finally all the intermediate silicon particles are oxidized into initial silicon dioxide powder.

[0041] The present invention does not impose any special limitation on the grinding method. It only needs to reduce the particle size of silicon particles and oxidize them. For example, manual grinding can be used. For another example, mechanical grinding can be used. For another example, high-energy ball milling can be used. In some embodiments, the grinding method uses a ball mill for ball milling oxidation. The ball milling oxidation can use at least one of room temperature ball milling and heated ball milling. The grinding balls of the ball mill are quartz balls or zirconia balls. The material hardness of the grinding balls needs to match the silicon powder abrasive. The use of quartz balls will not further pollute the ball mill to generate new impurities. The use of zirconia grinding balls has high wear resistance and high temperature resistance, and can fully grind the silicon powder in a high temperature environment to make the obtained particles smaller in size, which is more conducive to oxidation to form silicon dioxide.

[0042] The intermediate silicon granules are mixed with an oxidant, and the silicon on the surface of the silicon particles in the intermediate silicon granules is oxidized into silicon dioxide. However, the silicon dioxide on the surface of the silicon particles will be consumed by friction and collision during the grinding process, thereby exposing the internal silicon. The internal exposed silicon is further oxidized, and under repeated collision and friction, the initial silicon dioxide powder with a smaller particle size and completely oxidized and the remaining oxidant are finally obtained.

[0043] The present invention does not specifically limit the mixing method, as long as the intermediate silicon particles are dispersed in the oxidant in the form of silicon particles. For example, the intermediate silicon particles can be ground by a solid-liquid mixing method of physically stirring the intermediate silicon particles and the oxidant solution. For another example, the intermediate silicon particles can be ground by a mixing method of ultrasonically dispersing the intermediate silicon particles in the oxidant solution.

[0044] The present invention does not specifically limit the type of oxidant. It only needs to satisfy the ability to oxidize silicon particles into silicon dioxide and be removed from silicon dioxide powder. In some embodiments, the oxidant is water-soluble and has strong oxidizing ability, preferably but not limited to at least one of hydrogen peroxide, percarbonic acid and its salts, peracetic acid and its derivatives, dichloroisocyanuric acid and its salts, trichloroisocyanuric acid and its salts, chloric acid and its salts, hypochlorous acid and its salts, perchloric acid and its salts, and chlorous acid and its salts. For example, hydrogen peroxide is an oxidant that can react with silicon particles to produce water and silicon dioxide. When hydrogen peroxide reacts with silicon particles, the oxidation reaction is violent, releasing a large amount of energy, increasing the reaction temperature, and then accelerating the oxidation reaction rate, so that more silicon particles are oxidized to silicon dioxide faster.

[0045] The molar ratio of the oxidant to the intermediate silicon particles is between 1:1 and 10:1. In some embodiments, adding an excess of oxidant to the ball mill allows the silicon particles to undergo a sufficient redox reaction, thereby ensuring that the silicon particles are completely oxidized to obtain high-purity initial silicon dioxide powder.

[0046] The impurity removal treatment of the initial silicon dioxide powder includes at least one of water washing and filtration and acid washing and filtration.

[0047] The present invention does not specifically limit the methods of water washing and filtration and acid washing and filtration, and only needs to remove the remaining excess oxidant. In some embodiments, the excess oxidant remaining from the oxidation reaction is dissolved in water and exists in liquid form, while the initial silicon dioxide generated by the reaction is insoluble in water. The excess oxidant is removed by water washing and filtration, and the silicon dioxide powder and the oxidant can be easily filtered and separated to obtain silicon dioxide powder with higher purity. This step greatly saves costs, and compared with other alkali washing or organic solvent washing methods, it will not further introduce new impurities, so that the silicon dioxide powder after washing has higher purity.

[0048] The filtered silica powder is further calcined to obtain high-purity quartz. In some embodiments, silica powder of quartz-grade purity can be obtained by the above method. The remaining impurities, such as free carbon, sulfur, moisture, organic matter and other impurities, can be further removed and purified by high-temperature calcination to obtain high-purity quartz. On the other hand, during the mixed oxidation of silicon particles and oxidants, a portion of amorphous silica powder is formed. The calcination causes the amorphous silica powder to undergo a crystallization transformation at high temperature, thereby obtaining high-purity crystalline silica, i.e., high-purity quartz.

[0049] The present invention does not impose any special restrictions on the calcination process. It only needs to satisfy that the heating temperature is within the calcination temperature range of the present invention. For example, high-purity quartz can be obtained by laser heating silica powder. For another example, high-purity quartz can be obtained by heating silica powder in a high-temperature smelting furnace.

[0050] In the step of calcining to obtain high-purity quartz, the calcination temperature is between 500°C and 1300°C, and the calcination time is between 20min and 300min. In some embodiments, the calcination atmosphere includes at least one of compressed air, nitrogen, argon, oxygen, chlorine, and hydrogen chloride gas.

[0051] At the same time, in the present invention, the stage of silicon oxidation to form silicon dioxide is placed in the process of grinding and stirring, which reduces the high-temperature operating cost and is easier to control at low temperatures compared to the traditional method of obtaining silicon dioxide by high-temperature calcination.

[0052] The present invention also provides a high-purity quartz material, which is prepared by the above method.

[0053] In the present invention, silicon granules are purified by removing impurities, and then the silicon element in the silicon granules is combined with oxygen by an oxidation method and retained in the silicon dioxide phase, so that other impurity elements are separated and extracted from the silicon granules, and then the silicon dioxide powder is further purified by calcination to prepare industrially usable high-purity quartz.

[0054] The present invention will be further explained below in conjunction with the embodiments.

[0055] Example

[0056] In the following embodiments of the present invention, the initial silicon granules are waste materials generated during the diamond wire cutting process of single crystal silicon ingots.

[0057] When cutting silicon wafers, the coolant is a mixed solution containing a variety of organic substances, the wire cutting is diamond-wrapped metal wire, and the silicon wafers used are solar cell application grade silicon wafers with a resistivity of no less than 0.4Ω·cm.

[0058] Example 1

[0059] A method for preparing high-purity quartz using silicon granules comprises the following steps:

[0060] Step 1: First, weigh 1 kg of initial silicon particles, put it into deionized water for ultrasonic cleaning and filtering, repeat three times, then put it into 50% ethanol aqueous solution, ultrasonic cleaning and filtering, repeat three times, and repeatedly rinse with deionized water for several times, dry at 60°C for 3 hours, and obtain the first silicon particles. The various element contents of the first silicon particles are shown in Table 1 below, the particle size is between 0.5 microns and 3 microns, and the weight is 973g;

[0061] Table 1

[0062] element Si B P Fe Cr Ni Cu content(%) 99.9999 0.00002 0.000004 0.000000003 <0.0000000001 <0.0000000001 <0.0000000001

[0063] Step 2: The first silicon granules obtained in step 1 are placed in a 10% nitric acid aqueous solution, and are ultrasonically cleaned for 0.5 hours, and then filtered, and the process is repeated three times, and the particles are repeatedly rinsed with deionized water for several times, and dried at 60° C. for 3 hours to obtain intermediate silicon granules. The content of various elements in the intermediate silicon granules is shown in Table 2 below. The Si content is greater than 99.9999%, the particle size is between 0.5 μm and 3 μm, and the weight is 967 g;

[0064] Table 2

[0065] element Si B P Fe Cr Ni Cu content(%) 99.9999 0.00002 0.000004 0.0000000028 <0.0000000001 <0.0000000001 <0.0000000001

[0066] Step 3: Put the intermediate silicon particles obtained in step 2 and a 15% concentration hydrogen peroxide solution into a horizontal drum ball mill at a mass ratio of silicon: hydrogen peroxide solution = 1:20, and ball mill at a speed of 100 rpm for 8 hours to obtain an initial silicon dioxide powder slurry;

[0067] Step 4: The initial silica powder slurry obtained in step 3 is coarsely filtered, then ultrasonically cleaned in deionized water, and then filtered, and the process is repeated three times. The obtained solid is then placed in a 10% hydrochloric acid solution, ultrasonically cleaned for 1 hour, and then filtered, and the process is repeated three times. The solid is repeatedly rinsed with deionized water for several times, and dried in a vacuum drying oven at 80° C. for 1 hour to obtain intermediate silica powder. The contents of various impurity elements in the intermediate silica powder are shown in Table 3 below. The particle size is between 0.2 μm and 1.5 μm, and the weight is 1639 g.

[0068] Table 3

[0069] element B P Fe Cr Ni Cu Content (ppm) 0.16 0.03 0.28 <0.1 <0.1 <0.1

[0070] Step 5: Take 500 g of the intermediate silica powder in step 4, put it into a corundum crucible, and then place the corundum crucible in a tubular furnace, introduce oxygen, and the gas flow rate is 2 L / min. Heat and calcine. Raise the temperature to 1100°C at a rate of 20°C / min, and calcine for 2 hours to obtain a block of high-purity quartz sample 1. The contents of various impurity elements in the high-purity quartz sample 1 are shown in Table 4 below.

[0071] Table 4

[0072] element B P Fe Cr Ni Cu Content (ppm) 0.13 0.02 0.26 <0.1 <0.1 <0.1

[0073] Example 2

[0074] High-purity quartz was prepared by the same preparation method as in Example 1, except that the intermediate silicon particles obtained in step 2 were mixed with a 10% concentration of dichloroisocyanuric acid solution in a mass ratio of 1:15 to prepare a high-purity quartz sample 2. The contents of various impurity elements in the high-purity quartz sample 2 are shown in Table 5 below.

[0075] Table 5

[0076]

[0077]

[0078] Test Case

[0079] Using ICP-MS equipment, the high-purity quartz sample 1 obtained in Example 1 was subjected to a full spectrum scan of impurities, and the contents of various impurities obtained are shown in Table 6 below:

[0080] Table 6

[0081]

[0082]

[0083] According to the test results, it can be concluded that by removing impurities and purifying the silicon waste generated in the cutting process according to the present invention, silicon granules with an Si content greater than 99.9999% can be obtained, and the impurity removal method used is simple, low-cost, and effectively removes impurities, and the obtained silicon has a higher purity; secondly, the silicon granules are mixed and ground with a water-soluble strong oxidant, and the silicon element in the purified silicon granules is combined with oxygen and retained in the silicon dioxide phase, so that other impurity elements that are difficult to remove can be separated and extracted from the silicon granules, and silicon dioxide granules with higher purity can be further obtained, and then the silicon dioxide is further purified by calcination to prepare industrially usable high-purity quartz.

[0084] The high purity quartz sample 1 obtained in Example 1 was analyzed by X-ray diffractometer. The results are as follows: Figure 2 As shown, sample 1 in the present invention has a high-intensity, clear and sharp diffraction peak. Figure 2 The peak values ​​and peak positions in the X-ray diffraction peaks correspond one-to-one with the peak values ​​and peak positions of the standard α-quartz phase. Each diffraction peak position can correspond to a specific crystal plane of the α-quartz phase, and there are no other impurity peaks. Therefore, it can be concluded based on the above information that the products obtained by the present invention are all α-quartz phases.

[0085] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the drawings and the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.

Claims

1. A method for preparing high-purity quartz using silicon granules, It is characterized in that include: removing impurities from the initial silicon granules to obtain intermediate silicon granules; The intermediate silicon particles and the oxidant are mixed, ground and stirred to obtain initial silicon dioxide powder; The initial silicon dioxide powder is subjected to impurity removal treatment and then calcined to obtain high-purity quartz.

2. The method according to claim 1, It is characterized in that The method of removing impurities from the initial silicon granules comprises: Removing organic impurities from the initial silicon granules to obtain first silicon granules; The metal impurities in the first silicon granules are removed to obtain the intermediate silicon granules.

3. The method according to claim 2, It is characterized in that Removing organic impurities from the initial silicon granules includes at least one of water washing and filtration, organic solvent washing and filtration, and alkali washing and filtration.

4. The method according to claim 2, It is characterized in that Removing metal impurities in the first silicon granule material includes: acid washing and filtering.

5. The method according to claim 1, It is characterized in that The oxidant is water-soluble, and the impurity removal treatment of the initial silicon dioxide powder includes at least one of water washing and filtration and acid washing and filtration.

6. The method according to claim 5, It is characterized in that The oxidant includes at least one of hydrogen peroxide, percarbonic acid and its salts, peracetic acid and its derivatives, dichloroisocyanuric acid and its salts, trichloroisocyanuric acid and its salts, chloric acid and its salts, hypochlorous acid and its salts, perchloric acid and its salts, and chlorous acid and its salts.

7. The method according to claim 1, It is characterized in that In the step of calcining the initial silica powder after removing impurities, the calcination temperature is between 500° C. and 1300° C., the calcination time is between 20 min and 300 min, and the calcination atmosphere includes at least one of compressed air, nitrogen, argon, oxygen, chlorine, and hydrogen chloride gas.

8. The method according to any one of claims 1 to 7, It is characterized in that The molar ratio of the oxidant to the intermediate silicon particles is between 1:1 and 10:

1.

9. The method according to any one of claims 1 to 7, It is characterized in that The grinding and stirring comprises at least one of room temperature ball milling and heated ball milling.

10. A high purity quartz, It is characterized in that The high-purity quartz is prepared by the method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of high-purity low-uranium submicron spherical silicon dioxide micropowder

    CN114031086A

  • Method for preparing nanoscale silicon dioxide by wet oxidation of diamond wire cutting silicon wafer waste

    CN114180584A

  • High-purity micro-nano silicon powder purified from cut silicon waste in photovoltaic industry as well as purification method and application of high-purity micro-nano silicon powder

    CN114655959A

  • Method for preparing high-purity quartz sand from superfine silicon powder

    CN115676842A

  • Preparation method of high-purity cristobalite