Biomass fiber reinforced high-toughness polycarbonate composite material and preparation method thereof

By combining modified biomass fibers with polycarbonate, the gap sensitivity and stress cracking problems of polycarbonate materials are solved, toughness and environmental protection are improved, and higher mechanical strength and cost-effectiveness are achieved.

CN118895041APending Publication Date: 2024-11-05NANJING FORESTRY UNIV

Patent Information

Application Number
CN202410820413.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Polycarbonate materials have insufficient notch sensitivity and stress cracking, and traditional glass fiber or carbon fiber reinforced materials have environmental protection and cost problems.

Method used

Use biomass fibers (such as bamboo fiber, hemp fiber, coconut fiber) for modification and compound with polycarbonate, add coupling agent, antioxidant, toughening compatibility agent and flame retardant, and extrude through twin screws Process to prepare high-tough composite materials.

Benefits of technology

It improves the toughness and mechanical strength of polycarbonate materials, reduces notch sensitivity, and has better environmental protection characteristics and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of polycarbonate composite materials, and particularly discloses a biomass fiber reinforced high-toughness polycarbonate composite material and a preparation method thereof. The biomass fibers comprise bamboo fibers, jute fibers and coconut fibers, the biomass fibers are subjected to modification treatment and then are subjected to melt blending extrusion with polycarbonate, a coupling agent, an antioxidant, a toughening compatilizer and a flame retardant, and the biomass fiber reinforced high-toughness polycarbonate composite material is obtained. The biomass fiber used in the method is green, environment-friendly and low in price, the processing method is simple and safe, and the obtained material can be used in various occasions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polycarbonate composite materials, in particular to a biomass fiber reinforced high-toughness polycarbonate composite material and a preparation method thereof. Background Art

[0002] Polycarbonate (PC) refers to a high molecular polymer containing carbonate groups in the polymer molecular chain. It can be divided into aliphatic, aromatic, aliphatic-aromatic and other types according to the ester structure. It is one of the fastest growing general engineering plastics. However, polycarbonate molecular chains contain a large number of benzene rings, which makes it difficult for the molecular chain to move, resulting in a high viscosity of the polycarbonate melt. A large amount of stress remains in the injection molded products produced, and they will break during storage and use. At the same time, PC is a notch-sensitive material. In order to improve the notch sensitivity and stress cracking of polycarbonate materials, glass fiber or carbon fiber is used in actual production to enhance and modify polycarbonate to improve mechanical strength. In addition, with the popularization of green environmental protection, people are doing better and better in protecting the environment and sustainable development. Biomass fiber, as an environmentally friendly material, has the advantages of low price, degradability and recyclability compared to other fiber materials. Summary of the invention

[0003] The purpose of the present invention is to provide a biomass fiber reinforced high-toughness polycarbonate composite material and a preparation method thereof. The composite material uses biomass fiber instead of glass fiber or carbon fiber to modify polycarbonate, improve its toughness, solve the problems of notch sensitivity and stress cracking of polycarbonate materials, and also has the characteristics of being green and environmentally friendly.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: A biomass fiber reinforced high-toughness polycarbonate composite material, the composite material is made of polycarbonate, biomass fiber, coupling agent, toughening compatibilizer, antioxidant, and flame retardant. The mass fractions of the various components of the polycarbonate are as follows: 60-95 parts of polycarbonate, 6-24 parts of biomass fiber, 2-10 parts of coupling agent, 0.2-2 parts of antioxidant, 0.2-2 parts of toughening compatibilizer, and 0.05-1 part of flame retardant.

[0005] The polycarbonate is a compound of one or more of bisphenol A polycarbonate, polyester polycarbonate and cyclohexane bisphenol A polycarbonate.

[0006] The viscosity average molecular weight of the polycarbonate is 14000-26000.

[0007] The biomass fiber is prepared by the following method: (1) Take 2 to 8 parts of bamboo fiber, hemp fiber and coconut fiber, immerse them in 2% to 5% NaOH solution, keep them warm at 55 to 65 °C for 3 to 5 h, take out the fibers, rinse them with deionized water until the pH is neutral, dry and dehydrate them until the weight no longer changes, and grind the three fibers separately.

[0008] (2) The crushed coconut fiber and maleic anhydride are mixed and ball-milled in a weight ratio of 1:0.4-0.6. The speed of the ball mill should be set at 280-350 rpm and the grinding time should be controlled at 1-3 hours. After the grinding, the mixture is washed with ethanol and then placed in a drying oven for drying; (3) Mix the crushed hemp fiber, acetic anhydride and pyridine in a weight ratio of 1:0.4-0.6:4-6, stir evenly, continuously introduce nitrogen, keep warm at 75-85°C for 4-6 hours, cool, add acetone for washing, filter, and vacuum dry; (4) Mix the crushed bamboo fiber and concentrated sulfuric acid in a volume ratio of 1:8-12, keep warm at 75-85°C for 0.5-2h, filter, rinse with deionized water until the pH is neutral, add 2-3 times the weight of dimethylformamide, keep warm at 50-70°C for 1-3h, filter, and vacuum dry.

[0009] (5) The modified bamboo fiber, hemp fiber and coconut fiber are mixed evenly to obtain biomass fiber.

[0010] The coupling agent is a combination of one or more of 3-aminopropyl triethoxysilane, isopropyl dioleate acyloxy titanate, and isopropyl tristearate titanate; the antioxidant is a combination of one or more of antioxidant 168, antioxidant 1010, and antioxidant 1076; the toughening compatibilizer is a combination of one or more of styrene-acrylonitrile-maleic anhydride terpolymer and methyl methacrylate-butadiene-styrene copolymer; and the flame retardant is decabromodiphenyl ethane.

[0011] A method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material comprises the following steps: (1) drying the polycarbonate while continuously introducing nitrogen during the drying process. After the drying is completed, adding a coupling agent, an antioxidant, and a flame retardant to the polycarbonate in proportion to each other, and then stirring the mixture to obtain a polycarbonate mixture. (2) After the polycarbonate mixture is prepared, it is twin-screw extruded with the treated biomass fiber; (3) The extruded product is cooled, pelletized, and the pellets are tested and packaged to obtain the finished product.

[0012] The polycarbonate is dried at a temperature of 240 to 250° C. and for a drying time of 4 to 6 hours.

[0013] The rotation speed of the twin-screw extruder is 350-400 rpm, the extrusion temperature is set at 150-160° C. in zone 1, 210-220° C. in zone 2, 260-270° C. in zone 3, 300-320° C. in zone 4 to the die head, and the vacuum degree is -0.06--0.08 MPa.

[0014] The temperature of the cooling medium is 50-65°C when the product is cooled.

[0015] The beneficial effect achieved by the present invention is to use biomass fiber to enhance the toughness of polycarbonate, by sulfonating bamboo fiber, introducing sulfonic acid groups on bamboo fiber, improving its chemical stability and other properties, acetylation of hemp fiber, replacing hydroxyl groups on the fiber surface with acetyl groups, reducing its polarity, enhancing its mechanical processing, dimensional stability and thermal stability and other properties; ball milling coconut fiber with maleic anhydride to improve its compatibility with hydrophobic matrix and other properties. After the three fibers are evenly mixed, they are grafted onto polycarbonate to enhance its chemical stability, mechanical processing, thermal stability and other properties. At the same time, the composite material prepared by adding other additives has higher toughness and better notch sensitivity than ordinary polycarbonate materials. At the same time, compared with the use of glass fiber or carbon fiber for reinforcement and toughening, biomass fiber has the advantages of wide source, low cost and more environmental protection. DETAILED DESCRIPTION

[0016] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.

[0017] Bisphenol A polycarbonate (P301655) was provided by Shanghai Aladdin; 3-aminopropyltriethoxysilane (A800523), antioxidant 168 (T822863), antioxidant 1076 (I811772), decabromodiphenylethane (B802485) were provided by Shanghai Maclean; styrene-acrylonitrile-maleic anhydride terpolymer (SAM-010) was provided by Shanghai Jiayirong.

[0018] Example 1: A biomass fiber reinforced high-toughness polycarbonate composite material and its preparation method A biomass fiber reinforced high-toughness polycarbonate composite material, the composite material is made of the following raw materials in parts by weight: 95 parts of bisphenol A polycarbonate, 6 parts of biomass fiber, 2 parts of 3-aminopropyltriethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane.

[0019] The biomass fiber is prepared by the following method: (1) Take 2 parts of bamboo fiber, flax fiber and coconut fiber, immerse them in 2% to 5% NaOH solution respectively, keep them at 60℃ for 4 h, take out the fibers, rinse them with deionized water until the pH is neutral, dehydrate them in a constant temperature drying oven until the weight no longer changes, and grind the three fibers separately.

[0020] (2) The crushed coconut fiber and maleic anhydride are mixed and ball-milled in a weight ratio of 1:0.5. The rotation speed during ball milling should be set at 280-350 rpm and the grinding time should be controlled at 2 h. After the grinding, the obtained mixture is washed with ethanol and then placed in a drying oven for drying; (3) Mix the crushed hemp fiber, acetic anhydride and pyridine in a weight ratio of 1:0.5:5, stir evenly, continuously introduce nitrogen, keep warm at 80°C for 5 hours, cool, add acetone for washing, filter, and place in a drying oven for vacuum drying; (4) Mix the crushed bamboo fiber and concentrated sulfuric acid in a volume ratio of 1:10, keep warm at 80°C for 1 hour, filter, rinse with deionized water until the pH is neutral, add 2.5 times the weight of dimethylformamide, keep warm at 60°C for 2 hours, filter, and place in a drying oven for vacuum drying; (5) The modified bamboo fiber, hemp fiber and coconut fiber are mixed evenly to obtain 6 parts of biomass fibers.

[0021] A method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material comprises the following steps: (1) Place 95 parts of polycarbonate in a drying oven for drying. Nitrogen is continuously introduced during drying. The drying temperature is set to 245°C and the drying time is 5 hours. Add 2 parts of 3-aminopropyltriethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane to the polycarbonate in proportion, and then stir evenly to obtain a polycarbonate mixture. The speed during stirring should be controlled at 320-350rpm to ensure that the mixture is fully uniform; (2) After the polycarbonate mixture is prepared, it is fed into the first feed port of the twin-screw extruder, and the processed biomass fiber is fed into the second feed port of the twin-screw extruder. The extruder speed is set to 350-400 rpm to ensure smooth extrusion of high-toughness polycarbonate. The extruder temperature is set to 150°C in zone 1, 220°C in zone 2, 260°C in zone 3, and 300°C in zone 4 to the die head to ensure the quality of the extruded product. At the same time, the vacuum degree should be controlled at -0.06-0.08 MPa to prevent gas from being generated during the extrusion process; (3) The extruded product needs to be cooled in a water tank. The temperature of the water tank should be set to a constant temperature of 65°C to ensure the stability of the product. The cooled product is introduced into a pelletizer for pelletizing. The speed of the pelletizer is set to 650rpm to ensure that the size of the pellets is uniform. After the cut pellets are tested and packaged, the finished product can be obtained.

[0022] Example 2: A biomass fiber reinforced high-toughness polycarbonate composite material and its preparation method A biomass fiber reinforced high-toughness polycarbonate composite material, the composite material is made of the following raw materials in parts by weight: 90 parts of bisphenol A polycarbonate, 12 parts of biomass fiber, 2 parts of 3-aminopropyltriethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane.

[0023] The biomass fiber is prepared by the following method: (1) Take 4 parts of bamboo fiber, flax fiber and coconut fiber, immerse them in 2% to 5% NaOH solution respectively, keep them at 60℃ for 4 h, take out the fibers, rinse them with deionized water until the pH is neutral, dehydrate them in a constant temperature drying oven until the weight no longer changes, and grind the three fibers separately.

[0024] (2) The crushed coconut fiber and maleic anhydride are mixed and ball-milled in a weight ratio of 1:0.5. The speed of the ball mill should be set at 280-350 rpm and the grinding time is controlled at 2 h. After the grinding, the mixture is washed with ethanol and then placed in a drying oven for drying; (3) Mix the crushed hemp fiber, acetic anhydride and pyridine in a weight ratio of 1:0.5:5, stir evenly, continuously introduce nitrogen, keep warm at 80°C for 5 hours, cool, add acetone for washing, filter, and place in a drying oven for vacuum drying; (4) Mix the crushed bamboo fiber and concentrated sulfuric acid in a volume ratio of 1:10, keep warm at 80°C for 1 hour, filter, rinse with deionized water until the pH is neutral, add 2.5 times the weight of dimethylformamide, keep warm at 60°C for 2 hours, filter, and place in a drying oven for vacuum drying; (5) The modified bamboo fiber, hemp fiber and coconut fiber are mixed evenly to obtain 12 parts of biomass fibers.

[0025] A method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material comprises the following steps: (1) Place 90 parts of polycarbonate in a drying oven for drying. After drying, add 2 parts of 3-aminopropyl triethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane to the polycarbonate, and then stir evenly to obtain a polycarbonate mixture. The speed during stirring should be controlled at 320-350 rpm to ensure that the mixture is fully uniform; (2) After the polycarbonate mixture is prepared, it is fed into the first feed port of the twin-screw extruder, and the processed biomass fiber is fed into the second feed port of the twin-screw extruder. The extruder speed is set to 350-400 rpm to ensure smooth extrusion of high-toughness polycarbonate. The extruder temperature is set to 150°C in zone 1, 220°C in zone 2, 260°C in zone 3, and 300°C in zone 4 to the die head to ensure the quality of the extruded product. At the same time, the vacuum degree should be controlled at -0.06-0.08 MPa to prevent gas from being generated during the extrusion process; (3) The extruded product needs to be cooled in a water tank. The temperature of the water tank should be set to a constant temperature of 65°C to ensure the stability of the product. The cooled product is introduced into a pelletizer for pelletizing. The speed of the pelletizer is set to 650rpm to ensure that the size of the pellets is uniform. After the cut pellets are tested and packaged, the finished product can be obtained.

[0026] Example 3: A biomass fiber reinforced high-toughness polycarbonate composite material and its preparation method A biomass fiber reinforced high-toughness polycarbonate composite material, the composite material is made of the following raw materials in parts by weight: 80 parts of bisphenol A polycarbonate, 24 parts of biomass fiber, 2 parts of 3-aminopropyltriethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane.

[0027] The biomass fiber is prepared by the following method: (1) Take 8 parts of bamboo fiber, flax fiber and coconut fiber respectively, immerse them in 2% to 5% concentration NaOH solution, keep them at 60℃ for 4 h, take out the fibers, rinse them with deionized water until the pH is neutral, put them in a constant temperature drying oven to dehydrate until the weight no longer changes, and grind the three fibers separately.

[0028] (2) The crushed coconut fiber and maleic anhydride are mixed and ball-milled in a weight ratio of 1:0.5. The speed of the ball mill should be set at 280-350 rpm and the grinding time is controlled at 2 h. After the grinding, the mixture is washed with ethanol and then placed in a drying oven for drying; (3) Mix the crushed hemp fiber, acetic anhydride and pyridine in a weight ratio of 1:0.5:5, stir evenly, continuously introduce nitrogen, keep warm at 80°C for 5 hours, cool, add acetone for washing, filter, and place in a drying oven for vacuum drying; (4) Mix the crushed bamboo fiber and concentrated sulfuric acid in a volume ratio of 1:10, keep warm at 80°C for 1 hour, filter, rinse with deionized water until the pH is neutral, add 2.5 times the weight of dimethylformamide, keep warm at 60°C for 2 hours, filter, and place in a drying oven for vacuum drying; (5) The modified bamboo fiber, hemp fiber and coconut fiber are mixed evenly to obtain 24 parts of biomass fibers.

[0029] A method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material comprises the following steps: (1) Put 80 parts of polycarbonate into a drying oven for drying. After drying, add 2 parts of 3-aminopropyl triethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane to the polycarbonate according to the proportion, and then stir evenly to obtain a polycarbonate mixture. The speed during stirring should be controlled at 320-350rpm to ensure that the mixture is fully uniform; (2) After the polycarbonate mixture is prepared, it is fed into the first feed port of the twin-screw extruder, and the processed biomass fiber is fed into the second feed port of the twin-screw extruder. The extruder speed is set to 350-400 rpm to ensure smooth extrusion of high-toughness polycarbonate. The extruder temperature is set to 150°C in zone 1, 220°C in zone 2, 260°C in zone 3, and 300°C in zone 4 to the die head to ensure the quality of the extruded product. At the same time, the vacuum degree should be controlled at -0.06-0.08 MPa to prevent gas from being generated during the extrusion process; (3) The extruded product needs to be cooled in a water tank. The temperature of the water tank should be set to a constant temperature of 65°C to ensure the stability of the product. The cooled product is introduced into a pelletizer for pelletizing. The speed of the pelletizer is set to 650rpm to ensure that the size of the pellets is uniform. After the cut pellets are tested and packaged, the finished product can be obtained.

[0030] Based on Example 3, a control experiment was carried out, specifically Comparative Example 1 and Comparative Example 2, as described below: Comparative Example 1: No biomass fiber was added, and other conditions were carried out according to the steps of Example 1.

[0031] A high-toughness polycarbonate composite material, the composite material is made of the following raw materials in parts by weight: 80 parts of bisphenol A polycarbonate, 2 parts of 3-aminopropyltriethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane.

[0032] A method for preparing a high-toughness polycarbonate composite material comprises the following steps: (1) Put 80 parts of polycarbonate into a drying oven for drying. After drying, add 2 parts of 3-aminopropyl triethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane to the polycarbonate according to the proportion, and then stir evenly to obtain a polycarbonate mixture. The speed during stirring should be controlled at 320-350rpm to ensure that the mixture is fully uniform; (2) After the polycarbonate mixture is prepared, it is fed into the first feed port and the second feed port of the twin-screw extruder. The extruder speed is set to 350-400 rpm to ensure smooth extrusion of high-toughness polycarbonate. The extruder temperature is set to 150°C in zone 1, 220°C in zone 2, 260°C in zone 3, and 300°C in zone 4 to the die head to ensure the quality of the extruded product. At the same time, the vacuum degree should be controlled at -0.06-0.08 MPa to prevent gas from being generated during the extrusion process. (3) The extruded product needs to be cooled in a water tank. The temperature of the water tank should be set to a constant temperature of 65°C to ensure the stability of the product. The cooled product is introduced into a pelletizer for pelletizing. The speed of the pelletizer is set to 650rpm to ensure that the size of the pellets is uniform. After the cut pellets are tested and packaged, the finished product can be obtained.

[0033] Comparative Example 2: The biomass fiber was not modified, and the remaining conditions were the same as those in Example 3.

[0034] A biomass fiber reinforced high-toughness polycarbonate composite material, the composite material is made of the following raw materials in parts by weight: 80 parts of bisphenol A polycarbonate, 24 parts of biomass fiber, 2 parts of 3-aminopropyltriethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane.

[0035] The biomass fiber is prepared by the following method: Take 8 parts of bamboo fiber, hemp fiber and coconut fiber of equal weight, immerse them in 2% to 5% concentration NaOH solution respectively, keep warm at 60℃ for 4h, take out the fibers, rinse with deionized water until the pH is neutral, dry and dehydrate until the weight no longer changes, crush the three fibers separately, mix them evenly to obtain 24 parts of biomass fibers in total.

[0036] A method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material comprises the following steps: (1) Put 80 parts of polycarbonate into a drying oven for drying. After drying, add 2 parts of 3-aminopropyl triethoxysilane, 0.5 parts of a mixture of antioxidant 168 and antioxidant 1076 in a weight ratio of 1:3, 1 part of styrene-acrylonitrile-maleic anhydride terpolymer, and 0.2 parts of decabromodiphenylethane to the polycarbonate according to the proportion, and then stir evenly to obtain a polycarbonate mixture. The speed during stirring should be controlled at 320-350rpm to ensure that the mixture is fully uniform; (2) After the polycarbonate mixture is prepared, it is fed into the first feed port of the twin-screw extruder, and the processed biomass fiber is fed into the second feed port of the twin-screw extruder. The extruder speed is set to 350-400 rpm to ensure smooth extrusion of high-toughness polycarbonate. The extruder temperature is set to 150°C in zone 1, 220°C in zone 2, 260°C in zone 3, and 300°C in zone 4 to the die head to ensure the quality of the extruded product. At the same time, the vacuum degree should be controlled at -0.06-0.08 MPa to prevent gas from being generated during the extrusion process; (3) The extruded product needs to be cooled in a water tank. The temperature of the water tank should be set to a constant temperature of 65°C to ensure the stability of the product. The cooled product is introduced into a pelletizer for pelletizing. The speed of the pelletizer is set to 650rpm to ensure that the size of the pellets is uniform. After the cut pellets are tested and packaged, the finished product can be obtained.

[0037] Detection experiment: Equal amounts of the finished materials prepared in Example 1, Example 2, and Example 3 were respectively taken to make test samples, and their performance was tested according to ISO standards.

[0038] The results are as follows:

[0039] Conclusion: From the three groups of experiments, it can be seen that Example 3 performs better than Example 1, Example 2, Comparative Example 1 and Comparative Example 2, indicating that adding treated biomass fibers can indeed improve the toughness, surface sensitivity and other properties of polycarbonate.

[0040] It can be seen that the biomass fiber reinforced high-toughness polycarbonate composite material of the present invention improves the toughness and impact resistance of polycarbonate, greatly improves the processing performance, and has progressive significance for the application of polycarbonate materials.

[0041] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.

Claims

1. A biomass fiber reinforced high-toughness polycarbonate composite material, characterized in that: It is made of polycarbonate, biomass fiber, coupling agent, antioxidant, toughening compatibilizer and flame retardant, and the mass proportion of each component is as follows: 60-95 parts of polycarbonate, 6-24 parts of biomass fiber, 2-10 parts of coupling agent, 0.2-2 parts of antioxidant, 0.2-2 parts of toughening compatibilizer, and 0.05-1 part of flame retardant.

2. The biomass fiber reinforced high-toughness polycarbonate composite material according to claim 1, characterized in that: The biomass fiber consists of bamboo fiber, hemp fiber and coconut fiber.

3. The biomass fiber reinforced high-toughness polycarbonate composite material according to claim 1, characterized in that: The polycarbonate is a compound of one or more of bisphenol A polycarbonate, polyester polycarbonate and cyclohexane bisphenol A polycarbonate.

4. The biomass fiber reinforced high-toughness polycarbonate composite material according to claim 1, characterized in that: The viscosity average molecular weight of the polycarbonate is 16000-28000.

5. The biomass fiber reinforced high-toughness polycarbonate composite material according to claim 1, characterized in that: The biomass fiber is prepared by the following method: (1) Take equal weights of bamboo fiber, hemp fiber, and coconut fiber, immerse them in 2wt% to 5wt% NaOH solution, keep them at 55 to 65°C for 3 to 5 hours, take out the fibers, rinse them with deionized water until the pH is neutral, dry and dehydrate them until the weight no longer changes, and grind the three fibers separately; (2) The crushed coconut fiber and maleic anhydride are mixed and ball-milled in a weight ratio of 1:0.4-0.

6. The rotation speed during ball milling should be set at 280-350 rpm and the grinding time should be controlled at 1-3 hours. After the grinding, the obtained mixture is washed with ethanol and then dried; (3) Mix the crushed hemp fiber, acetic anhydride and pyridine in a weight ratio of 1:0.4-0.6:4-6, stir evenly, continuously introduce nitrogen, keep warm at 75-85°C for 4-6 hours, cool, add acetone for washing, filter, and vacuum dry; (4) Mix the crushed bamboo fiber and concentrated sulfuric acid in a volume ratio of 1:8-12, keep warm at 75-85°C for 0.5-2h, filter, rinse with deionized water until the pH is neutral, add 2-3 times the weight of dimethylformamide, keep warm at 50-70°C for 1-3h, filter, and vacuum dry; (5) The modified bamboo fiber, hemp fiber and coconut fiber are mixed evenly to obtain biomass fiber.

6. The biomass fiber reinforced high-toughness polycarbonate composite material according to claim 1, characterized in that: The coupling agent is a combination of one or more of 3-aminopropyl triethoxysilane, isopropyl dioleate acyloxy titanate, and isopropyl tristearate titanate; the antioxidant is a combination of one or more of antioxidant 168, antioxidant 1010, and antioxidant 1076; the toughening compatibilizer is a combination of one or more of styrene-acrylonitrile-maleic anhydride terpolymer and methyl methacrylate-butadiene-styrene copolymer; and the flame retardant is decabromodiphenyl ethane.

7. The method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material according to claim 6, characterized in that: The following steps are involved: (1) drying the polycarbonate while continuously introducing nitrogen during the drying process. After the drying is completed, adding a coupling agent, an antioxidant, and a flame retardant to the polycarbonate in proportion to each other, and then stirring the mixture to obtain a polycarbonate mixture. (2) After the polycarbonate mixture is prepared, it is twin-screw extruded with the biomass fiber; (3) The extruded product is cooled, pelletized, and the pellets are tested and packaged to obtain the finished product.

8. The method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material according to claim 7, characterized in that: The drying temperature of polycarbonate is 240-250°C, and the drying time is 4-6 hours.

9. The method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material according to claim 7, characterized in that: The rotation speed of the twin-screw extruder is 350-400 rpm, the temperature is set to 150-160°C in zone 1, 210-220°C in zone 2, 260-270°C in zone 3, 300-320°C in zone 4 to the die head, and the vacuum degree is -0.06--0.08 MPa.

10. The method for preparing a biomass fiber reinforced high-toughness polycarbonate composite material according to claim 7, characterized in that: The cooling medium temperature is 50-65°C when the product is cooled.

Citation Information

Patent Citations

  • Polycarbonate / natural fiber composite material and preparation method thereof

    CN103788617A

  • Natural oil adsorbing material made of maize straw

    CN105126774A

  • Preparation method of modified natural rubber type tire tread compound

    CN108410033A

  • Stress cracking-resistant PC (Polycarbonate) material and preparation method thereof

    CN109666278A

Cited By

  • Reinforced and toughened polycarbonate material and preparation method thereof

    CN122080611A