Wave-absorbing material with anti-static surge performance and application of wave-absorbing material
By preparing wave absorbing materials containing FeSiAl magnetic powder and resin, the damage problem of static surges to electronic equipment in the prior art is solved, efficient electrostatic discharge and electromagnetic shielding are achieved, and the magnetic permeability and mechanical properties of the material are improved. In a variety of industrial applications.
Patent Information
- Application Number
- CN202411346652.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The prior art is difficult to effectively protect electronic devices from damage from static surges, especially when electromagnetic shielding technology is mainly used to solve electromagnetic interference, there is a lack of a method to improve the damage of static surges to electronic devices or their components.
A wave absorbing material consisting of 85~90% FeSiAl magnetic powder and 8~13% resin is used to prepare anti-static surge performance through special processes and formulations, including mixing, coating, drying and high-temperature hot pressing treatment. Wave-absorbing materials ensure high magnetic permeability, smooth surface, bubbles, and particles, providing a smooth magnetic circuit for electrostatic release.
Significantly improves the damage of static surges to electronic equipment or its components, improves the magnetic permeability and mechanical properties of wave absorbing materials, and is suitable for electromagnetic shielding and electrostatic discharge protection devices to ensure the normal operation and stable production of the equipment.
Smart Images

Figure CN118895058A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of wave-absorbing materials, and in particular relates to a wave-absorbing material with anti-static surge performance and application thereof. Background Art
[0002] The accidental generation of excessive voltage or current due to electrostatic discharge is called electrostatic surge. Generally, electrostatic discharge (ESD) can cause serious damage to electronic components in an instant because it involves the rapid discharge of high voltage, which may cause circuit damage or permanent failure. Therefore, in some cases, electrostatic surge may cause more direct and serious damage, especially to sensitive equipment that is not properly protected.
[0003] In the current existing technology, in order to protect electronic equipment from damage caused by electrostatic surges, ESD diodes and TVS diodes can be introduced to quickly conduct static electricity and limit the voltage peak; or components such as gas discharge tubes and varistors can be used to absorb or conduct the energy released by instantaneous electrostatic surges. However, although electromagnetic shielding technology can theoretically cut off the propagation of electromagnetic waves, there are few cases of using electromagnetic shielding technology to improve the damage caused by electrostatic surges to electronic equipment or its components. This is because electromagnetic shielding technology is mainly used to solve the problem of electromagnetic wave interference, and electromagnetic wave interference is usually continuous signal interference, which may affect the normal operation of electronic equipment, but will not necessarily cause immediate damage to the equipment or its components.
[0004] The principle of electromagnetic shielding can be understood from the transmission line theory. This method regards the shield as a section of the transmission line. When the electromagnetic wave radiation field approaches the shield, a part of it will be reflected on its surface, and the rest will be transmitted into the shield to continue transmission. In the shield, the electromagnetic wave will be attenuated and multiple reflections and transmissions will occur on the two interfaces. Therefore, the shielding mechanism of the electromagnetic wave propagating to the surface of the shield includes the reflection dissipation on the incident surface, the dissipation absorbed by the material when entering the shield, and the dissipation during multiple reflections and transmissions inside the shield. Summary of the invention
[0005] In order to improve the damage of electrostatic surge to electronic equipment, the present invention provides an absorbing material with anti-static surge performance and application thereof.
[0006] According to one aspect of the present invention, there is provided an absorbing material with anti-static surge performance. The raw materials for preparing the absorbing material include 85-90% FeSiAl magnetic powder and 8-13% resin in terms of mass percentage; wherein the FeSiAl magnetic powder has a D 50 The diameter is 50~70μm, and the apparent density (AD) is 0.38~0.45g / cm 3; The preparation of the absorbing material includes the following steps: S1. Mixing the raw materials to obtain a slurry; S2. Applying the slurry on the surface of the film and simultaneously performing an orientation treatment to form a coating film from the slurry; then drying the coating film to a coating with a solvent content of 15-25% and a thickness of 60-100 μm through a drying treatment; S3. Performing a high-temperature hot pressing treatment on the coating, wherein the reaction temperature of the high-temperature hot pressing treatment is not less than 160°C, and the reaction pressure is not less than 160 Kg.
[0007] The present invention can prepare an absorbing material with anti-static surge performance through a special process and formula. Specifically, the present invention can ensure that the absorbing material has a smooth magnetic circuit at the moment of static electricity release by introducing a relatively high content of FeSiAl magnetic powder. Furthermore, by performing orientation treatment with auxiliary FeSiAl magnetic powder during the coating process, it can ensure that the magnetic powders are connected to each other, which can not only improve the magnetic permeability of the absorbing material, but also enable the absorbing material to have a smooth magnetic circuit when encountering static electricity release, so that static electricity can be released smoothly without affecting electronic components. In addition, the present invention can provide good reaction conditions for the preparation of absorbing materials by controlling the solvent content of the coating and the reaction temperature and pressure of the high-temperature hot pressing treatment, so that the surface of the absorbing material is smooth, free of bubbles and particles, thereby ensuring that the absorbing material can improve the damage of static electricity surges to electronic equipment or its components.
[0008] Preferably, the resin comprises a polyurethane resin, and the polyurethane resin comprises at least one of a polyether polyurethane resin, a polyester polyurethane resin, a polyimide polyurethane resin, and a polyurea polyurethane resin.
[0009] Preferably, the resin also includes acrylic resin, and the mass ratio is acrylic resin: polyurethane resin = 1~1.5:8.5~9. The inventors have found that by introducing an appropriate amount of acrylic resin and polyurethane resin to prepare the absorbing material, the absorbing material can be given good mechanical properties and chemical resistance, so that the absorbing material can adapt to the continuous industrial production mode (such as the application of absorbing materials in electromagnetic shielding devices, electrostatic discharge protection devices, and electrostatic surge protection devices).
[0010] Preferably, in S1, the viscosity of the slurry is adjusted to 20000-35000 mPa / s. The viscosity of the slurry can be adjusted by introducing a solvent.
[0011] Preferably, the solvent includes at least one of ethyl acetate, sec-butyl acetate, cyclohexanone, NN dimethylformamide, NN dimethylacetamide, butanone, ethyl acetate, butyl acetate, toluene and xylene.
[0012] Preferably, in S2, the drying process includes first stage drying, second stage drying, third stage drying, fourth stage drying, and fifth stage drying; wherein the drying temperature of the first stage drying is 75-85°C, the drying temperature of the second stage drying is 95-105°C, the drying temperature of the third stage drying and the fourth stage drying is 110-125°C, and the drying temperature of the fifth stage drying is 125-135°C. By controlling a reasonable temperature range, it is possible to ensure that the solvent in the coating can not only ensure that the solvent content is kept within a reasonable range, but also avoid the problem of the solvent boiling causing the product surface to be rough and cracked, thereby affecting the antistatic surge performance of the absorbing material.
[0013] Preferably, the drying time of the first drying stage, the second drying stage, the third drying stage, the fourth drying stage, and the fifth drying stage is 2 to 3 minutes respectively. When the drying time is too short, the residual solvent rate in the coating will be high and the humidity will be high. During the high-temperature hot pressing treatment, a large number of bubbles will be generated on the surface of the product (too much solvent residue, and the gas cannot be discharged in time under high temperature and high pressure), and it will affect the normal winding of the product (the layers of the product will stick together). When the drying time is too long, the product will produce a slight burnt smell. If a vulcanizing agent is added to the slurry, it will easily cause the coating to produce semi-vulcanization without the high temperature and high pressure stage, which will reduce the performance of the later products.
[0014] Preferably, in S3, the reaction temperature of the high temperature hot pressing treatment is 160-200° C.; and / or the reaction pressure is 160-200 Kg.
[0015] Preferably, in S3, at least two coating layers are completely overlapped and stacked and then subjected to high-temperature hot pressing treatment.
[0016] Preferably, the raw materials for preparing the absorbing material also include a vulcanizing agent, and the amount of the vulcanizing agent added is 5-8% of the mass of the resin.
[0017] Preferably, the vulcanizing agent includes at least one of sulfur, 4,4'-methylenebis(2-chloroaniline) (MOCA), dicumyl peroxide (DCP), di-tert-butyl peroxide (DTBP), and di-tert-butyl peroxyisopropylbenzene (BIPB).
[0018] Preferably, the raw materials for preparing the absorbing material also include a coupling agent, and the added amount of the coupling agent is 1-5% of the mass of the FeSiAl magnetic powder.
[0019] Preferably, the coupling agent includes a silane coupling agent, a titanate coupling agent, such as at least one of KH550, KH560, vinyl triethoxysilane, etc.
[0020] Preferably, the raw materials for preparing the absorbing material further include an auxiliary agent, and the auxiliary agent includes at least one of a wetting agent and a defoaming agent.
[0021] Preferably, the amount of the wetting agent added is 0.3-0.9% of the mass of the FeSiAl magnetic powder.
[0022] Preferably, the amount of the defoaming agent added is 0.3-0.9% of the mass of the FeSiAl magnetic powder.
[0023] Preferably, the film comprises a PET film.
[0024] Another aspect of the present invention provides an application of the above-mentioned absorbing material in the field of electromagnetic shielding. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 This is a test diagram of the magnetic permeability of the absorbing material provided by the processing group 1A of Example 1 of the present invention; Figure 2 The coating image provided for treatment group 1A of Example 1 of the present invention; Figure 3 This is a picture of the absorbing material product provided by the processing group 8A of Example 1 of the present invention; Figure 4 This is a product picture of the absorbing material provided by the processing group 11A of Example 1 of the present invention; Figure 5 This is a comparison diagram of the absorbing material product provided by treatment group 1A of Example 1 of the present invention and other samples that have experienced powder shedding. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention and the drawings in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0026] Example 1 Treatment Group 1A 1. Raw materials required for preparing absorbing materials The treatment group prepared the absorbing material according to the formula provided in Table 1.
[0027] Table 1. Raw materials required for preparing absorbing materials in treatment group 1A
[0028] 2. Method for preparing microwave absorbing material S1. Mix the raw materials shown in Table 1 to obtain a slurry; S2. coating the slurry on the surface of the film (PET) and performing an orientation treatment to form a coating film; then drying the coating film through the first drying stage, the second drying stage, the third drying stage, the fourth drying stage, and the fifth drying stage to a coating with a solvent content of 20% and a thickness of 80 μm; Among them, the drying temperature of the first drying stage is 80°C, and the drying time is 2.5 minutes; the drying temperature of the second drying stage is 100°C, and the drying time is 3 minutes; the drying temperature of the third drying stage is 110°C, and the drying time is 2 minutes; the drying temperature of the fourth drying stage is 120°C, and the drying time is 3 minutes; the drying temperature of the fifth drying stage is 130°C, and the drying time is 3 minutes.
[0029] S3. Take 13 of the above coatings, overlap and stack them completely, and then perform high-temperature hot pressing treatment to obtain an absorbing material with a thickness of 0.3 mm; wherein the reaction temperature of the high-temperature hot pressing treatment is 190° C. and the reaction pressure is 180 Kg.
[0030] Treatment Group 2A This treatment group prepares the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that when preparing the absorbing material, the thickness of the coating layer of this treatment group is 60 μm, and 18 coating layers are taken for high-temperature hot pressing in S3 to obtain the absorbing material with a thickness of 0.3 mm. Except for the above differences, the operation steps of preparing the absorbing material of this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0031] Treatment Group 3A This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that when preparing the absorbing material, the thickness of the coating layer of this treatment group is 100 μm, and 18 coating layers are taken for high-temperature hot pressing in S3 to obtain the absorbing material with a thickness of 0.3 mm. Except for the above differences, the operation steps of preparing the absorbing material of this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0032] Treatment Group 4A This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the solvent content of the coating layer in this treatment group is 25% when preparing the absorbing material. In addition to the above differences, the operation steps of preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0033] Treatment Group 5A This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the solvent content of the coating layer in this treatment group was 15% when preparing the absorbing material. Except for the above difference, the operation steps of preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0034] Treatment Group 6A This treatment group prepares the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the reaction temperature of the high-temperature hot pressing treatment in the preparation of the absorbing material in this treatment group is 160° C. In addition to the above differences, the operation steps for preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0035] Treatment Group 7A This treatment group prepares the absorbing material by referring to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the reaction temperature of the high temperature hot pressing treatment in the preparation of the absorbing material of this treatment group is 200° C. In addition to the above differences, the operation steps of preparing the absorbing material of this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0036] Treatment Group 8A This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the reaction temperature of the high-temperature hot pressing treatment in the preparation of the absorbing material in this treatment group is 210° C. In addition to the above differences, the operation steps of preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0037] Treatment Group 9A This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the reaction pressure of the high-temperature hot pressing treatment in this treatment group during the preparation of the absorbing material is 160 kg. In addition to the above differences, the operation steps of preparing the absorbing material by this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0038] Treatment Group 10A This treatment group prepares the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the reaction pressure of high temperature hot pressing treatment in this treatment group is 200Kg when preparing the absorbing material. In addition to the above differences, the operation steps of preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0039] Treatment Group 11A This treatment group prepares the absorbing material with reference to the formula and method provided by treatment group 1A of Example 1. The difference from treatment group 1A of Example 1 is that the reaction pressure of high temperature hot pressing treatment in this treatment group is 250Kg when preparing the absorbing material. Except for the above difference, the operation steps of preparing the absorbing material by this treatment group are strictly consistent with those of treatment group 1A of Example 1.
[0040] Comparative Group 1A The comparative group prepared the absorbing material by using the formula and method provided by the treatment group 1A of Example 1. The difference from the treatment group 1A of Example 1 is that when preparing the absorbing material, the thickness of the coating layer of the comparative group is 40 μm, and 26 coating layers are taken for high-temperature hot pressing in S3 to obtain the absorbing material with a thickness of 0.3 mm. Except for the above differences, the operation steps for preparing the absorbing material of the comparative group are strictly consistent with those of the treatment group 1A of Example 1.
[0041] Comparative Group 2A The comparative group prepared the absorbing material by the formula and method provided by the treatment group 1A of Example 1. The difference from the treatment group 1A of Example 1 is that when preparing the absorbing material, the thickness of the coating layer of the comparative group is 150 μm, and 7 coating layers are taken for high-temperature hot pressing in S3 to obtain the absorbing material with a thickness of 0.3 mm. Except for the above differences, the operation steps for preparing the absorbing material of the comparative group are strictly consistent with those of the treatment group 1A of Example 1.
[0042] Comparative group 3A The comparative group prepared the absorbing material by the formula and method provided by the treatment group 1A of Example 1. The difference from the treatment group 1A of Example 1 is that the solvent content of the coating layer in the comparative group was 30% when preparing the absorbing material. Except for the above difference, the operation steps for preparing the absorbing material in the comparative group were strictly consistent with those of the treatment group 1A of Example 1.
[0043] Comparative group 4A The comparative group prepared the absorbing material by the formula and method provided by the treatment group 1A of Example 1. The difference from the treatment group 1A of Example 1 is that the solvent content of the coating layer in the comparative group was 10% when preparing the absorbing material. Except for the above difference, the operation steps for preparing the absorbing material in the comparative group were strictly consistent with those of the treatment group 1A of Example 1.
[0044] Comparative group 5A This comparative group prepared the absorbing material by referring to the formula and method provided by the treatment group 1A of Example 1. The difference from the treatment group 1A of Example 1 is that the reaction temperature of the high temperature hot pressing treatment in the preparation of the absorbing material in this comparative group is 140° C. In addition to the above differences, the operation steps for preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1A of Example 1.
[0045] Comparative group 6A The comparative group prepared the absorbing material by referring to the formula and method provided by the treatment group 1A of Example 1. The difference from the treatment group 1A of Example 1 is that the reaction pressure of the high-temperature hot pressing treatment in the comparative group was 100 Kg when preparing the absorbing material. In addition to the above differences, the operation steps for preparing the absorbing material in the comparative group were strictly consistent with those of the treatment group 1A of Example 1.
[0046] Comparative group 7A This comparative group prepares the absorbing material by referring to the formula and method provided by the treatment group 1A of Example 1. The difference from the treatment group 1A of Example 1 is that the comparative group does not perform the orientation treatment in S2 when preparing the absorbing material. Except for the above difference, the operation steps of preparing the absorbing material by this comparative group are strictly consistent with those of the treatment group 1A of Example 1.
[0047] Test Example 1 1. Test subjects The absorbing materials prepared in each treatment group and comparison group in Example 1.
[0048] 2. Test Method (1) Magnetic permeability: The test object was cut into a ring with an inner diameter of 9 mm and an outer diameter of 16 mm on a mold and tested on an E4991B precision impedance analyzer.
[0049] (2) Density: tested using the Archimedes drainage method.
[0050] (3) Electrostatic test: Use an electrostatic gun (brand Noiseken, model: GT-30RA, host model: ESS-S3011A) to discharge vertically at the VGA port, 180 shots each time, for a total of 7 times. If the test object has the function of resisting electrostatic surge, the motherboard will work normally, otherwise it will freeze. "O" indicates that the test object has passed the electrostatic test (it has anti-static surge performance); "X" indicates that the electrostatic test has not passed (it does not have anti-static surge performance).
[0051] (4) Powder loss: First, take a 3M-610 tape longer than 150 mm. The adhesive surface of the tape should not come into contact with hands or other materials. Stick the tape surface to the surface of the test object, leaving a 20 mm tear-off space. Then use a manual rolling roller (2 kg) to roll back and forth on the test material three times at a nearly uniform speed under its own weight (no bubbles are allowed on the surface of the test object). Make sure the tape surface is fully attached to the test surface and let it stand for 10 seconds. Then, stand up one end of the tape at the tear-off position at a 90-degree right angle to the test surface and tear off the tape at a nearly uniform speed. Observe whether there is powder stuck in the tape. "O" indicates that the test object does not shed powder. "X" indicates that the test object shed powder.
[0052] (5) Appearance: Observe the surface condition of the test object visually, with the naked eye within a distance of 30 cm to 45 cm from the object. "O" indicates that the test object is smooth, free of particles and bubbles at the same time; "X" indicates that the test object is not smooth, has particles or bubbles.
[0053] (6) Solvent content in coating: measured by Ohaus moisture analyzer.
[0054] 3. Test results and analysis The test results of this test example are shown in Table 2. The magnetic permeability of the absorbing material prepared by the treatment group 1A of Example 1 is as follows: Figure 1 As shown (μ' represents magnetic permeability, μ' represents the real part of relative magnetic permeability; μ" represents the imaginary part of relative magnetic permeability; μ' represents the degree of response of the material to the magnetic flux under the action of the magnetic field, and represents the magnetization intensity of the material in the magnetic field; μ" represents the material's ability to absorb or radiate the magnetic field, and represents the loss characteristics of the material)), the coating is as shown Figure 2 shown.
[0055] The test results of treatment groups 1A~3A and comparison groups 1A~2A show that the thickness of the coating not only affects the anti-static surge performance of the absorbing material, but also affects normal production. Specifically, when the coating thickness is too thin, wire drawing will occur between the two scrapers during the coating process, resulting in normal production. Among them, comparison group 1A cannot be formed, and thus the corresponding data cannot be measured.
[0056] It can be seen from the treatment group 1A, the treatment groups 4A~5A and the comparison groups 3A~4A that the solvent content in the coating will also affect the anti-static surge performance, magnetic permeability and appearance of the absorbing material. Specifically, when the solvent content in the coating is too high, the gas cannot be discharged in time during the high-temperature hot pressing treatment, which will produce dense bubbles on the surface of the absorbing material, thereby significantly reducing the anti-static surge performance of the absorbing material; when the solvent content in the coating is too low, the resin component in the coating has initially undergone a cross-linking reaction, and the resin cannot be completely vulcanized during the later high-temperature hot pressing treatment, thereby making the obtained absorbing material soft and rough on the surface.
[0057] It can be seen from the treatment group 1A, the treatment groups 6A~8A and the comparison group 5A that when the reaction temperature in the high temperature hot pressing treatment is too low, the anti-static surge performance of the absorbing material will be affected; when the reaction temperature is too high, bubbles will appear, such as Figure 3 shown.
[0058] It can be seen from the treatment group 1A, treatment groups 9A~11A and comparison group 6A that when the reaction pressure in the high-temperature hot pressing treatment is too low, the anti-static surge performance of the absorbing material will be affected; when the reaction pressure is too high, cracks and bubbles will appear on the surface of the absorbing material, such as Figure 4 As shown. Figure 5 It can be seen that there is no powder falling, slight powder falling and severe powder falling in the absorbing material.
[0059] However, it can be seen from the treatment group 1A and the comparison group 7A that when the orientation treatment is not performed in S2, it is impossible to ensure that the absorbing material has a smooth magnetic circuit, thereby significantly reducing the anti-static surge performance of the absorbing material.
[0060] In addition, the present invention can improve the technical problems that occur when only one stage of drying is performed in the current prior art through multi-stage drying. For example, when the drying temperature of the currently provided one-stage drying is too low, it is easy to cause a high solvent residual rate in the coating, and boiling will still occur during high-temperature hot pressing, resulting in a rough product surface; and when the drying temperature is too high, the solvent in the slurry will boil during the drying process, resulting in a rough surface of the absorbing material, in the form of burst bubbles, thereby affecting the performance of the absorbing material.
[0061] Table 2. Test results of this test case
[0062] Example 2 Treatment Group 1B This treatment group prepared the absorbing material strictly according to the formula and method provided by treatment group 1A of Example 1.
[0063] Treatment Group 2B This treatment group prepared the absorbing material by referring to the formula and method provided by treatment group 1B of Example 2. The difference from treatment group 1B of Example 2 is that when preparing the absorbing material, the FeSiAl magnetic powder used in this treatment group has a D 50 =65 μm. Except for the above differences, the operation steps of preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1B in Example 2.
[0064] Treatment Group 4B This treatment group prepared the absorbing material by referring to the formula and method provided by treatment group 1B of Example 2. The difference from treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in this treatment group when preparing the absorbing material has an AD of 0.40 g / cm 3 Except for the above differences, the operation steps of preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1B in Example 2.
[0065] Treatment Group 5B This treatment group prepared the absorbing material by referring to the formula and method provided by treatment group 1B of Example 2. The difference from treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in this treatment group when preparing the absorbing material has an AD of 0.45 g / cm 3 Except for the above differences, the operation steps of preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1B in Example 2.
[0066] Treatment Group 6B This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1B of Example 2. The difference from treatment group 1B of Example 2 is that the resin used in this treatment group also includes acrylic resin (Mitsubishi, brand MB2952) when preparing the absorbing material. According to the mass ratio, acrylic resin: polyurethane resin = 1:9 (the total mass fraction of the resin remains unchanged). In addition to the above differences, the operation steps for preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1B of Example 2.
[0067] Treatment Group 7B This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1B of Example 2. The difference from treatment group 1B of Example 2 is that the resin used in this treatment group also includes acrylic resin (Yoshida, brand 116) when preparing the absorbing material. According to the mass ratio, acrylic resin: polyurethane resin = 1.5:8.5 (the total mass fraction of the resin remains unchanged). In addition to the above differences, the operation steps for preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1B of Example 2.
[0068] Treatment Group 8B This treatment group prepared the absorbing material with reference to the formula and method provided by treatment group 1B of Example 2. The difference from treatment group 1B of Example 2 is that the resin used in this treatment group also includes acrylic resin (Yoshida brand S-160) when preparing the absorbing material. According to the mass ratio, acrylic resin: polyurethane resin = 4:6 (the total mass fraction of the resin remains unchanged). In addition to the above differences, the operation steps for preparing the absorbing material in this treatment group are strictly consistent with those of treatment group 1B of Example 2.
[0069] Comparative group 1B The comparative group prepared the absorbing material by using the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the magnetic powder used in the preparation of the absorbing material in the comparative group is FeSiCr (D 50 =68μm, AD=0.37g / cm 3 ). Except for the above differences, the operation steps of preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B in Example 2.
[0070] Comparative group 2B The comparative group prepared the absorbing material by using the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the magnetic powder used in the preparation of the absorbing material in the comparative group is FeSiCr (D 50 =65μm, AD=0.40g / cm 3 ). Except for the above differences, the operation steps of preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B in Example 2.
[0071] Comparative group 3B The comparative group prepared the absorbing material by the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in the comparative group in preparing the absorbing material is D 50 =58 μm. Except for the above differences, the operation steps for preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B in Example 2.
[0072] Control group 4B The comparative group prepared the absorbing material by the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in the comparative group in preparing the absorbing material is D 50 =80 μm. Except for the above differences, the operation steps for preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B in Example 2.
[0073] Comparative group 5B The comparative group prepared the absorbing material by the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in the comparative group when preparing the absorbing material has an AD of 0.47 g / cm 3 Except for the above differences, the operation steps for preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B in Example 2.
[0074] Comparative group 6B The comparative group prepared the absorbing material by the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in the comparative group when preparing the absorbing material has an AD of 0.33 g / cm 3 Except for the above differences, the operation steps for preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B in Example 2.
[0075] Comparative group 7B This comparative group prepared the absorbing material by referring to the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in the preparation of the absorbing material in this comparative group is 70% by mass (at the same time, the mass content of the resin in the formula meets 8-13%). In addition to the above differences, the operation steps for preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B of Example 2.
[0076] Comparative group 8B This comparative group prepared the absorbing material by referring to the formula and method provided by the treatment group 1B of Example 2. The difference from the treatment group 1B of Example 2 is that the FeSiAl magnetic powder used in the preparation of the absorbing material in this comparative group is 95% by mass (at the same time, the mass content of the resin in the formula meets 8-13%). In addition to the above differences, the operation steps for preparing the absorbing material in this comparative group are strictly consistent with those of the treatment group 1B of Example 2.
[0077] Test Example 2 1. Test subjects The absorbing materials prepared in each treatment group and comparison group in Example 2.
[0078] 2. Test Method The test was performed according to the method provided in Test Example 2.
[0079] 3. Test results and analysis The test results of this test case are shown in Table 3.
[0080] The test results of the treatment group 1B and the comparison groups 1B-2B show that if other types of soft magnetic powder are replaced, the obtained absorbing material will be difficult to pass the electrostatic test.
[0081] The test results of treatment groups 1B~5B and comparison groups 3B~6B show that the D 50 The bulk density will significantly affect the magnetic permeability and anti-static surge performance of the absorbing material, because the size of the magnetic powder will affect its vulcanization and cross-linking reaction during high-temperature hot pressing.
[0082] It can be seen from treatment groups 1B and 6B~8B that the introduction of unreasonable acrylic resin will reduce the mechanical properties, mechanical properties and applications of the absorbing material. It can be seen from the absorbing material obtained by treatment group 8B that it is easy to become sticky when used at high temperatures, and becomes fragile at low temperatures, which will limit the application conditions; in addition, due to the decrease in adhesion, the coating and film will be delaminated and fall off. Combined with the data of treatment groups 6B~8B, it can be seen that when the mass ratio of acrylic resin to polyurethane resin meets 1~1.5:8.5~9, the polyurethane resin and acrylic resin can form a good combination to obtain a polyurethane-acrylic composite emulsion (PUA), which has the advantages of both polyurethane emulsion and acrylic emulsion, such as excellent mechanical properties and chemical resistance, and is suitable for continuous industrial production. When the mass ratio is not met (such as treatment group 8B), the absorbing material obtained can pass the electrostatic test, but its mechanical properties are too hard and do not meet the standards for actual use.
[0083] It can be seen from the treatment group 1B and the comparison groups 7B~8B that when the magnetic powder content is too low, it is impossible to ensure a smooth magnetic circuit at the moment of static electricity release, resulting in the failure of the obtained absorbing material to pass the electrostatic test; and when the magnetic powder content is too high, there are too few colloid particles (acting as a binder) in the whole material, and the magnetic powder cannot be formed in an orderly and uniform manner, which is not conducive to stable mass production.
[0084] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
[0085] Table 3. Test results of this test case
Claims
1. A wave absorbing material with anti-static surge performance, characterized in that: Calculated by mass percentage, the raw materials for preparing the absorbing material include 85-90% FeSiAl magnetic powder and 8-13% resin; Wherein, the D of the FeSiAl magnetic powder 50 The particle size is 50~70μm, and the bulk density is 0.38~0.45g / cm 3 ; The preparation of the absorbing material comprises the following steps: S1. mixing the raw materials to obtain a slurry; S2. coating the slurry on the surface of the film, and at the same time performing an orientation treatment to form a coating film of the slurry; then drying the coating film to a coating having a solvent content of 15 to 25% and a thickness of 60 to 100 μm by drying; S3. Perform high-temperature hot pressing treatment on the coating, wherein the reaction temperature of the high-temperature hot pressing treatment is not less than 160° C., and the reaction pressure is not less than 160 Kg.
2. The absorbing material according to claim 1, characterized in that: The resin includes a polyurethane resin, and the polyurethane resin includes at least one of a polyether polyurethane resin, a polyester polyurethane resin, a polyimide polyurethane resin, and a polyurea polyurethane resin.
3. The absorbing material according to claim 2, characterized in that: The resin also includes acrylic resin, and the mass ratio of the acrylic resin to the polyurethane resin is 1-1.5:8.5-9.
4. The absorbing material according to claim 1, characterized in that: In S1, the viscosity of the slurry is adjusted to 20000-35000 mpa / s.
5. The absorbing material according to claim 1, characterized in that: In S2, the drying process includes first stage drying, second stage drying, third stage drying, fourth stage drying and fifth stage drying; wherein the drying temperature of the first stage drying is 75-85°C, the drying temperature of the second stage drying is 95-105°C, the drying temperature of the third stage drying and the fourth stage drying is 110-125°C, and the drying temperature of the fifth stage drying is 125-135°C.
6. The absorbing material according to claim 1, characterized in that: In S3, the reaction temperature of the high temperature hot pressing treatment is 160-200° C.; and / or the reaction pressure is 160-200 Kg.
7. The absorbing material according to claim 1, characterized in that: The raw materials for preparing the absorbing material also include a vulcanizing agent, and the added amount of the vulcanizing agent is 5-8% of the mass of the resin.
8. The absorbing material according to claim 7, characterized in that: The vulcanizing agent includes at least one of sulfur, 4,4'-methylenebis(2-chloroaniline), dicumyl peroxide, di-tert-butyl peroxide, and di-tert-butyl peroxycumene.
9. The absorbing material according to claim 1, characterized in that: The raw materials for preparing the absorbing material also include a coupling agent, and the added amount of the coupling agent is 1-5% of the mass of the FeSiAl magnetic powder.
10. Use of the absorbing material according to any one of claims 1 to 9 in an electromagnetic shielding device, an electrostatic discharge protection device, or an electrostatic surge protection device.
Citation Information
Patent Citations
Composite materials comprising conductive nano-fillers
CN103946312A
Electromagnetic wave interference suppression coating
CN110484110A
Manufacturing method of shielding heat-dissipation type wave-absorbing material and adhesive tape structure thereof
CN110845802A
Preparation method of high-temperature-resistant and water-resistant desorption wave magnetic sheet
CN111875949A
Composite wave-absorbing material and preparation method thereof
CN113337248A