Continuous production system and method of battery-grade lithium sulfide

Through continuous production system and microchannel flow reaction technology, the problems of cumbersome preparation process and large pollution of lithium sulfide are solved, and efficient and low-cost battery-grade lithium sulfide production are achieved, which is suitable for industrial applications.

CN118904230APending Publication Date: 2024-11-08SUZHOU TA&A ULTRA CLEAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982387.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the preparation process of lithium sulfide has cumbersome processes, difficult product separation, poor quality, difficult intermittent reaction operation, high energy consumption and large pollution, resulting in high production costs, limiting the practicality of lithium-sulfur batteries and all-solid-state batteries. .

Method used

The continuous production system is adopted, including feeding units, continuous flow reaction units and purification units, and the micro-channel flow reaction device and liquid phase separation tower are used to realize the continuous production of lithium sulfide, through liquid sulfur and ultrafine metal lithium powder The reaction, combined with precision filtration and thin-film evaporation technology, improves the purity and yield of lithium sulfide.

Benefits of technology

The battery-grade purity production of lithium sulfide is achieved, the production cost is reduced, the production efficiency and product quality is improved, the problems of complex processes and large pollution in the existing technology are solved, and it is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904230A_ABST
    Figure CN118904230A_ABST
Patent Text Reader

Abstract

The invention discloses a continuous production system and method for battery-grade lithium sulfide. According to the continuous production device system of the battery-grade lithium sulfide, a conventional reaction kettle is replaced by a micro-channel flow reaction device, meanwhile, continuous production of a battery-grade lithium sulfide product is realized by matching equipment such as a wet grinding machine, a homogenizer, a liquid phase separation tower, a precision filter, a thin film evaporation device and a continuous drying device, the economical efficiency is good, and the production efficiency is high; and the process is safe and controllable. According to the method, metal lithium powder slurry and liquid sulfur are adopted as raw materials, a continuous production device system is matched to prepare the lithium sulfide product, the purity of the prepared lithium sulfide product reaches 99.99%, the water content is smaller than or equal to 15 ppm, the total amount of metal impurities is smaller than 100 ppm, Na is smaller than 30 ppm, Si is smaller than 30 ppm, Ca is smaller than 20 ppm, Mg is smaller than 20 ppm, other impurity metal is smaller than 10 ppm, d50 is smaller than 10 micrometers, d90 is smaller than 20 micrometers, the mass content of free chlorine is smaller than 10 ppm, and the mass content of sulfate radicals is smaller than 20 ppm. And the product application standards of the lithium-sulfur battery positive electrode and the solid sulfide electrolyte are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention particularly relates to a continuous production system and method for battery-grade lithium sulfide, belonging to the technical field of lithium battery positive electrode materials and solid electrolytes. Background Art

[0002] Lithium-sulfur batteries (Li-S) have a high theoretical specific capacity (1675mAh / g) and a high theoretical energy density (≈2600Wh / kg). The raw materials have the advantages of low cost (the cost of sulfur ≈ US$0.1 / kg) and abundant reserves, and are considered to be one of the most promising candidates for the next generation of rechargeable batteries. Lithium sulfide (Li2S) is the positive electrode material of lithium-sulfur batteries. The demand for it will be huge in the future, and all-solid-state lithium-sulfur batteries will require more lithium sulfide products. In addition, lithium sulfide (Li2S), as a key precursor material for the synthesis of sulfur-based solid electrolytes, is the main raw material for the preparation of sulfide solid electrolytes. Sulfide solid electrolytes are the preferred materials for flexible all-solid-state batteries due to their high ionic conductivity, high energy density, low hardness and easy processing, and have huge market prospects in the future.

[0003] At present, the preparation methods of lithium sulfide (Li2S) can be roughly divided into solid phase ball milling method, liquid phase reaction method, high temperature / high pressure method and thermal reduction method.

[0004] The principle of the solid phase ball milling method is to mix elemental sulfur and metallic lithium / lithium hydride under an inert atmosphere and then perform a mechanical ball milling reaction to obtain lithium sulfide. Representative patents include CN108336400A and CN1 12678781A. This method is relatively simple, environmentally friendly, and does not produce any waste liquid; however, it also has disadvantages such as low conversion rate, easy presence of impurity lithium polysulfide, and difficulty in reactor scale-up, and it is impossible to prepare high-purity lithium sulfide products.

[0005] The principle of the liquid phase reaction method is to prepare lithium sulfide by mixing lithium / lithium-containing (organic) compounds and sulfur / sulfur-containing compounds (such as H2S) in a liquid medium. Representative patents include CN106784754B, CN109244383A, CN111517288A and CN108358175A. The liquid medium can be an organic solvent or liquid ammonia, wherein the organic solvent includes aliphatic hydrocarbons, aromatic hydrocarbons or ethers. This method has the advantages of sufficient reaction, easy product purification, no need for high temperature treatment and simple process. The disadvantages are high preparation cost, poor batch stability of intermittent operation, and excessive or difficult removal of Na, Ca ions.

[0006] The principle of the high temperature / high pressure method is to prepare lithium sulfide by reacting lithium / lithium-containing compounds and sulfur / sulfur-containing compounds in liquid or gas phases under the protection of an inert / reducing atmosphere at high temperature / high pressure. Representative patents include CN103764566B and CN108190845A. The advantages of this method are simple process flow, no harmful gas generation, and short preparation process. The disadvantages are low product purity, difficulty in purification, high energy consumption, difficulty in operating condition control, and high requirements for equipment selection.

[0007] The pyrolysis reduction method includes: lithium sulfide precursors (one or more of lithium sulfate, lithium sulfite, lithium bisulfate, lithium dithionate) react with relevant reducing agents at high temperature for preparation. Representative patents include CN106299261B, CN108987713A, CN109360953A, CN110112390A and CN110212180A. The core step of this method is that lithium salts (such as lithium sulfate) are reduced by carbon or carbon-containing compounds (such as sugar) at high temperature. Its advantages are that raw materials are easily available, the operation is simple, and the crude products in the intermediate steps are convenient for storage and transportation. It is especially suitable for the one-step preparation of lithium sulfide / carbon composite materials. Its disadvantages are high temperature and high energy and the emission of greenhouse gas carbon dioxide.

[0008] In summary, the processes for preparing lithium sulfide in the prior art have defects such as complicated processes, difficult product separation, poor quality, difficult intermittent reaction operation, high energy consumption and pollution, and high manufacturing cost. This has caused the preparation cost of lithium sulfide to remain high, becoming an important constraint on the practical application of lithium-sulfur batteries and all-solid-state batteries based on sulfide electrolytes. Therefore, it is an urgent problem for those skilled in the art to develop a process system and production method for the continuous production of lithium sulfide with low cost, rapid and efficient, green and environmentally friendly, safe and stable, and easy large-scale industrialization. Summary of the invention

[0009] The main purpose of the present invention is to provide a continuous production system and method for battery-grade lithium sulfide, so as to solve the industry problems in the prior art that the lithium sulfide preparation process is complicated, the production cost is high, the quality difference between batches of intermittent operations is large, the product is easily deteriorated when exposed to water, resulting in high impurity content and difficult purification; the purity of lithium sulfide produced by the continuous production device system and production method provided by the present invention reaches the battery-grade application level, thereby overcoming the shortcomings of the prior art.

[0010] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0011] A first aspect of an embodiment of the present invention provides a continuous production system for battery-grade lithium sulfide, comprising: a feeding unit, a continuous flow reaction unit, and a purification unit connected in series;

[0012] The feeding unit includes a liquid sulfur feeding module, a metal lithium slurry feeding module and an organic solvent A feeding module which are independently arranged, wherein the liquid sulfur feeding module is used to convey liquid sulfur, the metal lithium slurry feeding module is used to mix metal lithium and organic solvent B to form metal lithium slurry and convey the metal lithium slurry, and the organic solvent A feeding module is used to convey organic solvent A;

[0013] The continuous flow reaction unit comprises m microchannel flow reaction devices connected in series, the first microchannel flow reaction device is connected to the liquid sulfur feeding module and the metal lithium slurry feeding module, and can be used for the liquid sulfur and the metal lithium slurry to mix and react to form a first mixed system containing lithium sulfide, and the mth microchannel flow reaction device is connected to the organic solvent A feeding module, and can be used for the first mixed system to mix with the organic solvent A to form a second mixed system;

[0014] The purification unit includes a liquid phase separation module and a desolventizing module connected in series. The liquid phase separation module is connected to the mth microchannel flow reaction device and is used to phase separate the second mixed system and obtain a third mixed system and an organic solvent B. The desolventizing module is at least used to separate the third mixed system into a fourth mixed system and an organic solvent A. The lithium sulfide contained in the fourth mixed system is battery-grade lithium sulfide, and m≥3.

[0015] In a more specific embodiment, the liquid sulfur feed module includes a liquid sulfur storage device and a heating device connected in sequence, and the heating device is directly connected to the first microchannel flow reaction device.

[0016] Furthermore, a liquid sulfur delivery pump is provided between the liquid sulfur storage device and the heating device.

[0017] Furthermore, a first check valve, a first flow meter and a first stop valve are sequentially arranged on the pipeline connecting the liquid sulfur storage device and the heating device.

[0018] In a more specific embodiment, the metallic lithium slurry feeding module includes a grinding device, an organic solvent B storage device, a homogenizer device and a first preheating device, the grinding device and the organic solvent B storage device are connected to the homogenizer device, the homogenizer device is connected to the first preheating device, and the first preheating device is directly connected to the first microchannel flow reaction device.

[0019] Furthermore, an inertial protection vibration feeding funnel is arranged between the grinding device and the homogenizer device.

[0020] Furthermore, the grinding device may be a wet grinding device, which includes a wet ball mill and a positive pressure closed vibrating hopper with a weighing module.

[0021] Furthermore, a metal lithium slurry delivery pump is also provided on the connecting pipeline between the homogenizer device and the first preheating device.

[0022] Furthermore, a second check valve and a second flow meter are sequentially arranged on the connecting pipeline between the metal lithium slurry delivery pump and the first preheating device.

[0023] In a more specific embodiment, the organic solvent A feeding module comprises an organic solvent A storage device and a second preheating device connected in sequence, and the second preheating device is directly connected to the mth microchannel flow reaction device.

[0024] Furthermore, an organic solvent A delivery pump, a third check valve, and a third flow meter are sequentially arranged on the connecting pipeline between the organic solvent A storage device and the second preheating device.

[0025] Furthermore, the material of the microchannel flow reaction device includes silicon carbide (SiC), stainless steel, glass and the like.

[0026] Furthermore, the channel diameter of the microchannel flow reaction device is 1 mm to 10 mm, for example, it can be 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm or 4.5 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Furthermore, the channel structure of the microchannel flow reaction device includes any one of a heart shape, a zigzag shape, a thorn shape, a baffle shape or a Y shape, or a combination of at least two of them, but is not limited thereto.

[0028] It is worth noting that the sandwich structure design of the microchannel flow reaction device adopted in the present invention improves the heat exchange efficiency by about 1000 times compared with the kettle reactor, and the channel design of its internal heart-shaped and baffle structures improves the mass transfer efficiency by about 100 times compared with the kettle mechanical stirring. The efficient mass transfer and heat transfer completed in the microchannel can realize the rapid, high-selectivity and high-yield preparation of lithium sulfide. It should be noted that the microchannel flow reaction device adopted in the present invention is known in the art and can be obtained commercially, and its specific structure is not limited here.

[0029] Furthermore, the liquid holding volume of the microchannel flow reaction device is 7 mL to 70 mL, for example, 7 mL, 10 mL, 15 mL, 20 mL, 25 mL, 30 mL, 35 mL, 40 mL, 45 mL, 50 mL, 60 mL or 70 mL, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] In a more specific embodiment, the liquid phase separation module includes p liquid phase separation towers connected in sequence, the first liquid phase separation tower is connected to the mth microchannel flow reaction device, the top of the pth liquid phase separation tower is connected to the top of the p-1th liquid phase separation tower through an overflow pipe, and the bottoms of the p liquid phase separation towers are independently connected to the desolventizing module, p≥2.

[0031] Furthermore, a back pressure valve is provided on the connecting pipeline between the first liquid phase separation tower and the mth microchannel flow reaction device.

[0032] Furthermore, the liquid phase separation tower is provided with a sight glass and / or an interface level meter.

[0033] As a preferred embodiment of the present invention, the length-to-diameter ratio of the liquid phase-separation tower is (30-3):1; for example, it can be 30:1, 25:1, 20:1, 15:1, 10:1, 5:1 or 3:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Furthermore, the pth liquid phase separation tower is also connected to the organic solvent B recovery device.

[0035] It should be noted that, in the present invention, the function of the liquid phase separation tower is to separate the two immiscible liquids through the joint control of the level meter and the flow meter.

[0036] Furthermore, the desolventizing module comprises at least one filtering device and at least one thin film evaporating device which are connected in sequence, and the p liquid phase separation towers are connected to the filtering device.

[0037] Furthermore, at least one filtering device includes a first filtering device and a second filtering device connected in sequence, and the pore size of the first filtering device is larger than the pore size of the second filtering device.

[0038] Further, the first filtering device includes at least two groups of filters connected in parallel, for example, it can be 2 groups, 3 groups, 4 groups, 5 groups, 6 groups, 7 groups, 8 groups, 9 groups or 10 groups, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Further, the second filtering device includes at least two groups of filters connected in parallel, for example, it can be 2 groups, 3 groups, 4 groups, 5 groups, 6 groups, 7 groups, 8 groups, 9 groups or 10 groups, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Furthermore, the first filtering device and the second filtering device are both precision filtering devices.

[0041] Furthermore, the pore size of the first filter device (i.e., the pore size of the filter element adopted by the first filter device) includes any one of 50μm, 200μm or 500μm, or a combination of at least two of them, wherein the typical combinations include but are not limited to: a combination of 50μm and 200μm, a combination of 200μm and 500μm, or a combination of 50μm, 200μm and 500μm, etc.

[0042] Further, the pore size of the second filter device (i.e., the pore size of the filter element used in the first filter device) includes any one of 0.45 μm, 1 μm, or 10 μm, or a combination of at least two of them. The typical combinations include but are not limited to: a combination of 0.45 μm and 1 μm, a combination of 1 μm and 10 μm, or a combination of 0.45 μm, 1 μm, and 10 μm, etc.

[0043] Further, the filter element of the first filter device and the second filter device is made of any one or a combination of at least two of stainless steel 304, stainless steel 316L, ceramic, polytetrafluoroethylene (PTFE), expanded polytetrafluoroethylene (EPTF), polyethylene (HDPE), polyvinylidene fluoride (PVDF) or silicon carbide, wherein typical combinations include but are not limited to: a combination of ceramic and PTFE, a combination of EPTF and PTFE, a combination of HDPE and PVDF, or a combination of SiC and PVDF, etc.

[0044] Furthermore, the desolventizing module also includes an organic solvent A recovery device, and the organic solvent A recovery device is connected to the thin film evaporation device.

[0045] Furthermore, the thin film evaporation device includes at least one vertical wiped film evaporator and / or at least one horizontal wiped film evaporator.

[0046] That is, the thin film evaporation device may include one or more vertical wiped film evaporators, and the multiple vertical wiped film evaporators may be connected in series, or the thin film evaporation device may include one or more horizontal wiped film evaporators, and the multiple horizontal wiped film evaporators may be connected in series, or the thin film evaporation device may include one or more vertical wiped film evaporators and one or more horizontal wiped film evaporators connected in series.

[0047] In a more specific embodiment, the purification unit also includes a post-processing module, which is connected to the desolventizing module, and the post-processing module includes a drying device, a crushing device, an air conveying device, a vibration screening device and an inert environment packaging device connected in sequence.

[0048] A second aspect of an embodiment of the present invention provides a method for continuously producing battery-grade lithium sulfide, comprising:

[0049] Providing a continuous production system for the battery-grade lithium sulfide;

[0050] Liquid sulfur is transported to the first microchannel flow reaction device via a liquid sulfur feeding module, metal lithium and organic solvent B are mixed to form metal lithium slurry via a metal lithium slurry feeding module, and the metal lithium slurry is transported to the first microchannel flow reaction device, and the liquid sulfur and the metal lithium slurry are mixed and reacted in the first microchannel flow reaction device to form a first mixed system containing lithium sulfide; organic solvent A is transported to the mth microchannel flow reaction device via an organic solvent A feeding module, and the first mixed system is sequentially processed through the second microchannel flow reaction device ... the m-1th microchannel flow reaction device, and then mixed with organic solvent A in the mth microchannel flow reaction device to form a second mixed system;

[0051] The second mixed system is transported to a liquid phase separation module for phase separation to obtain a third mixed system and an organic solvent B, and then the third mixed system is transported to a desolventizing module for desolventizing treatment to obtain a fourth mixed system and an organic solvent A, wherein the lithium sulfide contained in the fourth mixed system is battery-grade lithium sulfide.

[0052] Furthermore, the first mixed system is crude lithium sulfide, the second mixed system is a mixture formed by mixing crude lithium sulfide and organic solvent A; the third mixed system is a lithium sulfide solution, and the fourth mixed system is battery-grade lithium sulfide formed after impurity removal and obtained after evaporation.

[0053] It should be noted that organic solvent A is a good solvent for lithium sulfide, and the boiling point of organic solvent A is lower than that of organic solvent B. If metal lithium, organic solvent B, and organic solvent A are directly mixed together, the organic solvent A with a lower boiling point will vaporize at the process temperature, increase the pressure of the reaction module, increase the requirements for equipment and sealing, and there are safety risks. At the same time, the flow rate of the vaporized gas is faster than that of the liquid. The added organic solvent A does not dissolve according to the set ratio, which increases the risk of material precipitation in the microchannel flow reaction device. Once blocked, it will cause certain accidents; in addition, the direct mixing of metal lithium, organic solvent B, and organic solvent A will also dilute the concentration of the reaction substrate, reduce the reaction rate, and prolong the reaction time, thereby causing a decrease in conversion rate, increasing the difficulty of subsequent purification, and causing a series of problems. If the method of adding reaction modules is adopted, investment will be increased and the reaction pressure drop will be increased, which will continue to cause a series of safety and process problems.

[0054] In a more specific embodiment, the method for continuously producing battery-grade lithium sulfide specifically comprises:

[0055] The liquid sulfur is transported to the first microchannel flow reaction device after being kept warm by a heating device;

[0056] The lithium metal powder obtained by grinding the lithium metal by the grinding device is conveyed to the homogenizer device, and at the same time, the organic solvent B is conveyed to the homogenizer device for slurrying to obtain the lithium metal slurry, and the lithium metal slurry is preheated by the first preheating device and then conveyed to the first microchannel flow reaction device;

[0057] The organic solvent A is preheated by the second preheating device and then transported to the mth microchannel flow reaction device.

[0058] The present invention uses organic solvent B and metal lithium powder to preform metal lithium slurry, and then reacts the metal lithium slurry with high-purity liquid sulfur to prepare lithium sulfide. Ultrafine metal lithium powder (particle size ≤ 500 μm) with a purity of more than 99.9%, high-purity liquid sulfur (purity ≥ 99.95%), ultra-dry organic solvent B (water content < 50 ppm), and inert environmental protection are used to avoid contact with water during the preparation of lithium sulfide, and the purity of the obtained lithium sulfide reaches 99.99%, which meets the battery-grade application level.

[0059] Furthermore, the temperature of the heating device is 118°C to 128°C, for example, it can be 118°C, 120°C, 123°C or 125°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] Furthermore, the particle size of the metallic lithium powder obtained after grinding is ≤500μm, for example, it can be 10μm, 20μm, 50μm, 100μm, 200μm, 300μm, 400μm or 500μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] Furthermore, the temperature of the first preheating device is 115°C to 125°C, for example, it can be 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, 123°C or 125°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] Further, the temperature of the second preheating device is 70°C to 115°C, for example, it can be 70°C, 80°C, 100°C or 115°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] It should be noted that the melting point of sulfur is 119°C, and it will solidify below 119°C. If the lithium metal slurry is directly introduced into the reaction device without preheating and mixed with liquid sulfur, the liquid sulfur will solidify and block the microchannel, thus preventing the subsequent reaction from continuing.

[0064] Further, the organic solvent A includes any one of methanol, ethanol, isopropanol, n-butanol, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid or trifluoroacetic acid, or a combination of at least two thereof, but is not limited thereto, wherein exemplary combinations include a combination of ethanol and isopropanol, a combination of isopropanol and hexanoic acid, or a combination of n-butanol and trifluoroacetic acid, etc.

[0065] Further, the organic solvent B includes any one or a combination of at least two of methyl silicone oil, turpentine, ethylene glycol butyl ether, diphenyl ether, n-hexane, cyclohexane, n-dodecane, n-octadecane, 1-fluorohexane, toluene, xylene, cyclohexanone, N-methylpyrrolidone, amyl acetate, and ethyl benzoate, but is not limited thereto. Exemplary combinations include a combination of n-dodecane and N-methylpyrrolidone, a combination of diphenyl ether and n-octadecane, or a combination of xylene and cyclohexane, etc.

[0066] Furthermore, the water content of the organic solvent A is less than 50 ppm, that is, the organic solvent A is an ultra-dry solvent.

[0067] Furthermore, the water content of the organic solvent B is less than 50 ppm, that is, the organic solvent B is an ultra-dry solvent.

[0068] It is worth noting that the organic solvent B used in the reaction is removed from the reaction system in time through a liquid phase separation tower, no new solvent is introduced, and the reaction by-products are few. The organic solvent A used in the reaction is removed from the reaction system through a desolventizing module thin film evaporator, no new solvent is introduced, and the reaction by-products are few.

[0069] Further, the mass concentration of the metal lithium in the metal lithium slurry does not exceed 25%. Further, the mass concentration of the metal lithium in the metal lithium slurry is 5% to 25%, for example, it can be 5%, 8%, 10%, 15%, 20% or 25%, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. If the concentration of metal lithium is too low, the equipment utilization rate is too low. If the concentration of metal lithium is too high, the concentration of lithium sulfide generated is too high, and lithium sulfide will precipitate in solid form during the reaction stage. The reaction state is that the metal Li slurry becomes lithium sulfide slurry. If the concentration is too high, the channel will be blocked, causing the subsequent reaction to be unable to continue.

[0070] Furthermore, the purity of the metallic lithium is ≥99.9%, the particle size of the metallic lithium powder obtained after grinding is ≤500 μm, and the mass content of Na in the metallic lithium is ≤200 ppm, the mass content of Ca is ≤200 ppm, the mass content of free chlorine is <60 ppm, and the mass content of nitrogen is ≤200 ppm.

[0071] Furthermore, the purity of the liquid sulfur is ≥99.95%, for example, it can be 99.95%, 99.96%, 99.97%, 99.98% or 99.99%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0072] Furthermore, the mass content of water in the liquid sulfur is ≤500ppm, the mass content of acidity (calculated as sulfuric acid) is ≤30ppm, the mass content of Fe is ≤30ppm, and the mass content of As is ≤1ppm.

[0073] Furthermore, the Fe metal mass content in the liquid sulfur is ≤30 ppm, for example, it can be 25 ppm, 20 ppm, 15 ppm, 10 ppm, 5 ppm or 1 ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0074] In the present invention, except for Fe metal, the mass content of other metal ion impurities is less than 1 ppm.

[0075] Preferably, the moisture content of the liquid sulfur is ≤500ppm, for example, it can be 500ppm, 400ppm, 300ppm, 200ppm, 100ppm or 50ppm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0076] Preferably, the acidity of the liquid sulfur is ≤30 ppm, for example, it may be 30 ppm, 25 ppm, 20 ppm, 15 ppm or 10 ppm, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0077] In the present invention, the acidity of the liquid bis(fluorosulfonyl)imide salt is measured in terms of H2SO4.

[0078] Furthermore, the molar ratio of the liquid sulfur to the metallic lithium is (0.80-1.20):2, for example, it can be 0.80:2, 0.85:2, 0.90:2, 0.95:2, 1.00:2, 1.05:2, 1.10:2, 1.15:2, or 1.20:2, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. If the ratio of liquid sulfur to the metallic lithium is too small, too much metallic lithium will remain, and the pressure of subsequent filtration and recovery will be relatively large. In addition, metallic lithium is relatively active, and excessive metallic lithium will also cause active side reactions, such as an increase in the amount of LiOH generated by reacting with trace amounts of water in the solvent, affecting the purity of the final product. If the ratio of liquid sulfur to the metallic lithium is too large, there will be more sulfur remaining after the reaction is accepted. After adding solvent A, more sulfur will precipitate, and the reactor will be at risk of clogging.

[0079] Furthermore, the pressure conditions in the m microchannel flow reaction devices are the same, and the temperature conditions decrease gradually from the first microchannel flow reaction device to the mth microchannel flow reaction device.

[0080] It should be noted that the same pressure conditions mean that the pressure adjusted by the back pressure valve at the outlet of the last microchannel flow reactor is the same. In fact, the same pressure drop exists inside the microchannel flow reactor. The pressure is highest at the inlet of the microchannel flow reactor and lowest at the outlet.

[0081] Furthermore, the reduction of temperature gradient is conducive to controlling the occurrence of side reactions and reducing impurities. The high temperature of the first microchannel flow reactor can ensure that the material is in a liquid state (higher than the melting point of sulfur), giving the reaction sufficient activation energy. Since the reaction is exothermic, the heat can be removed by using the microchannel flow reactor's characteristic of rapid heat removal, and the temperature can be controlled by gradient to reduce side reactions.

[0082] Furthermore, the temperature in the first microchannel flow reaction device is 120°C to 130°C, and the temperature in the mth microchannel flow reaction device is 95°C to 115°C.

[0083] It should be noted that the organic solvent A is directly introduced into the mth microchannel flow reaction device. Since the boiling point of the organic solvent A is not high, it is generally lower than or equal to the process temperature. Therefore, exceeding the set temperature will cause the organic solvent A to vaporize, the pressure to be too high, the dissolution to be insufficient, and the high viscosity of the material to block the back pressure valve.

[0084] In a more typical embodiment, when m=3, the temperature in the first microchannel flow reaction device is 120℃~130℃, for example, it can be 120℃, 122℃, 125℃, 126℃, 128℃, 129℃ or 130℃, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; the temperature in the second microchannel flow reaction device is 115℃~125℃, for example, it can be 115℃, 116℃, 118℃, 120℃, 121℃, 122℃, 123℃, 124℃ or 125℃, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; the temperature in the third microchannel flow reaction device is 95℃~115℃, for example, it can be 95℃, 98℃, 100℃, 105℃, 110℃ or 115℃, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0085] Furthermore, the pressure in the m microchannel flow reaction devices is 0.25MpaG to 1.25MpaG, for example, it can be 0.3MpaG, 0.5MpaG, 0.7MpaG, 0.9MpaG, 1MpaG or 1.1MpaG, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0086] Further, the total residence time of the material in the m microchannel flow reaction devices is 15s to 150s, for example, it can be 15s, 20s, 40s, 60s, 80s, 100s, 120s, 130s, 140s or 150s, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable. It should be noted that the microchannel flow reaction device has a limited liquid holding volume, a high cost, a small channel, and a greater pressure drop with more modules, so the residence time of the material in each microchannel flow reaction device will not be too long. The microchannel is suitable for fast reactions but not for slow reactions. If the residence time is too short, the material reaction is incomplete, there are too many impurities, and it is difficult to separate.

[0087] Furthermore, the residence time of the material in each microchannel flow reaction device is the same.

[0088] It is worth noting that the present invention maintains the pressure of m microchannel flow reaction devices connected in series at 0.25MPaG~1.25MPaG, under the condition of reaction temperature of 95℃~130℃, total reaction residence time of 3min~15min, and the single-pass conversion rate can reach 95.0%~99.9%.

[0089] Furthermore, the operating temperature of the liquid phase-separation module is 50°C to 115°C, that is, the operating temperature of the liquid phase-separation tower contained in the liquid phase-separation module is 50°C to 115°C, for example, it can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 105°C, 110°C or 115°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0090] Furthermore, the internal working pressure of the liquid phase separation tower includes normal pressure or slightly positive pressure.

[0091] Furthermore, the desolventizing module includes at least one filtering device and at least one thin film evaporation device connected in sequence, and the third mixed system is transported to the filtering device and the thin film evaporation device in sequence for treatment, so as to separate the third mixed system to obtain a fourth mixed system and organic solvent A, and the thin film evaporation device includes a vertical scraped film evaporator and / or a horizontal scraped film evaporator.

[0092] Further, the operating temperature of the vertical scraped film evaporator is 50°C to 120°C, for example, it can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 115°C or 120°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable. The working pressure is 5kPaA to 15kPaA, for example, it can be 7kPaA, 9kPaA, 10kPaA, 12kPaA or 14kPaA, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable. The residence time of the material in the vertical scraped film evaporator is 15 to 40 min, for example, it can be 15 min, 20 min, 30 min, 35 min or 40 min, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0093] Further, the operating temperature of the horizontal wiped film evaporator is 50°C to 150°C, for example, it can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. The working pressure is 200PaA to 1200PaA, for example, it can be 200PaA, 300PaA, 500PaA, 600PaA, 700PaA , 800PaA, 900PaA, 1000PaA or 1200PaA, etc., but not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. The residence time of the material in the horizontal wiped film evaporator is 40min to 120min, for example, it can be 40min, 60min, 80min, 90min, 100min, 110min or 120min, etc., but not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0094] Furthermore, the purity of the battery-grade lithium sulfide reaches 99.99%; the total mass content of impurity metals in the battery-grade lithium sulfide is less than 100ppm, wherein the impurity metals include Na<30ppm, Si<30ppm, Ca<20ppm, Mg<20ppm, and other impurity metals are all less than 10ppm; the particle size d50 of the battery-grade lithium sulfide is less than 10μm, and d90 is less than 20μm; the moisture content of the battery-grade lithium sulfide is ≤15ppm; the mass content of free chlorine in the battery-grade lithium sulfide is less than 10ppm, and the mass content of sulfate is less than 20ppm.

[0095] In the present invention, the organic solvent B obtained after separation by the liquid phase separation module is recovered to the organic solvent B recovery device; the organic solvent A concentrated by the vertical scraped film evaporator and the horizontal scraped film evaporator is recovered to the organic solvent A recovery device.

[0096] It is worth noting that the present invention adopts three sets of purification devices connected in series, namely, a liquid phase separation tower + precision filtration + thin film evaporation, to timely discharge the used organic solvent A, organic solvent B and excess raw material S and impurities from the system, thereby reducing the risk of material decomposition and improving the selectivity of the reaction. The continuously recovered organic solvent is promptly returned to the premixing device and the feeding unit for continued use, thereby improving the utilization rate of the organic solvent, shortening the reaction time, and reducing the occurrence of side reactions.

[0097] In a more specific embodiment, the method for continuously producing battery-grade lithium sulfide also includes: conveying the fourth mixed system to a drying device, a crushing device, a pneumatic device, a vibrating screening device and an inert environment packaging device in sequence for post-processing, and the post-processing includes drying / drying treatment, crushing treatment, screening treatment, etc.

[0098] Furthermore, the drying temperature of the drying device is 300°C to 700°C, for example, 300°C, 400°C, 500°C, 600°C or 700°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0099] Furthermore, the residence time of the material in the drying device is 2h to 6h, that is, the drying time is 2h to 6h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0100] Furthermore, the material crushing processing time in the crushing device is 2h to 6h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0101] The lithium sulfide product prepared by the invention meets the application standards of positive electrode materials and solid electrolyte materials in batteries.

[0102] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0103] Compared with the prior art, the advantages of the present invention include:

[0104] (1) The continuous production device system of the present invention adopts a microchannel flow reaction device to replace a conventional reactor, and cooperates with a liquid phase separation tower device, a precision filter device, a thin film evaporation device, a continuous drying device, a drying device and other equipment to realize the continuous production of lithium sulfide, with good economy, high production efficiency, and a safe and controllable process;

[0105] (2) The continuous production device system of the present invention further adopts a purification method of liquid-liquid phase separation, precision filtration, and thin film evaporation in series, which can remove impurities more thoroughly, and the prepared Li2S has fewer impurities. After continuous drying and crushing, it is packaged in an inert environment, and the product quality is high; and after drying, a secondary crushing and air delivery method is adopted to reduce the agglomeration phenomenon of the product, and the particle size distribution uniformity of the product is improved by cooperating with a vibration screening device;

[0106] (3) The method of the present invention uses liquid sulfur and ultrafine lithium metal powder slurry as raw materials, and the lithium sulfide yield obtained by the continuous production device system is high, and the product yield can reach 99%; the product purity is high, the total mass content of impurity metals is less than 100ppm, among which Na is less than 30ppm, Si is less than 30ppm, Ca is less than 20ppm, Mg is less than 20ppm, and other impurity metals are less than 10ppm; moisture is ≤15ppm; particle size d50 is less than 10μm, d90 is less than 20μm; the mass content of free chlorine is less than 10ppm, and the mass content of sulfate is less than 20ppm. It meets the application standards in electrolyte;

[0107] (4) The method of the present invention uses organic solvent B as the mobile phase for grinding, homogenizing and diluting metallic lithium, and after continuous reaction, phase separation and removal are performed with the organic solvent A solution without introducing new solvents. There are few reaction by-products, which makes lithium sulfide highly selective and fluid, with stable product quality between batches, easy purification and high purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0108] Figure 1 It is a schematic diagram of the structure of a continuous production device system of lithium sulfide provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0109] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention is further illustrated by specific implementation methods below. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Unless otherwise specified, the functional devices used in the embodiments of the present invention are all known in the art and can be obtained commercially. The specific structure and model are not limited here.

[0110] The microchannel flow reaction devices in the following examples and comparative examples were purchased from Corning Microchannel Reactor Technology Co., Ltd. (G1). The first microchannel flow reaction device, the second microchannel flow reaction device, and the third microchannel flow reaction device all include a reaction module group consisting of two reaction modules (the channel structure is heart-shaped) connected in series.

[0111] Example 1

[0112] A continuous production device system of lithium sulfide, such as Figure 1 As shown, the continuous production device system includes a feeding unit, a continuous flow reaction unit and a purification unit connected in sequence;

[0113] The continuous flow reaction unit comprises a first microchannel flow reaction device 7, a second microchannel flow reaction device 8 and a third microchannel flow reaction device 9 which are connected in series in sequence; the first microchannel flow reaction device 7 is made of glass, has a channel diameter of 1 mm to 1.2 mm, and a liquid holding volume of 24 mL; the second microchannel flow reaction device 8 is made of glass, has a channel diameter of 1 mm to 1.2 mm, and a liquid holding volume of 24 mL; the third microchannel flow reaction device 9 is made of glass, has a channel diameter of 1 mm to 1.2 mm, and a liquid holding volume of 1 to 6 mL;

[0114] The feeding unit includes a liquid sulfur feeding module, a metal lithium slurry feeding module and an organic solvent A feeding module connected in parallel; the liquid sulfur feeding module and the metal lithium feeding unit are independently connected to the first microchannel flow reaction device 7; the organic solvent A feeding module is independently connected to the third microchannel flow reaction device 9;

[0115] The liquid sulfur feeding module includes a liquid sulfur storage device and a heating device 6 connected in sequence; a liquid sulfur delivery pump 5 is arranged between the liquid sulfur storage device and the heating device 6; the heating device 6 is connected to the first microchannel flow reaction device 7, and a first check valve 31, a first flow meter 32 and a first stop valve 37 are arranged in sequence on the pipeline connecting the liquid sulfur delivery pump 5 and the heating device 6;

[0116] The metal lithium slurry feeding module comprises a metal lithium wet grinding device 1, an organic solvent B storage device, a homogenizer device 2 and a first preheating device 4 which are connected in sequence; a metal lithium slurry delivery pump 3 is arranged between the homogenizer device 2 and the first preheating device 4; the first preheating device 4 is connected to the first microchannel flow reaction device 7, and a second check valve 33 and a second flow meter 34 are arranged in sequence on the pipeline connecting the metal lithium slurry delivery pump 3 and the first preheating device 4;

[0117] The organic solvent A feeding module comprises an organic solvent A storage tank, an organic solvent A delivery pump 10 and a second preheating device 28 which are connected in sequence; the second preheating device 28 is connected to the third microchannel flow reaction device 9, and a third check valve 35 and a third flow meter 36 are sequentially arranged on the pipeline connecting the organic solvent A delivery pump 10 and the second preheating device 28;

[0118] The purification unit includes a first liquid phase separation tower 11, a second liquid phase separation tower 12, a first precision filter 13, a first lithium sulfide solution storage tank 15, a second precision filter 17, a second lithium sulfide solution storage tank 18, a vertical scraped film evaporator 20, a horizontal scraped film evaporator 21, a continuous drying device 23, a crushing device 24, an air delivery device 25, a vibration screening device 26, and an inert environment packaging device 27, which are connected in sequence;

[0119] A first lithium sulfide solution delivery pump 16 is connected between the first lithium sulfide solution storage tank 15 and the second precision filter 17; a second lithium sulfide solution delivery pump 19 is connected between the second lithium sulfide solution storage tank 18 and the vertical thin film evaporator 20; the top of the second liquid phase separation tower 12 is connected to the organic solvent B recovery tank 14; the gas phase outlet of the vertical scraped film evaporator 20 is connected to the organic solvent A recovery tank; the gas phase outlet of the horizontal scraped film evaporator 21 is connected to the organic solvent A recovery tank; the third microchannel flow reaction device 9 is connected to the first liquid phase separation tower 11, and a back pressure valve 38 is provided on the connected pipeline;

[0120] The filter element of the first precision filter 13 is made of ceramic and has a pore size of 300 μm; the filter element of the second precision filter 17 is a ceramic filter element with pore sizes of 1 μm and 0.45 μm connected in series.

[0121] Example 2

[0122] The present embodiment provides a lithium sulfide continuous production device system, which has the same conditions as those of the embodiment 1 except that the horizontal wiped film evaporator 21 is not provided.

[0123] Comparative Example 1

[0124] This comparative example provides a continuous production device system for lithium sulfide. Except that the continuous flow reaction unit is only provided with a first microchannel flow reaction device 7 and a third microchannel flow reaction device 9, and the second microchannel flow reaction device 8 is not provided, other conditions are the same as those in Example 1.

[0125] Preparation Example 1

[0126] This preparation example provides a method for continuously producing lithium sulfide, which is implemented using the continuous production device system provided in Example 1, wherein the device in the continuous production device system is replaced with high-purity nitrogen for 1 hour to form an inert atmosphere, and the method comprises the following steps:

[0127] (1) After the high-quality liquid sulfur is maintained at 118° C. by the heating device 6, the first check valve and the first flow meter are regulated to pump the sulfur into the first microchannel flow reaction device 7 at a flow rate of 10 g / min;

[0128] The purity of high-quality liquid sulfur is greater than 99.95%, and the mass content of Fe is 28ppm, the mass content of water is 500ppm, and the acidity is 20.5ppm (calculated as sulfuric acid);

[0129] (2) 325 g of Li was ground in a lithium metal wet grinding device 1 at room temperature for 8 h until the particle size was less than 50 μm, and then the wet-ground Li powder was transported to a homogenizer device 2 through a vibrating hopper under the lithium metal wet grinding device 1, and 6170 g of n-dodecane was added to the homogenizer device 2 at room temperature. The mixture was stirred and mixed in the homogenizer device 2 for 15 min to obtain 6495 g of lithium metal slurry; the obtained lithium metal slurry was then preheated to 115° C. by a first preheating device 4, and then the second check valve 33 and the second flowmeter 34 were regulated to pump the mixture into the first microchannel flow reaction device 7 at a flow rate of 108 g / min;

[0130] Wherein, the molar ratio of the liquid sulfur in step (1) to the metallic lithium in step (2) is 0.8:2;

[0131] (3) After the trifluoroacetic acid is maintained at 70° C. by the second preheating device 28 , the third check valve 35 and the third flow meter 36 are regulated to pump the trifluoroacetic acid into the first microchannel flow reaction device 9 at a flow rate of 86 g / min;

[0132] (4) Setting the temperature of the first microchannel flow reaction device 7 to 120° C., setting the temperature of the second microchannel flow reaction device 8 to 115° C., setting the temperature of the third microchannel flow reaction device 9 to 95° C., adjusting the back pressure valve 38 to adjust the pressure before the valve to 0.8 MPaG, and obtaining a crude Li2S solution through redox reaction;

[0133] (5) The crude Li2S solution obtained in step (4) is introduced into the first liquid phase-separation tower 11 for heat preservation, and the upper n-dodecane phase carries a small amount of lithium sulfide solution through the overflow pipe into the second liquid phase-separation tower 12, and the stratification is completed again in the second liquid phase-separation tower 12, and the n-dodecane enters the organic solvent B recovery tank 14 through the overflow pipe.

[0134] (6) The second stop valve 30 and the third stop valve 31 are controlled to allow the lithium sulfide solution that has completed phase separation to enter the first precision filter 13, and after removing most of the insoluble impurities, enter the first lithium sulfide solution storage tank 15, and then be pumped into the second precision filter 17 by the first lithium sulfide solution delivery pump 16 for secondary fine filtration, and the filtered solution obtained enters the second lithium sulfide solution storage tank 18.

[0135] (7) The 14% Li2S / trifluoroacetic acid solution is pumped into the vertical wiped film evaporator 20 by the second lithium sulfide solution delivery pump 19, and the first desolventizing treatment is carried out at a temperature of 50° C. and a pressure of 10 to 12 kPaA for 20 min, and then the solution enters the horizontal wiped film evaporator 21, and the second desolventizing treatment is carried out at a temperature of 50° C. and a pressure of 1200 PaA for 60 min;

[0136] (8) The fine lithium sulfide after the second desolventizing treatment in step (7) enters the continuous drying device 23, is dried at 500° C. for 5 h, and then is transferred to the crusher 24 for dry grinding for 5 h, and then is sent to the vibration screening device 26 by the air conveying device 25, and finally a high-purity lithium sulfide product is obtained in the inert packaging system 27.

[0137] Preparation Example 2

[0138] This preparation example provides a method for continuously producing lithium sulfide, which is implemented using the continuous production device system provided in Example 1. The device in the continuous production device system uses high-purity nitrogen to replace for 1 hour to form an inert atmosphere. The method includes the following steps:

[0139] (1) After the high-quality liquid sulfur is maintained at 118° C. by the heating device 6, the first check valve 31 and the first flow meter 32 are regulated to pump the sulfur into the first microchannel flow reaction device 7 at a flow rate of 10 g / min;

[0140] The purity of high-quality liquid S is greater than 99.95%, and the mass content of Fe is 28 ppm, the mass content of water is 500 ppm, and the acidity is 20.5 ppm (calculated as sulfuric acid);

[0141] (2) 433 g of Li was ground in a lithium metal wet grinding device 1 at room temperature for 6 h until the particle size was less than 100 μm, and then the wet-ground Li powder was transported to a homogenizer device 2 through a vibrating hopper under the lithium metal wet grinding device 1, and 4980 g of turpentine was introduced into the homogenizer device 2, and stirred and mixed in the homogenizer device 2 at room temperature for 20 min to obtain 5412 g of lithium metal powder slurry; then the obtained lithium metal slurry was preheated to 117° C. by a first preheating device 4, and then the second check valve 33 and the second flowmeter 34 were regulated to pump the slurry into the first microchannel flow reaction device 7 at a flow rate of 60 g / min;

[0142] Wherein, the molar ratio of the liquid sulfur in step (1) to the metallic lithium in step (2) is 0.9:2;

[0143] (3) After the ethanol is maintained at 78° C. by the second preheating device 28 , the third check valve 35 and the third flow meter 36 are regulated to pump the ethanol into the first microchannel flow reaction device 9 at a flow rate of 43 g / min;

[0144] (4) Setting the temperature of the first microchannel flow reaction device 7 to 123° C., setting the temperature of the second microchannel flow reaction device 8 to 117° C., setting the temperature of the third microchannel flow reaction device 9 to 98° C., adjusting the back pressure valve 38 to adjust the pressure before the valve to 0.3 MpaG, and obtaining a crude Li2S solution through redox reaction;

[0145] (5) The crude Li2S solution obtained in step (4) is introduced into the first liquid phase separation tower 11 for heat preservation, and the upper turpentine phase carries a small amount of lithium sulfide solution through the overflow pipe into the second liquid phase separation tower 12, and the phase separation is completed again in the second liquid phase separation tower 12, and the turpentine enters the organic solvent B recovery tank 14 through the overflow pipe.

[0146] (6) The second stop valve 30 and the third stop valve 31 are controlled to allow the lithium sulfide solution that has completed phase separation to enter the first precision filter 13, and after removing most of the insoluble impurities, enter the first lithium sulfide solution storage tank 15, and then be pumped into the second precision filter 17 by the first lithium sulfide solution delivery pump 16 for secondary fine filtration, and the filtered solution obtained enters the second lithium sulfide solution storage tank 18.

[0147] (7) The 25% Li2S / ethanol solution is pumped into the vertical wiped film evaporator 20 by the second lithium sulfide solution delivery pump 19, and the first desolventizing treatment is carried out at a temperature of 60° C. and a pressure of 10 to 12 kPaA for 30 min, and then enters the horizontal wiped film evaporator 21, and the second desolventizing treatment is carried out at a temperature of 60° C. and a pressure of 300 PaA for 90 min;

[0148] (8) The fine lithium sulfide after the second solvent treatment in step (7) enters the continuous drying device 23, is dried at 450° C. for 4 hours, and then is transferred to the crusher 24 for dry grinding for 4 hours, and then is sent to the vibration screening device 26 by the air conveying device 25, and finally a high-purity lithium sulfide product is obtained in the inert packaging system 27.

[0149] Preparation Example 3

[0150] The method for continuously producing lithium sulfide provided in this preparation example is implemented by using the continuous production device system provided in Example 1. The device in the continuous production device system uses high-purity nitrogen to replace for 1 hour to form an inert atmosphere. The method comprises the following steps:

[0151] (1) After the high-quality liquid sulfur is maintained at 118° C. by the heating device 6, the first check valve and the first flow meter are regulated to pump the sulfur into the first microchannel flow reaction device 7 at a flow rate of 10 g / min;

[0152] The purity of high-quality liquid S is greater than 99.95%, and the mass content of Fe is 28 ppm, the mass content of water is 500 ppm, and the acidity is 20.5 ppm (calculated as sulfuric acid);

[0153] (2) 547 g of Li was ground in a lithium metal wet grinding device 1 at room temperature for 5 h until the particle size was less than 150 μm, and then the wet-ground Li powder was transported to a homogenizer device 2 through a vibrating hopper under the lithium metal wet grinding device 1, and 4923 g of ethylene glycol butyl ether was introduced into the homogenizer device 2, and stirred and mixed in the homogenizer device 2 at room temperature for 30 min to obtain 5469 g of lithium metal powder slurry; then the obtained lithium metal slurry was preheated to 119° C. by a first preheating device 4, and then the second check valve 33 and the second flowmeter 34 were regulated to pump the slurry into the first microchannel flow reaction device 7 at a flow rate of 45 to 46 g / min;

[0154] Wherein, the molar ratio of the liquid sulfur in step (1) to the metallic lithium in step (2) is 0.95:2;

[0155] (3) After the isopropanol is maintained at 82° C. by the second preheating device 28 , the third check valve 35 and the third flow meter 36 are regulated to pump the isopropanol into the first microchannel flow reaction device 9 at a flow rate of 28 to 29 g / min;

[0156] (4) Setting the temperature of the first microchannel flow reaction device 7 to 125° C., setting the temperature of the second microchannel flow reaction device 8 to 119° C., setting the temperature of the third microchannel flow reaction device 9 to 100° C., adjusting the back pressure valve 38 to adjust the pressure before the valve to 0.25 MPaG, and obtaining a crude Li2S solution through redox reaction;

[0157] (5) The crude Li2S solution obtained in step (4) is introduced into the first liquid phase-separation tower 11 for heat preservation, and the upper layer of ethylene glycol butyl ether carries a small amount of lithium sulfide solution into the second liquid phase-separation tower 12 through the overflow pipe, and the phase separation is completed again in the second liquid phase-separation tower 12, and the ethylene glycol butyl ether enters the organic solvent B recovery tank 14 through the overflow pipe.

[0158] (6) The second stop valve 30 and the third stop valve 31 are controlled to allow the phase-separated lithium sulfide solution to enter the first precision filter 13, and after removing most of the insoluble impurities, enter the first lithium sulfide solution storage tank 15. The first lithium sulfide solution delivery pump 16 pumps the solution into the second precision filter 17 for secondary fine filtration, and the filtered solution enters the second lithium sulfide solution storage tank 18.

[0159] (7) The 33% Li2S / isopropanol solution is pumped into the vertical wiped film evaporator 20 by the second lithium sulfide solution delivery pump 19. The first desolventizing treatment is performed at a temperature of 65°C and a pressure of 5-7 kPaA for 36 minutes, and then the solution enters the horizontal wiped film evaporator 21 and is subjected to a second desolventizing treatment at a temperature of 60°C and a pressure of 500 PaA for 90 minutes;

[0160] (8) The fine lithium sulfide after the second solvent treatment in step (7) enters the continuous drying device 23, is dried at 500° C. for 3 hours, and then is transferred to the crusher 24 for dry grinding for 3 hours, and then is sent to the vibration screening device 26 by the air conveying device 25, and finally a high-purity lithium sulfide product is obtained in the inert packaging system 27.

[0161] Preparation Example 4

[0162] The method for continuously producing lithium sulfide provided in this preparation example is implemented by using the continuous production device system provided in Example 1. The device in the continuous production device system uses high-purity nitrogen to replace for 1 hour to form an inert atmosphere. The method comprises the following steps:

[0163] (1) After the high-quality liquid sulfur is maintained at 118° C. by the heating device 6, the first check valve and the first flow meter are regulated to pump the sulfur into the first microchannel flow reaction device 7 at a flow rate of 10 g / min;

[0164] The purity of high-quality liquid S is greater than 99.95%, and the mass content of Fe is 28 ppm, the mass content of water is 500 ppm, and the acidity is 20.5 ppm (calculated as sulfuric acid);

[0165] (2) 520 g of Li was ground in a lithium metal wet grinding device 1 at room temperature for 4 h until the particle size was less than 200 μm, and then the wet-ground Li powder was transported to a homogenizer device 2 through a vibrating hopper under the lithium metal wet grinding device 1, and 2945 g of xylene was introduced into the homogenizer device 2 at the same time, and stirred and mixed in the homogenizer device 2 at room temperature for 60 min to obtain 3464 g of lithium metal powder slurry; then the obtained lithium metal slurry was preheated to 121° C. by a first preheating device 4, and then the second check valve 33 and the second flowmeter 34 were regulated to pump the slurry into the first microchannel flow reaction device 7 at a flow rate of 29 g / min;

[0166] Wherein, the molar ratio of the liquid sulfur in step (1) to the metallic lithium in step (2) is 1:2;

[0167] (3) After the n-butanol is maintained at 117° C. by the second preheating device 28 , the third check valve 35 and the third flow meter 36 are regulated to pump the n-butanol into the first microchannel flow reaction device 9 at a flow rate of 14 to 15 g / min;

[0168] (4) The temperature of the first microchannel flow reaction device 7 is set to 128° C., the temperature of the second microchannel flow reaction device 8 is set to 121° C., and the temperature of the third microchannel flow reaction device 9 is set to 105° C. The back pressure valve 38 is regulated to adjust the pressure before the valve to 1.15 MPaG, and a crude Li2S solution is obtained through redox reaction;

[0169] (5) The crude Li2S solution obtained in step (4) is introduced into the heat-insulating first liquid phase-separation tower 11, and the upper xylene phase carries a small amount of lithium sulfide solution through the overflow pipe into the second liquid phase-separation tower 12, and the phase separation is completed again in the second liquid phase-separation tower 12, and the xylene enters the organic solvent B recovery tank 14 through the overflow pipe.

[0170] (6) The second stop valve 30 and the third stop valve 31 are controlled to allow the lithium sulfide solution that has completed phase separation to enter the first precision filter 13, and after removing most of the insoluble impurities, enter the first lithium sulfide solution storage tank 15, and then be pumped into the second precision filter 17 by the first lithium sulfide solution delivery pump 16 for secondary fine filtration, and the filtered solution obtained enters the second lithium sulfide solution storage tank 18.

[0171] (7) The 50% Li2S / n-butanol solution is pumped into the vertical wiped film evaporator 20 by the second lithium sulfide solution delivery pump 19. The first desolventizing treatment is performed at a temperature of 80°C and a pressure of 10-12 kPaA for 40 minutes, and then the solution enters the horizontal wiped film evaporator 21 and is subjected to a second desolventizing treatment at a temperature of 80°C and a pressure of 200 PaA for 120 minutes;

[0172] (8) The fine lithium sulfide after the second solvent treatment in step (7) enters the continuous drying device 23, is dried at 700° C. for 5 h, and then is transferred to the crusher 24 for dry grinding for 5 h, and then is sent to the vibration screening device 26 by the air conveying device 25, and finally a high-purity lithium sulfide product is obtained in the inert packaging system 27.

[0173] Preparation Example 5

[0174] The method for continuously producing lithium sulfide provided in this preparation example is implemented by using the continuous production device system provided in Example 1. The device in the continuous production device system uses high-purity nitrogen to replace for 1 hour to form an inert atmosphere. The method comprises the following steps:

[0175] (1) After the high-quality liquid sulfur is maintained at 118° C. by the heating device 6, the first check valve and the first flow meter are regulated to pump the sulfur into the first microchannel flow reaction device 7 at a flow rate of 10 g / min;

[0176] The purity of high-quality liquid S is greater than 99.95%, and the mass content of Fe is 28 ppm, the mass content of water is 500 ppm, and the acidity is 20.5 ppm (calculated as sulfuric acid);

[0177] (2) 472.5 g of Li was ground in a lithium metal wet grinding device 1 at room temperature for 3 h until the particle size was less than 300 μm, and then the wet-ground Li powder was transported to a homogenizer device 2 through a vibrating hopper under the lithium metal wet grinding device 1, and 1890 g of N-methylpyrrolidone (NMP) was introduced into the homogenizer device 2, and stirred and mixed in the homogenizer device 2 at room temperature for 25 min to obtain 2361 g of lithium metal powder slurry; then the obtained lithium metal slurry was preheated to 123° C. by a first preheating device 4, and then the second check valve 33 and the second flowmeter 34 were regulated to pump the slurry into the first microchannel flow reaction device 7 at a flow rate of 20 g / min;

[0178] Wherein, the molar ratio of the liquid sulfur in step (1) to the metallic lithium in step (2) is 1.1:2;

[0179] (3) After the ethanol is maintained at 78° C. by the second preheating device 28 , the third check valve 35 and the third flow meter 36 are regulated to pump the ethanol into the first microchannel flow reaction device 9 at a flow rate of 9 to 10 g / min;

[0180] (4) The temperature of the first microchannel flow reaction device 7 is set to 130° C., the temperature of the second microchannel flow reaction device 8 is set to 125° C., and the temperature of the third microchannel flow reaction device 9 is set to 110° C. The back pressure valve 38 is adjusted to adjust the pressure before the valve to 1.25 MPaG, and a crude Li2S solution is obtained through redox reaction;

[0181] (5) The crude Li2S solution obtained in step (4) is introduced into the heat-insulating first liquid phase-separation tower 11, and the upper NMP phase carries a small amount of lithium sulfide solution through the overflow pipe into the second liquid phase-separation tower 12, and the phase separation is completed again in the second liquid phase-separation tower 12, and the NMP enters the organic solvent B recovery tank 14 through the overflow pipe.

[0182] (6) The second stop valve 30 and the third stop valve 31 are controlled to allow the phase-separated lithium sulfide solution to enter the first precision filter 13, and after removing most of the insoluble impurities, enter the first lithium sulfide solution storage tank 15. The first lithium sulfide solution delivery pump 16 pumps the solution into the second precision filter 17 for secondary fine filtration, and the filtered solution enters the second lithium sulfide solution storage tank 18.

[0183] (7) The 59% Li2S / ethanol solution is pumped into the vertical wiped film evaporator 20 by the second lithium sulfide solution delivery pump 19. The first desolventizing treatment is performed at a temperature of 62° C. and a pressure of 12-15 kPaA for 25 min, and then the solution enters the horizontal wiped film evaporator 21 and is subjected to a second desolventizing treatment at a temperature of 60° C. and a pressure of 600 PaA for 100 min;

[0184] (8) The fine lithium sulfide treated with the second solvent in step (7) enters the continuous drying device 23, is dried at 450° C. for 2 hours, and is then transferred to the crusher 24 for dry grinding for 2 hours. It is then transferred to the vibration screening device 26 by the air conveying device 25, and finally a high-purity lithium sulfide product is obtained in the inert packaging system 27.

[0185] Preparation Example 6

[0186] The method for continuously producing lithium sulfide provided in this preparation example is implemented by using the continuous production device system provided in Example 1. The device in the continuous production device system uses high-purity nitrogen to replace for 1 hour to form an inert atmosphere. The method comprises the following steps:

[0187] (1) After the high-quality liquid sulfur is maintained at 118° C. by the heating device 6, the first check valve and the first flow meter are regulated to pump the sulfur into the first microchannel flow reaction device 7 at a flow rate of 10 g / min;

[0188] The purity of high-quality liquid S is greater than 99.95%, and the mass content of Fe is 28 ppm, the mass content of water is 500 ppm, and the acidity is 20.5 ppm (calculated as sulfuric acid);

[0189] (2) 433 g of Li was ground in a lithium metal wet grinding device 1 at room temperature for 2 h until the particle size was less than 500 μm, and then the wet-ground Li powder was transported to a homogenizer device 2 through a vibrating hopper under the lithium metal wet grinding device 1, and 1300 g of ethyl benzoate was introduced into the homogenizer device 2, and stirred and mixed in the homogenizer device 2 at room temperature for 10 min to obtain 1732 g of lithium metal powder slurry; then the obtained lithium metal slurry was preheated to 125° C. by a first preheating device 4, and then the second check valve 33 and the second flowmeter 34 were adjusted to pump the slurry into the first microchannel flow reaction device 7 at a flow rate of 14 to 15 g / min;

[0190] Wherein, the molar ratio of the liquid sulfur in step (1) to the metallic lithium in step (2) is 1.2:2;

[0191] (3) After the methanol is maintained at 64° C. by the second preheating device 28 , the third check valve 35 and the third flow meter 36 are regulated to pump the methanol into the first microchannel flow reaction device 9 at a flow rate of 6 to 7 g / min;

[0192] (4) Setting the temperature of the first microchannel flow reaction device 7 to 120° C., setting the temperature of the second microchannel flow reaction device 8 to 123° C., setting the temperature of the third microchannel flow reaction device 9 to 115° C., adjusting the back pressure valve 38 to adjust the pressure before the valve to 0.7 MPaG, and obtaining a crude Li2S solution through redox reaction;

[0193] (5) The crude Li2S solution obtained in step (4) is introduced into the first liquid phase-separation tower 11 for heat preservation, and the upper ethyl benzoate phase carries a small amount of lithium sulfide solution through the overflow pipe into the second liquid phase-separation tower 12, and the phase separation is completed again in the second liquid phase-separation tower 12, and the ethyl benzoate enters the organic solvent B recovery tank 14 through the overflow pipe.

[0194] (6) The second stop valve 30 and the third stop valve 31 are controlled to allow the phase-separated lithium sulfide solution to enter the first precision filter 13, and after removing most of the insoluble impurities, enter the first lithium sulfide solution storage tank 15. The first lithium sulfide solution delivery pump 16 pumps the solution into the second precision filter 17 for secondary fine filtration, and the filtered solution enters the second lithium sulfide solution storage tank 18.

[0195] (7) The 65% Li2S / methanol solution is pumped into the vertical wiped film evaporator 20 by the second lithium sulfide solution delivery pump 19. The first desolventizing treatment is performed at a temperature of 50°C and a pressure of 10-12 kPaA for 15 minutes, and then the solution enters the horizontal wiped film evaporator 21 and is subjected to a second desolventizing treatment at a temperature of 50°C and a pressure of 1200 PaA for 40 minutes;

[0196] (6) The fine lithium sulfide after the second solvent treatment in step (7) enters the continuous drying device 23, is dried at 300° C. for 6 hours, and is then transferred to the crusher 24 for dry grinding for 6 hours. It is then transferred to the vibration screening device 26 by the air conveying device 25, and finally a high-purity lithium sulfide product is obtained in the inert packaging system 27.

[0197] Preparation Example 7

[0198] This preparation example provides a method for continuously producing lithium sulfide. Except for using the continuous production device system provided in Example 2, other conditions are the same as those in Preparation Example 1.

[0199] Preparation Example 8

[0200] This preparation example provides a method for continuously producing lithium sulfide. Except for adjusting the back pressure valve 38 to adjust the pressure before the valve to 0.25 MPaG in step (3), other conditions are the same as those in Preparation Example 1.

[0201] Preparation Example 9

[0202] This preparation example provides a method for continuously producing lithium sulfide. Except for adjusting the back pressure valve 38 to adjust the pressure before the valve to 1.25 MpaG in step (3), other conditions are the same as those in Preparation Example 1.

[0203] Comparative Preparation Example 1

[0204] This comparative preparation example 1 provides a method for continuously producing lithium sulfide. Except for using the continuous production device system provided in comparative example 1, other conditions are the same as those in preparation example 1.

[0205] The lithium sulfide products obtained in the above preparation examples and comparative preparation examples were characterized and the yields were calculated. The results are shown in Table 1.

[0206] Among them, the test method is:

[0207] Moisture: Tested using Karl Fischer Coulometry;

[0208] Impurity metal content: quantitative analysis using ICP-OES instrument;

[0209] Free chlorine and sulfate content: tested using ion chromatography, column model Thermo Fisher AS22 anion analysis column 4×250mm; 150mmol / L sulfuric acid solution was used as the inhibitory solution; eluent preparation steps: 1) first prepare the buffer solution (mother liquor): 4.5428g NaHCO3, 8.4813g Na2CO3, add 200mL distilled water to dissolve, ultrasonic dissolution, and filter; 2) prepare the mobile phase: take 20mL mother liquor, 1380g distilled water, and 600ml acetonitrile, stir and mix well, and set aside.

[0210] Table 1 Performance Characterization Parameters of Lithium Sulfide Products Prepared in Preparation Examples and Comparative Preparation Examples

[0211]

[0212]

[0213] From Table 1 we can see that:

[0214] (1) The continuous production device system and production method provided by the present invention have a high yield of lithium sulfide, with a comprehensive yield of >97%. The Li2S product has a high purity, with a purity of >99.99% by deduction method. Water content ≤15ppm, SO4 2 -<20ppm, free chlorine mass content<10ppm, Na<30ppm, Si<30ppm, Ca<20ppm, Mg<20ppm, other impurity metals are all <10ppm, which meets the application standards in electrolyte;

[0215] (2) From the comparison between Preparation Example 1 and Preparation Example 7, it can be seen that when the horizontal wiped film evaporator 21 is not provided, the solvent in the lithium sulfide cannot be completely removed, resulting in a low compaction density of the product, by-product impurities are generated during the drying process, resulting in an increase in the content of sulfate, chloride ions, and ethanol insolubles, and the content of each impurity metal ion also increases to varying degrees;

[0216] (3) From the comparison between Preparation Example 1 and Preparation Examples 8-9, it can be seen that when the pressure drop of the microchannel flow reaction device is low, the metal salt will precipitate and settle in the microchannel due to the rapid loss of the reaction solvent, and the reaction channel is easily blocked, resulting in low product conversion rate, large liquid sulfur residue, high product acid value, and high impurity and insoluble content; when the pressure drop of the microchannel flow reaction device is high, polysulfide side reactions may occur easily, resulting in an increase in the product color number, and the corresponding sulfate and ethanol insolubles are also high;

[0217] (4) It can be seen from the comparison between Preparation Example 1 and Comparative Preparation Example 1 that when the reaction device is only the first microchannel flow reaction device 7, the product yield is greatly reduced due to insufficient reaction.

[0218] The method provided by the present invention overcomes the industry pain points of complex lithium sulfide preparation process, the need for ball milling or greenhouse gas generation, the presence of polysulfides, the need for multiple redissolution and purification, low product yield, difficult separation of metal impurities and inability to produce continuously. The method has a simple process flow design, and continuous production is suitable for industrial transformation. The obtained product has high yield and high purity, has a high solvent utilization rate, is low in three wastes, and has low energy consumption. It is a safe, environmentally friendly, low-cost production method for continuously preparing battery-grade lithium sulfide, and has good economic benefits.

[0219] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0220] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0221] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0222] In addition, the various embodiments of the present invention may be arbitrarily combined, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed in the present invention.

[0223] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A continuous production system for battery-grade lithium sulfide, It is characterized in that include: A feeding unit, a continuous flow reaction unit and a purification unit connected in series; The feeding unit includes a liquid sulfur feeding module, a metal lithium slurry feeding module and an organic solvent A feeding module which are independently arranged, wherein the liquid sulfur feeding module is used to convey liquid sulfur, the metal lithium slurry feeding module is used to mix metal lithium and organic solvent B to form metal lithium slurry and convey the metal lithium slurry, and the organic solvent A feeding module is used to convey organic solvent A; The continuous flow reaction unit comprises m microchannel flow reaction devices connected in series, the first microchannel flow reaction device is connected to the liquid sulfur feeding module and the metal lithium slurry feeding module, and can be used for the liquid sulfur and the metal lithium slurry to mix and react to form a first mixed system containing lithium sulfide, and the mth microchannel flow reaction device is connected to the organic solvent A feeding module, and can be used for the first mixed system to mix with the organic solvent A to form a second mixed system; The purification unit includes a liquid phase separation module and a desolventizing module connected in series. The liquid phase separation module is connected to the mth microchannel flow reaction device and is used to phase separate the second mixed system and obtain a third mixed system and an organic solvent B. The desolventizing module is at least used to separate the third mixed system into a fourth mixed system and an organic solvent A. The lithium sulfide contained in the fourth mixed system is battery-grade lithium sulfide, and m≥3.

2. The continuous production system of battery-grade lithium sulfide according to claim 1, Features: The liquid sulfur feed module comprises a liquid sulfur storage device and a heating device connected in sequence, wherein the heating device is directly connected to the first microchannel flow reaction device; Preferably, a liquid sulfur delivery pump is provided between the liquid sulfur storage device and the heating device. Preferably, a first check valve, a first flow meter and a first stop valve are sequentially arranged on the pipeline connecting the liquid sulfur storage device and the heating device; And / or, the metal lithium slurry feeding module includes a grinding device, an organic solvent B storage device, a homogenizer device and a first preheating device, the grinding device and the organic solvent B storage device are connected to the homogenizer device, the homogenizer device is connected to the first preheating device, and the first preheating device is directly connected to the first microchannel flow reaction device; Preferably, an inertial protection vibration feeding funnel is further provided between the grinding device and the homogenizer device; Preferably, a metal lithium slurry delivery pump is further provided on the connecting pipeline between the homogenizer device and the first preheating device; Preferably, a second check valve and a second flow meter are sequentially arranged on the connecting pipeline between the metal lithium slurry delivery pump and the first preheating device; And / or, the organic solvent A feeding module comprises an organic solvent A storage device and a second preheating device connected in sequence, and the second preheating device is directly connected to the mth microchannel flow reaction device; Preferably, an organic solvent A delivery pump, a third check valve, and a third flow meter are sequentially arranged on the connecting pipeline between the organic solvent A storage device and the second preheating device.

3. The continuous production system of battery-grade lithium sulfide according to claim 1, Features: The channel diameter of the microchannel flow reaction device is 1 mm to 10 mm; And / or, the channel structure of the microchannel flow reaction device includes any one of a heart shape, a zigzag shape, a thorn shape, a baffle shape or a Y shape, or a combination of at least two thereof; Preferably, the liquid holding volume of the microchannel flow reaction device is 7 mL to 70 mL.

4. The continuous production system of battery-grade lithium sulfide according to claim 1, Features: The liquid phase separation module comprises p liquid phase separation towers connected in sequence, the first liquid phase separation tower is connected to the mth microchannel flow reaction device, the top of the pth liquid phase separation tower is connected to the top of the p-1th liquid phase separation tower through an overflow pipe, and the bottoms of the p liquid phase separation towers are independently connected to the desolventizing module, p≥2; Preferably, a back pressure valve is further provided on the connecting pipeline between the first liquid phase separation tower and the mth microchannel flow reaction device; Preferably, the pth liquid phase separation tower is also connected to an organic solvent B recovery device; Preferably, the desolventizing module comprises at least one filtering device and at least one thin film evaporation device connected in sequence, and the p liquid phase separation towers are connected to the filtering device; Preferably, at least one filtering device comprises a first filtering device and a second filtering device connected in sequence, and the pore size of the first filtering device is larger than the pore size of the second filtering device; Preferably, the pore size of the first filter device includes any one of 50 μm, 200 μm or 500 μm, or a combination of at least two thereof; Preferably, the pore size of the second filter device includes any one of 0.45 μm, 1 μm or 10 μm, or a combination of at least two of them; Preferably, the first filtering device comprises at least two sets of filters connected in parallel; Preferably, the second filtering device comprises at least two sets of filters connected in parallel; Preferably, the desolventizing module further comprises an organic solvent A recovery device, and the organic solvent A recovery device is connected to the thin film evaporation device; Preferably, the thin film evaporation device comprises at least one vertical wiped film evaporator and / or at least one horizontal wiped film evaporator; Preferably, the thin film evaporation device comprises a plurality of vertical scraped film evaporators or a plurality of horizontal scraped film evaporators or at least one of the vertical scraped film evaporators and at least one of the horizontal scraped film evaporators which are connected in series in sequence.

5. The continuous production system of battery-grade lithium sulfide according to claim 1, Features: The purification unit also includes a post-processing module, which is connected to the desolventizing module, and includes a drying device, a crushing device, an air conveying device, a vibration screening device and an inert environment packaging device which are connected in sequence.

6. A method for continuously producing battery-grade lithium sulfide, It is characterized in that include: Providing a continuous production system for the battery-grade lithium sulfide according to any one of claims 1 to 5; Liquid sulfur is transported to the first microchannel flow reaction device via a liquid sulfur feeding module, metal lithium and organic solvent B are mixed to form metal lithium slurry via a metal lithium slurry feeding module, and the metal lithium slurry is transported to the first microchannel flow reaction device, and the liquid sulfur and the metal lithium slurry are mixed and reacted in the first microchannel flow reaction device to form a first mixed system containing lithium sulfide; organic solvent A is transported to the mth microchannel flow reaction device via an organic solvent A feeding module, and the first mixed system is sequentially processed through the second microchannel flow reaction device ... the m-1th microchannel flow reaction device, and then mixed with organic solvent A in the mth microchannel flow reaction device to form a second mixed system; The second mixed system is transported to a liquid phase separation module for phase separation to obtain a third mixed system and an organic solvent B, and then the third mixed system is transported to a desolventizing module for desolventizing treatment to obtain a fourth mixed system and an organic solvent A, wherein the lithium sulfide contained in the fourth mixed system is battery-grade lithium sulfide.

7. The method for continuously producing battery-grade lithium sulfide according to claim 6, It is characterized in that Specifically include: The liquid sulfur is transported to the first microchannel flow reaction device after being kept warm by a heating device; The metallic lithium is ground by a grinding device and then conveyed to a homogenizer device. Meanwhile, the organic solvent B is conveyed to the homogenizer device for slurrying to obtain metallic lithium slurry. The metallic lithium slurry is preheated by a first preheating device and then conveyed to a first microchannel flow reaction device. The organic solvent A is preheated by the second preheating device and then transported to the mth microchannel flow reaction device; Preferably, the temperature of the heating device is 118°C to 128°C; Preferably, the temperature of the first preheating device is 115°C to 125°C; Preferably, the temperature of the second preheating device is 70°C to 115°C; And / or, the organic solvent A comprises any one or a combination of at least two of methanol, ethanol, isopropanol, n-butanol, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid or trifluoroacetic acid; And / or, the organic solvent B includes any one or a combination of at least two of methyl silicone oil, turpentine, ethylene glycol butyl ether, diphenyl ether, n-hexane, cyclohexane, n-dodecane, n-octadecane, 1-fluorohexane, toluene, xylene, cyclohexanone, N-methylpyrrolidone, amyl acetate, and ethyl benzoate; And / or, the water mass content of the organic solvent A is less than 50ppm; And / or, the water mass content of the organic solvent B is less than 50ppm; And / or, the mass concentration of metallic lithium in the metallic lithium slurry does not exceed 25%; The mass concentration of the metallic lithium in the metallic lithium slurry is 5% to 25%; Preferably, the purity of the metallic lithium is ≥99.9% and the particle size is ≤500 μm; Preferably, in the metallic lithium, the mass content of Na is ≤200ppm, the mass content of Ca is ≤200ppm, the mass content of free chlorine is <60ppm, and the mass content of nitrogen is ≤200ppm; And / or, the molar ratio of the liquid sulfur to the metallic lithium is (0.80-1.20):

2.

8. The method for continuously producing battery-grade lithium sulfide according to claim 6, Features: The pressure conditions in the m microchannel flow reaction devices are the same, and the temperature conditions decrease gradually from the first microchannel flow reaction device to the mth microchannel flow reaction device; Preferably, the temperature in the first microchannel flow reaction device is 120°C to 130°C, and the temperature in the mth microchannel flow reaction device is 95°C to 115°C; Preferably, when m=3, the temperature in the first microchannel flow reaction device is 120°C to 130°C, the temperature in the second microchannel flow reaction device is 115°C to 125°C, and the temperature in the third microchannel flow reaction device is 95°C to 115°C; Preferably, the pressure in the m microchannel flow reaction devices is 0.25MpaG to 1.25MpaG; Preferably, the total residence time of the material in the m microchannel flow reaction devices is 15s to 150s.

9. The method for continuously producing battery-grade lithium sulfide according to claim 6, Features: The operating temperature of the liquid phase separation module is 50°C to 115°C; And / or, the desolventizing module comprises at least one filtering device and at least one thin film evaporating device connected in sequence, and the third mixed system is sequentially conveyed to the filtering device and the thin film evaporating device for treatment, so as to separate the third mixed system into a fourth mixed system and an organic solvent A, and the thin film evaporating device comprises a vertical scraped film evaporator and / or a horizontal scraped film evaporator, the vertical scraped film evaporator has an operating temperature of 50°C to 120°C and an operating pressure of 5kPaA to 15kPaA, and the horizontal scraped film evaporator has an operating temperature of 50°C to 150°C and an operating pressure of 200PaA to 1200PaA; Preferably, the residence time of the material in the vertical scraped film evaporator is 15 min to 40 min, and the residence time of the material in the horizontal scraped film evaporator is 40 min to 120 min; Preferably, the purity of the battery-grade lithium sulfide reaches 99.99%; the total mass content of impurity metals in the battery-grade lithium sulfide is <100ppm, wherein the impurity metals include Na<30ppm, Si<30ppm, Ca<20ppm, Mg<20ppm, and other impurity metals are all <10ppm; the particle size d50 of the battery-grade lithium sulfide is <10μm, and d90<20μm; the moisture content of the battery-grade lithium sulfide is ≤15ppm; the mass content of free chlorine in the battery-grade lithium sulfide is <10ppm, and the mass content of sulfate is <20ppm.

10. The method for continuously producing battery-grade lithium sulfide according to claim 6, It is characterized in that Also includes: The fourth mixed system is sequentially conveyed to a drying device, a crushing device, an air conveying device, a vibration screening device and an inert environment packaging device for post-processing.