Application of hollow carbon nanoparticle material as adsorbent to adsorption of gold ions

By calcining metal organic frame nanoparticles into hollow carbon nanoparticles with graphene layer, the problems of low gold ion concentration and high impurities in electronic waste are solved, and the effect of efficient extraction and recovery of gold ions is achieved.

CN118904291AActive Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH

Patent Information

Application Number
CN202411254516.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-08
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently extract gold ions from electronic waste, especially in complex environments where the concentration of gold ions is extremely low and there are a large number of metal impurities.

Method used

The hollow carbon nanoparticle material that uses metal organic frame nanoparticles with hollow structure to form a graphene layer is calcined as an adsorption agent. The gold ions are efficiently adsorbed through the adsorption and reduction of the graphene layer, and the selection is improved through the doping of nitrogen and oxygen elements. sex.

Benefits of technology

It achieves efficient and stable extraction and recovery of gold ions in complex water quality, with high selectivity and high adsorption, simple preparation process and wide material sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904291A_ABST
    Figure CN118904291A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of gold adsorption, and discloses an application of a hollow carbon nanoparticle material as an adsorbent for adsorbing gold ions. The graphene layer of the hollow carbon nanoparticle material has an adsorption and reduction effect on metal ions, gold ions are subjected to adsorption and reduction, metal organic framework nanoparticles with hollow structures are used as starting raw materials, carbon elements are graphitized in the pyrolysis process to form the hollow structures, doping of nitrogen and oxygen elements is achieved at the same time, and the metal organic framework nanoparticles with the hollow structures are used as the starting raw materials. Therefore, the selective adsorption performance on gold ions is obviously improved. The preparation process of the hollow carbon nanoparticle material is simple, the source of the preparation materials is wide, the preparation of the metal organic framework nanoparticles is a relatively mature technology in the prior art, a new application can be provided for the metal organic framework nanoparticles based on the hollow carbon nanoparticle material, and a new thought is provided for gold recovery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gold adsorption, and in particular to an application of a hollow carbon nanoparticle material as an adsorbent to adsorb gold ions. Background Art

[0002] Gold (Au), as a precious metal, has a wide range of applications in science, industry and commerce, especially in catalysis, antibacterial agents and anticancer drugs. In addition, gold is also one of the core materials for electronic products and jewelry. With the continuous growth of demand for gold in industries such as electronics and new energy, relying on raw ore mining can no longer meet the increasing demand. The value of gold continues to rise, mainly due to its scarcity, high consumption and increasing global demand. It is worth noting that the manufacture of electronic equipment consumes about 300 metric tons of gold each year, and the gold content in products such as mobile phones and computer circuit boards is as high as 200-350 grams per metric ton, far exceeding the gold concentration in currently exploitable deposits. There is also a large amount of gold in secondary reservoirs such as incineration ash, wastewater, freshwater bodies and marine environments, which provides a new resource for extracting gold from "electronic waste". However, how to efficiently extract gold from these secondary sources remains a challenge that needs to be solved.

[0003] Currently, one of the main difficulties in extracting gold from "electronic waste" is that the gold concentration in these sources is extremely low, such as in wastewater, the gold concentration is usually less than 10 μg / L, and in seawater it is less than 10 ng / L. In addition, another difficulty is that there are a large number of metal impurities in these secondary sources, and their concentrations are much higher than gold. For example, the liquids in these sources usually contain a variety of organic compounds and competing metal ions, such as sodium, potassium, copper, nickel, iron and rare earth metals, whose concentrations are significantly higher than gold, thereby increasing the complexity of the extraction process. Therefore, developing a material that is low in cost, simple to prepare, and can stably and efficiently extract trace amounts of gold in complex water quality has become an urgent and challenging task at present. Summary of the invention

[0004] In view of the problem of how to efficiently extract gold in a complex environment with extremely low gold ion concentration and high metal impurity concentration, the present invention provides an application of a hollow carbon nanoparticle material as an adsorbent to adsorb gold ions. The present invention provides a hollow carbon nanoparticle material as an adsorbent to adsorb gold ions, which can not only effectively solve the challenge of efficiently extracting gold in a complex environment with low gold concentration and high impurities, but also provide a new solution for efficiently recovering gold from complex liquids.

[0005] The specific technical scheme of the present invention is: The present invention provides an application of a hollow carbon nanoparticle material as an adsorbent for adsorbing gold ions. The special feature of this application is that the hollow carbon nanoparticle material is obtained by calcining metal organic framework nanoparticles with a hollow structure; The calcination process transforms the structure of the metal organic framework nanoparticles into a graphene layer.

[0006] In order to solve the technical problem of extracting gold in a complex environment with extremely low gold ion concentration, numerous metal impurities and relatively high impurity concentration, the present invention uses metal organic framework nanoparticles with a hollow structure as raw materials, and converts the carbon in the structure of the metal organic framework nanoparticles into graphene layers through calcination, thereby preparing a hollow carbon nanoparticle material adsorbent with high selectivity and high adsorption capacity for gold ions.

[0007] The hollow carbon nanoparticle material of the present invention has excellent adsorption performance for gold ions, and the principle is as follows: Through the adsorption and reduction effect of the graphene layer of the hollow carbon nanoparticle material on metal ions, efficient adsorption of gold ions is achieved. In addition, since metal-organic framework nanoparticles with hollow structures are used as starting materials, nitrogen and oxygen elements are doped into the carbon element during the process of transformation into graphene layers, which plays a key role in improving the selective adsorption of gold ions by the hollow carbon nanoparticle material.

[0008] As a preferred embodiment of the above application, the metal organic framework nanoparticles are ZIF-8 nanoparticles.

[0009] As a preferred embodiment of the above application, the temperature of the calcination treatment is 700-1000°C.

[0010] As a preference for the above application, the calcination treatment is carried out under an inert gas atmosphere.

[0011] Specifically, the present invention describes the preparation of the hollow carbon nanoparticle material by taking the following preparation method as an example. The preparation method of the hollow carbon nanoparticle material comprises the following steps: Step S1: adding zinc nitrate hexahydrate and 2-methylimidazole into a solvent respectively, stirring to form nuclei, and obtaining metal organic framework nanoparticles; Step S2: dispersing the metal organic framework nanoparticles obtained in step S1 in a solvent, adding tannic acid, and stirring to react to obtain metal organic framework nanoparticles with a hollow structure; Step S3: taking the metal organic framework nanoparticles with a hollow structure obtained in step S2 and subjecting them to calcination treatment to transform and form a graphene layer in the structure of the nanoparticles.

[0012] The principle of the hollow carbon nanoparticle material of the present invention for adsorbing gold ions is that the gold ions are adsorbed and reduced by the adsorption and reduction effect of the graphene layer of the hollow carbon nanoparticle material on metal ions, and the metal organic framework nanoparticles with a hollow structure are used as the starting material, and nitrogen and oxygen elements are doped in the process of converting the carbon element therein into graphene, thereby improving the selective adsorption effect of the finished hollow carbon nanoparticle material on gold ions. Therefore, the preparation of the metal organic framework nanoparticles with a hollow structure and the preparation of the graphene layer play a relatively important role, and through the above steps S1 to S3, a specific preparation method of a hollow carbon nanoparticle material adsorbent with high selectivity and high adsorption amount for gold ions can be provided.

[0013] Based on the adsorption principle of hollow carbon nanoparticles on gold ions, the present invention can take the above preparation method as an example to adjust the specific preparation process to obtain an adsorbent with better adsorption performance for gold ions. For example, the molar ratio of zinc nitrate hexahydrate and 2-methylimidazole is adjusted, and the mass ratio of metal organic framework nanoparticles and tannic acid, the stirring reaction time, etc. are adjusted, and the temperature and gas atmosphere of the calcination treatment are adjusted.

[0014] As a preferred embodiment of the above method, in step S1, the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole is 1:6-10.

[0015] As a preferred embodiment of the above method, in step S2, the mass ratio of the metal organic framework nanoparticles to tannic acid is 1:4-6.

[0016] As a preferred embodiment of the above method, in step S2, the stirring reaction is carried out at a rotation speed of 200 rpm to 600 rpm and for a time of 5 minutes to 10 minutes.

[0017] As a preferred embodiment of the above method, in step S3, the calcination treatment is performed at a temperature of 700° C. to 1000° C. and for a time of 0.5 hour to 4 hours.

[0018] As a preferred embodiment of the above method, in step S3, the calcination treatment is performed under an inert gas atmosphere.

[0019] Compared with the prior art, the present invention has the following technical effects: (1) The present invention uses metal organic framework nanoparticles with a hollow structure as raw materials, and converts the carbon in the structure of the metal organic framework nanoparticles into graphene layers through calcination. The prepared hollow carbon nanoparticle material has a high selectivity and high adsorption capacity for gold ions.

[0020] (2) The present invention uses the adsorption and reduction effect of the graphene layer of the hollow carbon nanoparticle material on metal ions to adsorb and reduce gold ions, and uses metal organic framework nanoparticles with a hollow structure as the starting material. In the process of converting the carbon element therein to form graphite, nitrogen and oxygen are doped therein, thereby improving the selective adsorption of gold ions by the hollow carbon nanoparticle material. The preparation process is simple and the source of the preparation materials is wide. The preparation of metal organic framework nanoparticles is a relatively mature technology in the prior art. Based on the present invention, a new application of metal organic framework nanoparticles can be provided, which provides a new idea for gold recovery. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 SEM / TEM structural characterization diagram of hollow carbon nanoparticles; Figure 2 XRD comparison diagram of metal organic framework nanoparticles, hollow modified metal organic framework nanoparticles and hollow carbon nanoparticles; Figure 3 This is the Raman spectrum of hollow carbon nanoparticles; Figure 4 is the relationship between the adsorption rate of hollow carbon nanoparticles to gold ions and the pH value of the solution; Figure 5 is the adsorption isotherm of hollow carbon nanoparticles at different initial gold ion concentrations; Figure 6 The effect of adsorption time on the gold ion adsorption performance of hollow carbon nanoparticles; Figure 7 This is a test diagram of the adsorption selectivity of hollow carbon nanoparticles to gold ions; Figure 8 This is a test diagram of the adsorption cycle performance of hollow carbon nanoparticles. DETAILED DESCRIPTION

[0022] The present invention will be further described below in conjunction with embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should belong to the scope of protection of the present invention.

[0023] Example 1 This embodiment provides a hollow carbon nanoparticle material, which is prepared according to the following steps: (1) Preparation of metal organic framework nanoparticles First, weigh 1.968g of 2-methylimidazole (0.0239mol) and 0.891 of hexahydrated zinc nitrate (0.003mol), that is, weigh zinc nitrate hexahydrate and 2-methylimidazole in a molar ratio of 1:8. Dissolve the above two raw materials in 50mL of methanol respectively. After fully dissolved, mix the two at room temperature, and then stir magnetically for 8 hours. After the reaction is completed, centrifuge the resulting reaction solution at 8000rpm for 5 minutes to take the solid precipitate. Then continue to wash the precipitate with 30mL of methanol. After washing, centrifuge at 8000rpm for 5 minutes and discard the upper methanol. Repeat the above washing and centrifugation steps for 3 times. Put the solid powder obtained after washing and centrifugation into a vacuum oven and vacuum dry it at 60°C for 24 hours to obtain metal organic framework nanoparticles, i.e., ZIF-8 materials, which will be retained in the next step.

[0024] (2) Hollow modified ZIF-8 material Weigh 200 mg of the ZIF-8 material prepared in step (1) and 1 g of tannic acid, that is, the ZIF-8 material and tannic acid are weighed in a mass ratio of 1:5. Ultrasonic disperse the weighed ZIF-8 material in 100 mL of methanol, dissolve the weighed tannic acid in 100 mL of deionized water, mix the dispersed methanol suspension and the dissolved tannic acid aqueous solution, and react with magnetic stirring at room temperature for 10 minutes at a stirring rate of 400 rpm. After the stirring reaction, centrifuge the obtained suspension at 8000 rpm for 5 minutes to obtain a solid precipitate. Then continue to wash the precipitate with 30 mL of methanol, centrifuge at 8000 rpm for 5 minutes after washing, discard the upper methanol, repeat the above washing and centrifugation steps, and repeat 5 times. Finally, put the solid powder obtained by washing and centrifugation into a vacuum oven and vacuum dry it at 60°C for 24 hours to obtain hollow modified metal organic framework nanoparticles, that is, HZIF-8 material, which will be retained in the next step.

[0025] (3) Preparation of hollow carbon nanoparticle materials 200 mg of the HZIF-8 material obtained in step (2) was weighed and placed in a porcelain boat of a tubular furnace. Nitrogen was passed through for 30 minutes before the temperature was raised to ensure that all the air in the tube was exhausted. Subsequently, the temperature was raised to 900°C at a heating rate of 5°C / min in a nitrogen atmosphere, and calcined at 900°C for 2 hours. After the temperature was raised and the temperature in the furnace was cooled to room temperature, the calcined solid powder was taken out to obtain a hollow carbon nanoparticle material, which was recorded as HNPC material.

[0026] Example 2 In this example, the materials prepared in step (1), step (2) and step (3) in Example 1 were subjected to structural characterization analysis. The results are shown in Figure 1 , Figure 2 and Figure 3.in, Figure 1 The SEM / TEM structural characterization images of the hollow carbon nanoparticles (HNPC) prepared in step (3) of Example 1, the left image is the SEM structural characterization image, and the right image is the TEM structural characterization image; Figure 2 XRD comparison diagram of metal organic framework nanoparticles (ZIF-8), hollow modified metal organic framework nanoparticles (HZIF-8) and hollow carbon nanoparticles (HNPC); Figure 3 This is the Raman spectrum of the hollow carbon nanoparticles (HNPC) prepared in step (3) of Example 1, where the G peak is the graphene peak and the D peak is the amorphous peak.

[0027] From the characterization results of this embodiment, it can be seen that: Figure 1 The SEM and TEM images of HNPC prepared in Example 1 are shown, and the surface morphology and internal hollow structure of the hollow nanocarbon particles of HNPC are characterized. It can be seen from the TEM image that HNPC successfully prepared a hollow structure. At the same time, from the SEM and TEM characterizations, it can be seen that the particle size of HNPC is about 100nm.

[0028] Figure 2 The results show that the diffraction peaks of synthesized ZIF-8 and HZIF-8 are the same as those of simulated crystal structures, proving the successful synthesis of the crystal structure. The XRD diffraction curve of HNPC shows that HNPC has obvious carbon material diffraction peaks, HNPC is amorphous, and the crystal planes have all disappeared, proving the successful preparation of carbon materials. Figure 2 It can be seen that the HNPC does not have a diffraction peak of zinc metal, indicating that zinc does not exist in the structure of the HNPC material after calcination. Further, this example performed X-ray photoelectron spectroscopy on the HNPC prepared in Example 1, and determined that the HNPC only contained C, N, and O elements, wherein the C content was 91%, the N content was 4%, and the O content was 5%.

[0029] Figure 3 The Raman spectrum of HNPC prepared in Example 1 is shown. Figure 3 It can be seen that the HNPC structure has a graphene layer, and the proportion of the graphene layer, that is, the degree of graphene is 0.88.

[0030] Example 3 In this example, the adsorption performance of the HNPC obtained in Example 1 was tested under the conditions of gold ion solutions with different pH values, and the influence of liquid states with different pH values ​​on the adsorption and recovery of gold ions was studied with a single variable.

[0031] Prepare Au with pH values ​​of 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0 3+ Ionic sample solution, in which Au 3+ The concentration of ions was 100 mg / L, and the pH value was adjusted by HCl or NaOH solution. 2 mg HNPC was added to 5 mL sample solution, and the mixture was stirred at room temperature for 60 minutes. The supernatant was centrifuged and filtered, and the gold ion concentration of the supernatant was measured by inductively coupled plasma mass spectrometry (ICP-MS). The adsorption rate was calculated by the following equation: Where R is the removal efficiency, C0 is the initial concentration, C t is the final concentration at a specific time. Figure 4 As shown in the figure, at different pH values ​​from 1 to 11, HNPC has an adsorption rate of more than 99%, which proves that HNPC has good anti-interference ability in gold adsorption, and HNPC has significant effects in recovering gold at different pH values.

[0032] Example 4 In this example, the adsorption saturation concentration of the HNPC prepared in Example 1 was determined to explore the adsorption behavior of HNPC.

[0033] The adsorption isotherm results of HNPC are shown in Figure 5 As shown. Figure 5 It shows that as the concentration of gold ions increases, the adsorption capacity of HNPC also increases rapidly. When the gold ion concentration reaches 4000ppm, the adsorption process reaches saturation, and the adsorption amount at this time is 2670mg / g.

[0034] The adsorption amount was calculated by the following equation: Where C0 is the initial concentration, Ce is the equilibrium concentration, V is the volume, and m is the mass of the composite material initially used.

[0035] Example 5 In this example, the HNPC prepared in Example 1 was subjected to an adsorption kinetics test to determine the adsorption rate of gold ions on the HNPC and to study the adsorption kinetics of the HNPC.

[0036] The operation of this embodiment is as follows: 5 mg of HNPC is dispersed in 50 mL of a gold ion sample with an initial concentration of 100 ppm, and the gold ion concentration of the solution is tested at each time point at 1 min, 3 min, 10 min, 30 min, 60 min, 2 h, 5 h, 10 h, 24 h and 48 h under magnetic stirring at room temperature of 25 ° C. The adsorption amount is analyzed by ICP-OES and ICP-MS. The results are as follows: Figure 6 shown.

[0037] Depend on Figure 6 It can be seen that the maximum adsorption capacity of HNPC for gold ions is 2461 mg / g.

[0038] Example 6 In this example, the HNPC prepared in Example 1 was added to a mixture containing Cu 2+ 、Na + 、Zn 2+ 、Ni 2+ and Mg 2+ Au as a competing ion 3+ Selective adsorption experiments were carried out in mixed solutions to explore the selective adsorption performance of HNPC for gold ions.

[0039] The operation of this example is as follows: prepare an Au³⁺ mixed solution containing Cu²⁺, Na⁺, Zn²⁺, Ni²⁺ and Mg²⁺ as competitive ions, wherein the concentrations of Cu²⁺, Na⁺, Zn²⁺, Ni²⁺ and Mg²⁺ are approximately 100 mg / L, and the concentration of Au³⁺ is 10 mg / L. Then add 2 mg of HNPC to 5 mL of the mixed solution, stir for 1 hour, and detect the adsorption results. The results are as follows: Figure 7 shown.

[0040] Depend on Figure 7 It can be seen that HNPC has a strong effect on Na + 、Zn 2+ 、Ni 2+ and Mg 2+ The adsorption rate of interfering ions was below 0.05%, Cu 2+ The adsorption rate of Au is the largest, which is 0.09%, and other ions are almost not adsorbed. 3+ It has been almost completely adsorbed, with an adsorption rate of 99.6%, proving that it has good selective adsorption performance for gold ions.

[0041] Example 7 In this example, the recyclability of the HNPC prepared in Example 1 was tested to determine the recyclability of the HNPC.

[0042] In this example, the cyclic performance of HNPC was tested. The adsorbed material was reduced with 20 mL of ascorbic acid (0.002 M). The results of the HNPC adsorption reduction cycle experiment are shown in FIG. Figure 8 shown.

[0043] Depend on Figure 8 It can be seen that after 5 cycles, HNPC 3+ The adsorption performance of the hollow carbon nanoparticles has hardly decreased, which indicates that the hollow carbon nanoparticle material prepared in Example 1 has good recyclability.

[0044] Example 8 The HNPC prepared in Example 1 was applied to the recovery of gold from waste CPUs.

[0045] The specific operation is as follows: Cut the waste CPU into small pieces. The waste CPU contains metal copper, nickel, magnesium, zinc, and gold. The mass contents of copper, nickel, magnesium, zinc, and gold are 90%, 8.1%, 0.5%, 0.6%, and 0.8%, respectively. Mix 119.034 mL of distilled water, 0.966 mL of pyridine (100 mM), and 0.750 g of N-bromosuccinimide (35 mM), weigh 0.3 g of the waste CPU and soak it therein for 24 hours to obtain a CPU leaching solution, and test the initial gold concentration in the CPU leaching solution. Subsequently, 4 mg of HNPC was added to 10 mL of the CPU leaching solution and allowed to stand for 1 hour to extract the gold. After the extraction, the system was centrifuged at 8000 r / min, and the supernatant was taken for ICPMS testing to obtain the final concentration of gold. The adsorption rate of gold was calculated by the equation in Example 3, which is the recovery efficiency of gold in the waste CPU in this experiment.

[0046] This experiment shows that HNPC can adsorb and recover gold ions in waste CPU samples with a recovery efficiency of 99.1%.

[0047] Example 9 Taking Example 1 as a control, this example prepares hollow carbon nanoparticle materials by different preparation processes to explore the influence of the preparation process of the hollow carbon nanoparticle material itself on the gold ion adsorption performance of the product.

[0048] First, various parameters in the preparation of metal organic framework nanoparticles in step (1) were adjusted, and it was found that when the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole was 1:6-10, the hollow carbon nanoparticle material finally prepared had better adsorption performance for gold ions. Specifically, when the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole was 1:6 (other preparation conditions were the same as those in Example 1), the prepared HNPC, when subjected to the experiment shown in Example 6, had a Au 3+The adsorption rate was 99.4%. When the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole was 1:10, the adsorption rate was 99.3%. When the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole was 1:5 (other preparation conditions were the same as those in Example 1), the prepared HNPC was subjected to the experiment shown in Example 6. 3+ The adsorption rate is 88.1%. When the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole is 1:12, the adsorption rate is 88.4%. The role of 2-methylimidazole is to provide organic ligands for metal organic framework nanoparticles. Its role in HNPC is to provide nitrogen and oxygen doping elements for hollow carbon nanoparticle materials. It can be seen that the amount of nitrogen and oxygen doping in hollow carbon nanoparticle materials will have a greater impact on the selective adsorption of gold ions in hollow carbon nanoparticle materials. The research results show that when the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole is between 1:6 and 1:10, the gold ion selective adsorption performance of HNPC is most significant. Therefore, the nitrogen and oxygen doping amount within this ratio range helps to improve the selective adsorption capacity of hollow carbon nanoparticle materials for gold ions.

[0049] In order to verify the effect of nitrogen and oxygen doping on the selective adsorption of gold ions, this example uses commercial graphene and expanded graphite as comparative adsorbents, and performs the saturated adsorption test in Example 4 and the selective adsorption experiment in Example 6. The results show that commercial graphene exhibits different degrees of adsorption and reduction effects on metal ions such as Cu²⁺, Na⁺, Zn²⁺, Ni²⁺ and Mg²⁺, with adsorption rates of 6.6%, 2.9%, 3.2%, 2.4% and 1.3%, respectively, while the adsorption rate for Au³⁺ is only 51%. The test also shows that the saturated adsorption capacity of commercial graphene is 85 mg / g, and the saturated adsorption capacity of expanded graphite is 92 mg / g. These results show that the hollow carbon nanoparticle material of the present invention plays a key role in the adsorption of gold ions, not only in the formation of the graphene layer, but also in the doping of nitrogen and oxygen elements. It is precisely because of the doping of nitrogen and oxygen elements that the hollow carbon nanoparticle material exhibits higher selective adsorption and stronger adsorption capacity for gold ions. Therefore, starting with metal organic framework nanoparticles, the preparation of hollow carbon nanoparticle materials with a graphene layer structure plays a significant role in improving the selective adsorption and adsorption capacity of gold ions.

[0050] Secondly, the various parameters in the preparation of hollow metal organic framework nanoparticles in step (2) were adjusted, and it was found that when the mass ratio of metal organic framework nanoparticles to tannic acid was 1:4-6, the hollow carbon nanoparticle material finally prepared had better adsorption performance for gold ions. Specifically, when the mass ratio of metal organic framework nanoparticles to tannic acid was 1:4 (other preparation conditions were the same as those in Example 1), the prepared HNPC, when subjected to the saturated adsorption test experiment shown in Example 4, had a saturated adsorption capacity of Au 2+. 3+ The saturated adsorption capacity of Au was 2664 mg / g. When the mass ratio of metal organic framework nanoparticles to tannic acid was 1:6, 3+ The saturated adsorption capacity of the prepared HNPC was slightly increased to 2669 mg / g; when the mass ratio of metal organic framework nanoparticles to tannic acid was 1:3 (other preparation conditions were the same as those in Example 1), when the adsorption capacity test experiment shown in Example 4 was performed, Au 3+ The saturated adsorption capacity is 2001 mg / g. When the mass ratio of metal organic framework nanoparticles to tannic acid is 1:7, Au 3+ The saturated adsorption capacity is 1994 mg / g. The role of tannic acid is to etch the metal organic framework nanoparticles to produce a hollow structure. Its role in HNPC is to make the hollow carbon nanoparticle material have a hollow structure. Different concentrations of tannic acid will affect the hollow morphology, hollow degree and porosity of HNPC. It can be seen that the morphology and pore structure of the hollow structure in the hollow carbon nanoparticle material will have a greater impact on the adsorption of gold ions in the hollow carbon nanoparticle material. Studies have shown that when the mass ratio of metal organic framework nanoparticles to tannic acid is between 1:4 and 1:6, the hollow structure and porosity formed are most conducive to the adsorption of gold ions. Therefore, the hollow carbon nanoparticle material exhibits the best adsorption effect within this range.

[0051] In order to further verify the important role of the hollow structure and porosity of the hollow carbon nanoparticle material on the gold adsorption performance, this example compares the adsorption performance of non-hollow structure carbon nanomaterials. Specifically, we used the ZIF-8 material prepared in step (1) of Example 1 and treated it according to the calcination method of step (3) of Example 1 to obtain a carbon nanomaterial. The Raman spectrum test results showed that a graphene layer was successfully formed in the structure of the carbon nanomaterial. Subsequently, the carbon nanomaterial was subjected to the saturated adsorption test experiment shown in Example 4, and the results showed that its saturated adsorption capacity for Au³⁺ was only 1237 mg / g. Compared with the adsorption performance of the hollow carbon nanoparticle material, this result is significantly lower, indicating that the hollow structure and porosity play a key role in improving the adsorption capacity of the hollow carbon nanoparticle material for gold ions. This experiment further proves the importance of the hollow structure and graphene layer in optimizing the gold adsorption performance.

[0052] Secondly, by adjusting the stirring reaction time of preparing hollow metal organic framework nanoparticles in step (2), the preparation process of hollow carbon nanoparticle material was further optimized. The experimental results show that when the stirring time is 5 minutes, the prepared hollow carbon nanoparticle material shows a saturated adsorption capacity of Au³⁺ of 2665 mg / g in the saturated adsorption capacity test in Example 4; when the stirring time is shortened to 4 minutes, the saturated adsorption capacity decreases to 2341 mg / g; and when the stirring time is extended to 12 minutes, the saturated adsorption capacity increases slightly to 2669 mg / g. These results show that too short stirring time leads to incomplete acid etching, affecting the formation of the hollow structure, thereby reducing the adsorption performance of the material. When the stirring time is extended to 12 minutes, the adsorption capacity does not change much compared to 10 minutes, indicating that the acid etching is basically completed at 10 minutes, and further extending the stirring time has limited improvement on the adsorption performance. Therefore, combined with the stirring time in Example 1, the optimal stirring reaction time should be 5 to 10 minutes to ensure the full formation of the hollow structure and optimize the adsorption performance.

[0053] Furthermore, the temperature of the calcination treatment for preparing the hollow carbon nanoparticle material in step (3) was adjusted. It was found that when the calcination temperature was 700°C, the obtained hollow carbon nanoparticle material was subjected to the saturated adsorption test experiment shown in Example 4. 3+ The saturated adsorption capacity of Au is 2660 mg / g. When the calcination temperature is 1000℃, 3+ The saturated adsorption capacity is 2662 mg / g; when the calcination temperature is 600°C, the obtained hollow carbon nanoparticle material has fewer graphene layers, and the Raman spectrum shows that the degree of graphene is 0.31. The hollow carbon nanoparticle material is subjected to the saturated adsorption capacity test experiment shown in Example 4, Au 3+ The saturated adsorption capacity of Au was 1786 mg / g; when the calcination temperature was 1100℃, 3 + The saturated adsorption capacity is 1279 mg / g respectively. Analysis shows that the reason for the significant reduction in saturated adsorption capacity may be that the excessively high calcination temperature destroys the structure of nitrogen and oxygen doping, thereby affecting the adsorption capacity of the material. Therefore, the calcination treatment temperature in the range of 700°C to 1000°C can better balance the formation of the graphene layer and the stability of nitrogen and oxygen doping, thereby optimizing the adsorption performance of the hollow carbon nanoparticle material. Too low a temperature will lead to insufficient graphene layers, while too high a temperature will destroy the key doping structure, both of which are not conducive to maximizing the adsorption performance.

[0054] Finally, this example adjusts the gas atmosphere of the calcination treatment in step (3) to further optimize the preparation process of the hollow carbon nanoparticle material. When the calcination treatment gas atmosphere in step (3) of Example 1 was changed from inert gas nitrogen to air, it was found that the carbon material reacted in the air, causing the solid in the porcelain boat to completely disappear, and no product was obtained.

[0055] The commercial graphene and expanded graphite used in the examples of the present invention were purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd. The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0056] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. An application of a hollow carbon nanoparticle material as an adsorbent for adsorbing gold ions, characterized in that: The hollow carbon nanoparticle material is obtained by calcining metal organic framework nanoparticles with a hollow structure; The calcination process transforms the structure of the metal organic framework nanoparticles into a graphene layer.

2. The use according to claim 1, characterized in that: The metal organic framework nanoparticles are ZIF-8 nanoparticles.

3. The use according to claim 2, characterized in that: The calcination temperature is 700-1000°C.

4. The use according to claim 2, characterized in that: The calcination process is performed in an inert gas atmosphere.

5. The use according to any one of claims 1 to 4, characterized in that: The preparation method of the hollow carbon nanoparticle material comprises the following steps: Step S1: adding zinc nitrate hexahydrate and 2-methylimidazole into a solvent respectively, stirring to form nuclei, and obtaining metal organic framework nanoparticles; Step S2: dispersing the metal organic framework nanoparticles obtained in step S1 in a solvent, adding tannic acid, and stirring to react to obtain metal organic framework nanoparticles with a hollow structure; Step S3: taking the metal organic framework nanoparticles with a hollow structure obtained in step S2 and subjecting them to calcination treatment to transform and form a graphene layer in the structure of the nanoparticles.

6. The use according to claim 5, characterized in that: In step S1, the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole is 1:6-10.

7. The use according to claim 5, characterized in that: In step S2, the mass ratio of the metal organic framework nanoparticles to tannic acid is 1:4-6.

8. The use according to claim 5, characterized in that: In step S2, the stirring reaction is carried out at a rotation speed of 200 rpm to 600 rpm and for a time of 5 minutes to 10 minutes.

9. The use according to claim 5, characterized in that: In step S3, the calcination treatment is performed at a temperature of 700° C. to 1000° C. and for a time of 0.5 to 4 hours.

10. The use according to claim 5, characterized in that: In step S3, the calcination treatment is performed in an inert gas atmosphere.

Citation Information

Patent Citations

  • Solid-phase micro-extraction coating based on hollow carbon nanometer material and preparation method thereof

    CN108311125A

  • Preparation method and application of post-modified ZIF-8 material

    CN114307973A

  • Method of preparation of ultrathin metal-organic frameworks & uses thereof

    EP4368285A1

  • Monoclonal antibody for immunoassay of detergents and their degradation products and its use

    US6251612B1

Cited By

  • Shrimp shell derived carbon-based efficient gold ion adsorption material and preparation method thereof