Preparation method of shell-controllable magnetic agarose gel microspheres

The shell-controllable magnetic agarose gel microspheres prepared by the core-shell alternating coating method solve the problems of poor magnetic response performance and insufficient stability of magnetic microspheres in the prior art, and realize efficient magnetic separation and biological phase Capacity meets the application needs in medical and biological separation.

CN118904298AActive Publication Date: 2024-11-08JIMEI UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411157783.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing agarose magnetic microsphere preparation method cannot achieve the ideal magnetic particles with super paramagnetic properties, fast magnetic response speed, good chemical stability, narrow particle size distribution, monodispersion, high epoxy density, simple process and low cost. The comprehensive effect limits its application in medical and biological isolation and purification.

Method used

The core-shell alternating coating method is used to prepare micron-scale core agarose gel microspheres by emulsification under high-speed stirring, and the thickness and number of shells are controlled by spraying agarose and magnetic powder suspensions multiple times to form shells. Layer controllable magnetic agarose gel microspheres.

Benefits of technology

The superparamagnetic and high response speed of magnetic particles is achieved, the acid and alkali resistance and oxidation resistance of microspheres are improved, and the biocompatibility is ensured. The magnetic separation time and epoxy density are controlled by controlling the core-shell thickness to satisfy the Efficient magnetic separation and stable chemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904298A_ABST
    Figure CN118904298A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of shell layer controllable magnetic agarose gel microspheres. Adding a first agarose solution into the mixed oil phase under high-speed stirring to emulsify, stirring and cooling the emulsion, curing in an ice-water bath, demulsifying and washing to obtain agarose microspheres; putting into equipment, introducing air flow to enable the substrate to be in a suspended state, and spraying to enable a layer of agarose solution to be adhered; spraying the magnetic powder suspension to enable a layer of magnetic particles to be adhered; spraying again to enable a layer of agarose solution to be adhered again, and introducing air flow to guide the agarose magnetic microspheres into water to obtain magnetic agarose gel microspheres; wherein the spraying step is repeated as required. According to the prepared agarose gel microspheres, the magnetic separation time and epoxy group density of the agarose magnetic microspheres can be regulated and controlled, meanwhile, the acid and alkali resistance, oxidation resistance and other solvent resistance are remarkably improved, and the biocompatibility of magnetic cores is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of gel microspheres, and in particular to a method for preparing shell-controllable magnetic agarose gel microspheres. Background Art

[0002] Magnetic microspheres are a kind of multifunctional material widely used in the field of biomedicine. The core part gives it the separation function, and the outer biopolymer functional groups give it the function of carrier. It has broad application prospects in the fields of enzyme immobilization, immunoassay, cell separation, targeted drugs, chemical analysis, etc. Agarose is a linear, water-soluble natural polysaccharide extracted from seaweed. It is a polymer composed of 1,3-linked β-D-pyranose and 1,4-linked 3,6-anhydro-aL-pyranose residues connected alternately. Agarose gel as a matrix has the following advantages: rich in hydroxyl groups, after chemical activation, it can be coupled with various ligands; the multi-hole network structure is conducive to the diffusion of macromolecules in the beads, thereby increasing the effective density of ligands; it has good hydrophilicity, so that biological molecules can easily approach and interact with ligands without inactivating biological molecules; it is uncharged and has extremely low nonspecific adsorption capacity. Therefore, it is a good inert support for separation media.

[0003] At present, the preparation method of agarose magnetic microspheres is very limited, mainly using ultrasound, mechanical stirring, homogenizer emulsification and other methods. Patent CN1376730A discloses a method for preparing magnetic agarose composite microspheres, and magnetic agarose microspheres are obtained by dripping alkali solution into a mixed solution of agarose and ferrous chloride under mechanical stirring. The initial state of the mixed solution is a homogeneous system. As the magnetic particles precipitate, a layer of agarose is adsorbed on the surface of the particles, but it does not have sufficient ball-forming ability, and the particle size distribution of the microspheres is wide and non-spherical. Patent CN1316450A discloses a method for preparing magnetic agarose microspheres by an oil-water two-phase method, directly dispersing rubidium iron boron particles in an agarose solution, adding them to the oil phase under stirring to form oil-in-water droplets, and obtaining agarose magnetic microspheres after cooling, cross-linking, curing, and washing. Using micron-sized rubidium iron boron alloy particles as magnetic materials to embed in agarose to form magnetic agarose microspheres, although the acid and alkali resistance and oxidation resistance are improved, the particles are large in size and density, very easy to settle, and easy to magnetize in a magnetic field and have remanence, resulting in easy agglomeration and difficult dispersion between magnetic agarose microspheres; Patent CN104587977A discloses a method for preparing agarose magnetic microspheres modified by surface carboxylation, characterized in that W / O-type agarose microspheres are first prepared, iron ions are adsorbed after activation and cross-linking, and agarose microspheres containing magnetic particles are prepared through ammonia precipitation. Due to the free diffusion of iron salt ions into the interior of agarose microspheres or adsorption on the surface of microspheres, the magnetic particles loaded by the microspheres are less, and the magnetic response speed is slow during the application process. In addition, when the surface of agarose magnetic microspheres needs to be connected to different types of ligands, it is often necessary for the surface of agarose magnetic microspheres to contain a high density of epoxy groups, therefore, the epoxy group density is particularly important for the application expansion of agarose magnetic microspheres. In order to enhance the high magnetic responsiveness, agarose magnetic microspheres currently prepared by the emulsion solidification method need to add high concentrations of magnetic cores, which results in a thinner agarose shell and reduces the hydroxyl content of agarose, that is, the epoxy density decreases.

[0004] Ideal agarose magnetic microspheres and production methods should have the following characteristics: 1) Magnetic particles should have superparamagnetism and no residual magnetism; 2) Microspheres have high magnetic content and fast magnetic response speed; 3) Microspheres have good chemical stability, acid resistance, alkali resistance, and oxidation resistance, no magnetic particles or iron ions are precipitated, and no pollution; 4) Microsphere particle size distribution is narrow and monodisperse; 5) Agarose magnetic microspheres have a high epoxy group density; 6) The process is simple, the production cost is low, the repeatability is good, and it is easy to mass produce. From the above preparation methods reported in existing patents, it is not difficult to find that there is no existing method that can prepare agarose magnetic microspheres that can meet the requirements of ideal microspheres, which also limits the wide application of agarose magnetic microspheres in medical and biological separation and purification. Therefore, it is necessary to provide a method for preparing agarose magnetic microspheres to solve the above problems. Summary of the invention

[0005] The invention improves the traditional method of coating magnetic particles with agarose, and improves the traditional direct coating method to a core-shell alternating coating method, aiming to provide a method for preparing magnetic agarose gel microspheres with controllable shells.

[0006] To achieve the above object, the present invention provides a method for preparing shell-controllable magnetic agarose gel microspheres, characterized in that it comprises the following steps:

[0007] S1. Preparation of micron-sized core agarose gel microspheres:

[0008] The first agarose solution is added to the mixed oil phase of Span 80 and liquid paraffin under high-speed stirring conditions for emulsification under high-speed stirring. After the emulsification is completed, the emulsion is cooled to room temperature under stirring conditions and then solidified in an ice water bath; after the solidification is completed, the emulsion is broken; the lower layer of precipitate is added with distilled water for multiple washing to obtain the first agarose microspheres;

[0009] S2. Preparation of shell-controllable magnetic agarose gel microspheres:

[0010] The obtained first agarose microspheres are placed in the device, and the first airflow is introduced to make the first agarose microspheres in a suspended state, and then the second agarose solution is sprayed into the reaction chamber to make a layer of agarose solution adhere to the surface of the first agarose microspheres; the magnetic powder suspension is sprayed into the reaction chamber of the device to make another layer of magnetic particles adhere to the surface of the first agarose microspheres; the third agarose solution is sprayed into the reaction chamber to make another layer of agarose solution adhere to the outermost surface of the agarose microspheres, and then the second airflow is introduced to introduce the agarose magnetic microspheres into deionized water to obtain magnetic agarose gel microspheres; wherein, the first agarose microspheres are sprayed with the second agarose solution, and the magnetic powder suspension and the second agarose solution are repeatedly applied as needed.

[0011] Further, in the step S1, the concentration of the first agarose solution is 2 to 6 w / v%; and / or

[0012] The Span80 concentration is 1-5 w / v%.

[0013] Furthermore, in step S1, the water-to-oil ratio in the emulsified system is 1:10 to 9:10; and / or

[0014] The emulsification under high-speed stirring is upper stirring emulsification and lower stirring emulsification; wherein the rate of the upper stirring emulsification is 16000rpm-24000rpm, and the rate of the lower stirring emulsification is 800rpm-1600rpm; and / or

[0015] The emulsification temperature is 70-100° C. and the emulsification time is 5-30 minutes.

[0016] Further, in the step S1, the stirring rate of the curing is 800 rpm to 1200 rpm; and / or

[0017] The particle size of the first agarose microspheres is 1 to 10 μm.

[0018] Further, in the step S2, the concentration of the second agarose solution is 0.1 w / v% to 0.5 w / v%; and / or

[0019] The concentration of the magnetic powder suspension is 5 w / v% to 20 w / v%; and / or

[0020] The concentration of the third agarose solution is 2 w / v% to 6 w / v%.

[0021] Furthermore, in the step S2, the magnetic powder in the magnetic powder suspension is at least one of ferroferric oxide powder and ferrous oxide powder; and / or

[0022] The magnetic powder has a particle size of 10 to 100 nm and a shape of rod, polyhedron or hollow sphere; and / or

[0023] The magnetic saturation intensity of the magnetic powder is greater than 80emu / g.

[0024] Furthermore, in the step S2, the temperature of the first airflow is 60-100° C.; and / or

[0025] The spraying temperature of the second agarose solution is 60-100° C.; and / or

[0026] The spray temperature of the magnetic powder suspension is 90 to 120°C; and / or

[0027] The spray temperature of the third agarose solution is 80-100° C.; and / or

[0028] The temperature of the second air flow is 0-25°C.

[0029] In S2 of the present invention, the second agarose solution, the magnetic powder suspension and the third agarose solution are sprayed repeatedly once, and the particle size of the agarose magnetic microspheres increases by 20 to 40 μm. Therefore, the number of repetitions can be selected according to needs.

[0030] The agarose magnetic microspheres prepared by the invention have a particle size of 20 to 150 μm and a magnetic separation time of less than 10 seconds.

[0031] Compared with the existing technology, the present invention has the following advantages:

[0032] The present invention adopts superparamagnetic Fe3O4 particles or Fe2O3 particles with high saturation magnetization as magnetic material, and improves the problem that the magnetic agarose microspheres prepared by the original technology have poor magnetic response performance or are easy to generate residual magnetism in the magnetic field; by introducing a shell layer with good chemical inertness, hydrophilicity and biocompatibility on the surface of the magnetic Fe3O4 or Fe2O3, the acid and alkali resistance, oxidation resistance and other solvent resistance of the magnetic agarose are significantly improved, and the biocompatibility of the magnetic core is improved, ensuring that the entire magnetic agarose microsphere has good biocompatibility. By controlling the thickness and number of core-shell layers, the magnetic separation time and epoxy group density of the agarose magnetic microspheres can be adjusted. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the result diagram obtained in Comparative Example 1.

[0034] Figure 2 This is the result diagram obtained from Comparative Example 2.

[0035] Figure 3 This is the result diagram obtained from Comparative Example 3.

[0036] Figure 4 This is a graph showing the results obtained in Example 1.

[0037] Figure 5 This is the result diagram obtained in Example 2.

[0038] Figure 6 This is a graph showing the results obtained in Example 3.

[0039] Figure 7 This is a graph showing the results obtained in Example 4.

[0040] Figure 8 This is a graph showing the results obtained in Example 5.

[0041] Fig. 9 This is a graph showing the results obtained in Example 6.

[0042] Fig.10 This is a graph showing the results obtained in Example 7.

[0043] Fig.11 The present invention is a flow chart for preparing shell-controllable magnetic agarose gel microspheres. DETAILED DESCRIPTION

[0044] Embodiments of the present invention are described in detail below, and the examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements with the same or similar functions from beginning to end. The embodiments described below by reference to the accompanying drawings are exemplary, are intended to be used to explain the present invention, and are not to be construed as limitations of the present invention. Those who do not indicate specific techniques or conditions in the embodiments are carried out according to the techniques or conditions described in the documents in this area or according to the product specification. Those who do not indicate the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially.

[0045] A method for preparing shell-controllable magnetic agarose gel microspheres, characterized in that it comprises the following steps:

[0046] S1. Preparation of micron-sized core agarose gel microspheres:

[0047] The first agarose solution is added to the mixed oil phase of Span 80 and liquid paraffin under high-speed stirring conditions for emulsification under high-speed stirring. After the emulsification is completed, the emulsion is cooled to room temperature under stirring conditions and then solidified in an ice water bath; after the solidification is completed, the emulsion is broken; the lower layer of precipitate is added with distilled water for multiple washing to obtain the first agarose microspheres;

[0048] S2. Preparation of shell-controllable magnetic agarose gel microspheres:

[0049] The obtained first agarose microspheres are placed in the device, and the first airflow is introduced to make the first agarose microspheres in a suspended state, and then the second agarose solution is sprayed into the reaction chamber to make a layer of agarose solution adhere to the surface of the first agarose microspheres; the magnetic powder suspension is sprayed into the reaction chamber of the device to make another layer of magnetic particles adhere to the surface of the first agarose microspheres; the third agarose solution is sprayed into the reaction chamber to make another layer of agarose solution adhere to the outermost surface of the agarose microspheres, and then the second airflow is introduced to introduce the agarose magnetic microspheres into deionized water to obtain magnetic agarose gel microspheres; wherein, the first agarose microspheres are sprayed with the second agarose solution, and the magnetic powder suspension and the second agarose solution are repeatedly applied as needed.

[0050] Further, in the step S1, the concentration of the first agarose solution is 2 to 6 w / v%; and / or

[0051] The Span80 concentration is 1-5 w / v%.

[0052] Furthermore, in step S1, the water-to-oil ratio in the emulsified system is 1:10 to 9:10; and / or

[0053] The emulsification under high-speed stirring is upper stirring emulsification and lower stirring emulsification; wherein the rate of the upper stirring emulsification is 16000rpm-24000rpm, and the rate of the lower stirring emulsification is 800rpm-1600rpm; and / or

[0054] The emulsification temperature is 70-100° C. and the emulsification time is 5-30 minutes.

[0055] Further, in the step S1, the stirring rate of the curing is 800 rpm to 1200 rpm; and / or

[0056] The particle size of the first agarose microspheres is 1 to 10 μm.

[0057] Further, in the step S2, the concentration of the second agarose solution is 0.1 w / v% to 0.5 w / v%; and / or

[0058] The concentration of the magnetic powder suspension is 5 w / v% to 20 w / v%; and / or

[0059] The concentration of the third agarose solution is 2 w / v% to 6 w / v%.

[0060] Furthermore, in the step S2, the magnetic powder in the magnetic powder suspension is at least one of ferroferric oxide powder and ferrous oxide powder; and / or

[0061] The magnetic powder has a particle size of 10 to 100 nm and a shape of rod, polyhedron or hollow sphere; and / or

[0062] The magnetic saturation intensity of the magnetic powder is greater than 80emu / g.

[0063] Furthermore, in the step S2, the temperature of the first airflow is 60-100° C.; and / or

[0064] The spraying temperature of the second agarose solution is 60-100° C.; and / or

[0065] The spray temperature of the magnetic powder suspension is 90 to 120°C; and / or

[0066] The spray temperature of the third agarose solution is 80-100° C.; and / or

[0067] The temperature of the second air flow is 0-25°C.

[0068] The process flow chart of the preparation of the shell-controllable magnetic agarose gel microspheres of the present invention is shown in Fig.11 The following examples are combined Fig.11 conduct.

[0069] The method for determining the epoxy content of magnetic microspheres in the following experiment is as follows: weigh 7.5g of agarose magnetic microspheres into a wide-mouth conical flask, add 4mL of 5M sodium hydroxide solution and 6mL of deionized water and shake to mix, then add 4mL of epichlorohydrin and 4mL of 1,4-dioxane in sequence, seal the flask, place it in a 30-degree Celsius shaker for activation for a certain period of time, then take it out, wash it with deionized water and drain the microspheres. Weigh 1.0g of the cross-linked activated microsphere sample, add 2-3 drops of phenolphthalein, add 3mL of 1.3 mol / L sodium thiosulfate solution, react in a shaker for 30 minutes, titrate with 0.01mol / L hydrochloric acid, and record the data. The calculation formula is Q (μmol / g) = c 盐酸 (v0-v1) / m 磁球 *1000.

[0070] Magnetic separation time of magnetic beads: Accurately weigh 0.1g sample powder, add 10mL water into a 10mL glass bottle, and after sufficient ultrasonic dispersion, place a magnet vertically on one side of the glass bottle, and calculate the time it takes for the solution to change from turbid to clear.

[0071] Comparative Example 1: A method for preparing agarose magnetic microspheres

[0072] The following steps are involved:

[0073] S1: adding agarose to 40 mL of distilled water to form a suspension, dissolving the agarose suspension into a 4% (w / v) homogeneous solution by heating; using 200 mL of liquid paraffin as the oil phase, adding 1.5% (w / v) Span 80 to the oil phase to obtain a mixed oil phase; adding the agarose solution to the mixed oil phase;

[0074] 6g of polyhedral magnetic powder was dispersed in 20mL of distilled water, and the magnetic powder was slowly poured into the agarose solution (i.e., the agarose solution was added to the mixed oil phase), and the emulsification temperature was adjusted to 80°C, and the emulsification was carried out under stirring at an emulsification rate of 1200rpm for 20min. After the emulsification was completed, the emulsion was cooled to room temperature at 500rpm, and then solidified in an ice water bath for a period of time; after the solidification was completed, the emulsion was demulsified. The lower layer of sediment was added to distilled water for multiple washings to obtain the finished product of about 100μm agarose magnetic microspheres ( Figure 1 ).

[0075] The magnetic separation time of the magnetic microspheres was measured to be 42 s, and the epoxy content of the magnetic microspheres was 60 μmol / g.

[0076] Comparative Example 2: A method for preparing agarose magnetic microspheres

[0077] The following steps are involved:

[0078] Agarose was added to 40 mL of distilled water to form a suspension, and the agarose suspension was dissolved into a 4% (w / v) homogeneous solution by heating; 200 mL of liquid paraffin was used as the oil phase, and 1.5% (w / v) Span 80 was added to the oil phase to obtain a mixed oil phase; the agarose solution was added to the mixed oil phase;

[0079] Disperse 15g of polyhedral magnetic powder in 20mL of distilled water, slowly pour the magnetic powder into the agarose solution (i.e., add the agarose solution to the mixed oil phase), adjust the emulsification temperature to 80°C, stir and emulsify at an emulsification rate of 1200rpm for 20min, and after the emulsification is completed, cool the emulsion to room temperature at 500rpm, and then use an ice water bath to solidify for a period of time; after the solidification is completed, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of about 100μm agarose magnetic microspheres ( Figure 2 ).

[0080] The magnetic separation time of the magnetic microspheres was measured to be 8.5 s, and the epoxy content of the magnetic microspheres was 24 μmol / g.

[0081] Comparative Example 3: Preparation method of agarose magnetic microspheres with controllable shell

[0082] The following steps are involved:

[0083] S1. Add agarose to distilled water to form a suspension, and dissolve the agarose suspension into a 2% (w / v) homogeneous solution by heating; use liquid paraffin as the oil phase, add 1% (w / v) Span 80 to the oil phase to obtain a mixed oil phase, and add the agarose solution to the mixed oil phase;

[0084] The emulsification temperature was adjusted to 70°C, the emulsification rate was 800 rpm at the bottom and 16000 rpm at the top, and the emulsification time was 5 minutes. After the emulsification, the emulsion was cooled to room temperature at 800 rpm, and then solidified in an ice water bath for a period of time; after the solidification, the emulsion was broken. The lower layer of precipitate was added with distilled water for multiple washings to obtain the finished product 1 μm agarose microspheres.

[0085] S2, 1 μm agarose microspheres are placed in the device, and an air flow at a temperature of 60°C is introduced to suspend the agarose microspheres, and a 0.1% (w / v) agarose solution 1 is sprayed into the reaction chamber at a spray temperature of 60°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, and a rod-shaped ferroferric oxide suspension with a magnetic saturation intensity of 82emu / g, a length of 100nm, and a concentration of 5% (w / v) is sprayed into the reaction chamber, and the spray temperature of the magnetic fluid is 90°C, so that magnetic particles adhere to the surface of the agarose microspheres, and 2% (w / v) agarose solution 2 is sprayed into the reaction chamber at a spray temperature of 80°C, so that a layer of agarose solution adheres to the surface of the agarose magnetic microspheres, and the air flow temperature is adjusted to 25°C, and the agarose magnetic microspheres are introduced into deionized water for collection to obtain agarose magnetic microspheres with a particle size of about 20 μm ( Figure 3 ).

[0086] It was determined that the magnetic separation time of the magnetic microspheres was 42 s, and the epoxy content of the magnetic microspheres was 66 μmol / g.

[0087] Example 1: Preparation method of agarose magnetic microspheres with controllable shell

[0088] The following steps are involved:

[0089] S1. Add agarose to distilled water to form a suspension, dissolve the agarose suspension into a homogeneous solution with a concentration of 2% (w / v) by heating; use liquid paraffin as the oil phase, add 1% (w / v) Span 80 to the oil phase, add the agarose solution to the mixed oil phase, adjust the emulsification temperature to 70°C, stir the emulsification rate at 800rpm at the bottom, stir the emulsification rate at 16000rpm at the top, emulsify for 5 minutes, and after the emulsification is completed, cool the emulsion to room temperature at 800rpm, and then use an ice water bath to solidify for a period of time; after the solidification is completed, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of 1μm agarose microspheres.

[0090] S2, 1 μm agarose microspheres are placed in the device, and an air flow at a temperature of 60°C is introduced to suspend the agarose microspheres, and a 0.1% (w / v) agarose solution 1 is sprayed into the reaction chamber at a spray temperature of 60°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, and a rod-shaped ferroferric oxide suspension with a magnetic saturation intensity of 82emu / g, a length of 100nm, and a concentration of 10% (w / v) is sprayed into the reaction chamber, and the spray temperature of the magnetic fluid is 90°C, so that magnetic particles adhere to the surface of the agarose microspheres, and 2% (w / v) agarose solution 2 is sprayed into the reaction chamber at a spray temperature of 80°C, so that a layer of agarose solution adheres to the surface of the agarose magnetic microspheres, and the air flow temperature is adjusted to 25°C, and the agarose magnetic microspheres are introduced into deionized water for collection to obtain agarose magnetic microspheres with a particle size of about 20 μm ( Figure 4 ).

[0091] It was determined that the magnetic separation time of the magnetic microspheres was less than 10 s, and the epoxy content of the magnetic microspheres was 80 μmol / g.

[0092] Example 2: Preparation method of agarose magnetic microspheres with controllable shell

[0093] The following steps are involved:

[0094] S1. Add agarose to distilled water to form a suspension, dissolve the agarose suspension into a homogeneous solution with a concentration of 2% (w / v) by heating; use liquid paraffin as the oil phase, add 1% (w / v) Span 80 to the oil phase, add the agarose solution to the mixed oil phase, adjust the emulsification temperature to 70°C, stir the emulsification rate at 800rpm at the bottom, stir the emulsification rate at 16000rpm at the top, emulsify for 5 minutes, and after the emulsification is completed, cool the emulsion to room temperature at 800rpm, and then use an ice water bath to solidify for a period of time; after the solidification is completed, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of 1μm agarose microspheres.

[0095] S2. Place 1 μm agarose microspheres in the equipment, introduce air flow at a temperature of 60°C to suspend the agarose microspheres, spray 0.1% (w / v) agarose solution 1 into the reaction chamber at a spray temperature of 60°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, spray a rod-shaped ferroferric oxide suspension with a magnetic saturation intensity of 82emu / g, a particle size of 20nm, and a concentration of 10% (w / v) into the reaction chamber, and spray the magnetic fluid at a spray temperature of 90°C to adhere magnetic particles to the surface of the agarose microspheres, and spray 2% (w / v) agarose solution 2 into the reaction chamber at a spray temperature of 80°C to adhere a layer of agarose solution to the surface of the agarose magnetic microspheres.

[0096] A rod-shaped ferroferric oxide suspension with a magnetic saturation strength of 82emu / g, a particle size of 20nm, and a concentration of 5% (w / v) was sprayed into the reaction chamber. The spray temperature of the magnetic fluid was 90°C, so that the magnetic particles adhered to the surface of the agarose microspheres again. A 2% (w / v) agarose solution 2 was sprayed into the reaction chamber at a spray temperature of 80°C, so that a layer of agarose solution adhered to the surface of the agarose magnetic microspheres. The air flow temperature was adjusted to 25°C, and the agarose magnetic microspheres were introduced into deionized water for collection to obtain a particle size of about 45μm ( Figure 5 ).

[0097] It was determined that the magnetic separation time of the magnetic microspheres was less than 10 s and the epoxy content of the magnetic microspheres was 76 μmol / g.

[0098] Example 3: Preparation method of agarose magnetic microspheres with controllable shell

[0099] The following steps are involved:

[0100] S1. Add agarose to distilled water to form a suspension, dissolve the agarose suspension into a homogeneous solution with a concentration of 4% (w / v) by heating; use liquid paraffin as the oil phase, add 2.5% (w / v) Span 80 to the oil phase, add the agarose solution to the mixed oil phase, adjust the emulsification temperature to 80°C, stir the emulsification rate at 1000rpm and the emulsification rate at 18000rpm, emulsify for 10 minutes, and place the emulsion at 900rpm to cool to room temperature after emulsification, and then use an ice water bath to solidify for a period of time; after solidification, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of 6μm agarose microspheres.

[0101] S2, 6 μm agarose microspheres are placed in the device, and an air flow at a temperature of 80°C is introduced to make the agarose microspheres in a suspended state, and a 0.2% (w / v) agarose solution 1 is sprayed into the reaction chamber at a spray temperature of 80°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, and a polyhedral ferroferric oxide suspension with a magnetic saturation intensity of 85emu / g, a particle size of 30nm, and a concentration of 15% (w / v) is sprayed into the reaction chamber, and the spray temperature of the magnetic fluid is 100°C, so that magnetic particles adhere to the surface of the agarose microspheres, and 4% (w / v) agarose solution 2 is sprayed into the reaction chamber at a spray temperature of 90°C, so that a layer of agarose solution adheres to the surface of the agarose magnetic microspheres, and the air flow temperature is adjusted to 20°C, and the agarose magnetic microspheres are introduced into deionized water for collection to obtain agarose magnetic microspheres with a particle size of 30 μm ( Figure 6 ).

[0102] It was determined that the magnetic separation time of the magnetic microspheres was less than 10 s, and the epoxy content of the magnetic microspheres was 72 μmol / g.

[0103] Example 4: Preparation method of agarose magnetic microspheres with controllable shell

[0104] The following steps are involved:

[0105] S1. Add agarose to distilled water to form a suspension, dissolve the agarose suspension into a homogeneous solution with a concentration of 4% (w / v) by heating; use liquid paraffin as the oil phase, add 2.5% (w / v) Span 80 to the oil phase, add the agarose solution to the mixed oil phase, adjust the emulsification temperature to 80°C, stir the emulsification rate at 1000rpm and the emulsification rate at 18000rpm, emulsify for 10 minutes, and place the emulsion at 900rpm to cool to room temperature after emulsification, and then use an ice water bath to solidify for a period of time; after solidification, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of 6μm agarose microspheres.

[0106] S2. Place 6 μm agarose microspheres in the equipment, pass an air flow at a temperature of 80°C to suspend the agarose microspheres, spray 0.2% (w / v) agarose solution 1 into the reaction chamber at a spray temperature of 80°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, spray a polyhedral ferrosoferric oxide suspension with a magnetic saturation intensity of 85emu / g, a particle size of 30nm, and a concentration of 10% (w / v) into the reaction chamber, and spray the magnetic fluid at a spray temperature of 100°C to adhere magnetic particles to the surface of the agarose microspheres, spray 4% (w / v) agarose solution 2 into the reaction chamber at a spray temperature of 90°C to adhere a layer of agarose solution to the surface of the agarose magnetic microspheres.

[0107] A polyhedral ferroferric oxide suspension with a magnetic saturation strength of 85emu / g, a particle size of 30nm, and a concentration of 10% (w / v) was sprayed into the reaction chamber. The spray temperature of the magnetic fluid was 100°C, so that the magnetic particles adhered to the surface of the agarose microspheres again. A 4% (w / v) agarose solution 2 was sprayed into the reaction chamber. The spray temperature was 90°C, so that a layer of agarose solution adhered to the surface of the agarose magnetic microspheres. The air flow temperature was adjusted to 20°C, and the agarose magnetic microspheres were introduced into deionized water for collection to obtain agarose magnetic microspheres with a particle size of about 60μm ( Figure 7 ).

[0108] It was determined that the magnetic separation time of the magnetic microspheres was less than 10 s, and the epoxy content of the magnetic microspheres was 66 μmol / g.

[0109] Example 5: Preparation method of agarose magnetic microspheres with controllable shell

[0110] The following steps are involved:

[0111] S1. Add agarose to distilled water to form a suspension, dissolve the agarose suspension into a homogeneous solution with a concentration of 6% (w / v) by heating; use liquid paraffin as the oil phase, add 4% (w / v) Span 80 to the oil phase, add the agarose solution to the mixed oil phase, adjust the emulsification temperature to 90°C, stir the emulsification rate at 1200rpm and the emulsification rate at 24000rpm, emulsify for 30 minutes, and place the emulsion at 1000rpm to cool to room temperature, and then use an ice water bath to solidify for a period of time; after solidification, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of 10μm agarose microspheres.

[0112] S2, placing 10 μm agarose microspheres in the equipment, passing an airflow at a temperature of 90°C to suspend the agarose microspheres, spraying a 0.5% (w / v) agarose solution 1 into the reaction chamber, the spraying temperature is 90°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, spraying a hollow spherical ferroferric oxide suspension with a magnetic saturation intensity of 90emu / g, a particle size of 100nm, and a concentration of 20% (w / v) into the reaction chamber, the spraying temperature of the magnetic fluid is 110°C, so that magnetic particles adhere to the surface of the agarose microspheres, spraying 6% (w / v) agarose solution 2 into the reaction chamber, the spraying temperature is 100°C, so that a layer of agarose solution adheres to the surface of the agarose magnetic microspheres, adjusting the airflow temperature to 10°C, introducing the agarose magnetic microspheres into deionized water for collection, and obtaining a particle size of 40 μm ( Figure 8 ).

[0113] It was determined that the magnetic separation time of the magnetic microspheres was less than 10 s, and the epoxy content of the magnetic microspheres was 68 μmol / g.

[0114] Example 6: Preparation method of agarose magnetic microspheres with controllable shell

[0115] The following steps are involved:

[0116] S1. Add agarose to distilled water to form a suspension, dissolve the agarose suspension into a homogeneous solution with a concentration of 6% (w / v) by heating; use liquid paraffin as the oil phase, add 4% (w / v) Span 80 to the oil phase, add the agarose solution to the mixed oil phase, adjust the emulsification temperature to 90°C, stir the emulsification rate at 1200rpm and the emulsification rate at 24000rpm, emulsify for 30 minutes, and place the emulsion at 1000rpm to cool to room temperature, and then use an ice water bath to solidify for a period of time; after solidification, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of 10μm agarose microspheres.

[0117] S2. Place 10 μm agarose microspheres in the equipment, introduce air flow at a temperature of 90°C to suspend the agarose microspheres, spray 0.5% (w / v) agarose solution 1 into the reaction chamber at a spray temperature of 90°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, spray a hollow spherical ferroferric oxide suspension with a magnetic saturation intensity of 90emu / g, a particle size of 100nm, and a concentration of 5% (w / v) into the reaction chamber, and spray the magnetic fluid at a spray temperature of 110°C, so that magnetic particles adhere to the surface of the agarose microspheres, and spray 6% (w / v) agarose solution 2 into the reaction chamber at a spray temperature of 100°C, so that a layer of agarose solution adheres to the surface of the agarose magnetic microspheres.

[0118] A hollow spherical ferroferric oxide suspension with a magnetic saturation strength of 90emu / g, a particle size of 100nm, and a concentration of 20% (w / v) was sprayed into the reaction chamber. The spray temperature of the magnetic fluid was 110°C, so that the magnetic particles adhered to the surface of the agarose microspheres. A 6% (w / v) agarose solution 2 was sprayed into the reaction chamber. The spray temperature was 100°C, so that a layer of agarose solution adhered to the surface of the agarose magnetic microspheres. The air flow temperature was adjusted to 10°C, and the agarose magnetic microspheres were introduced into deionized water for collection to obtain agarose magnetic microspheres with a particle size of 80μm ( Fig. 9 ).

[0119] It was determined that the magnetic separation time of the magnetic microspheres was less than 10 s, and the epoxy content of the magnetic microspheres was 77 μmol / g.

[0120] Example 7: Preparation method of agarose magnetic microspheres with controllable shell

[0121] The following steps are involved:

[0122] S1. Add agarose to distilled water to form a suspension, dissolve the agarose suspension into a homogeneous solution with a concentration of 6% (w / v) by heating; use liquid paraffin as the oil phase, add 4% (w / v) Span 80 to the oil phase, add the agarose solution to the mixed oil phase, adjust the emulsification temperature to 90°C, stir the emulsification rate at 1200rpm and the emulsification rate at 24000rpm, emulsify for 30 minutes, and after the emulsification is completed, cool the emulsion to room temperature at 1200rpm, and then use an ice water bath to solidify for a period of time; after the solidification is completed, demulsify. Add distilled water to the lower precipitate and wash it several times to obtain a finished product of 10μm agarose microspheres.

[0123] S2. Place 10 μm agarose microspheres in the equipment, introduce air flow at a temperature of 100°C to suspend the agarose microspheres, spray 0.5% (w / v) agarose solution 1 into the reaction chamber at a spray temperature of 100°C, so that a layer of agarose solution adheres to the surface of the agarose microspheres, spray a hollow spherical ferric oxide suspension with a magnetic saturation intensity of 82emu / g, a particle size of 50nm, and a concentration of 5% (w / v) into the reaction chamber, and spray the magnetic fluid at a spray temperature of 120°C to adhere magnetic particles to the surface of the agarose microspheres, and spray 6% (w / v) agarose solution 2 into the reaction chamber at a spray temperature of 100°C to adhere a layer of agarose solution to the surface of the agarose magnetic microspheres.

[0124] First repetition: a rod-shaped ferroferric oxide suspension with a magnetic saturation intensity of 85emu / g, a length of 150nm and a concentration of 10% (w / v) was sprayed into the reaction chamber, and the spray temperature of the magnetic fluid was 110°C, so that the magnetic particles adhered to the surface of the agarose microspheres. A 6% (w / v) agarose solution 2 was sprayed into the reaction chamber, and the spray temperature was 100°C, so that a layer of agarose solution adhered to the surface of the agarose magnetic microspheres.

[0125] Second repetition: a polyhedral ferroferric oxide suspension with a magnetic saturation strength of 90emu / g, a particle size of 100nm, and a concentration of 10% (w / v) was sprayed into the reaction chamber. The spray temperature of the magnetic fluid was 110°C, so that the magnetic particles adhered to the surface of the agarose microspheres. A 6% (w / v) agarose solution 2 was sprayed into the reaction chamber. The spray temperature was 100°C, so that a layer of agarose solution adhered to the surface of the agarose magnetic microspheres. The air flow temperature was adjusted to 0°C, so that the agarose solution on the surface of the agarose magnetic microspheres solidified rapidly, and agarose magnetic microspheres with a particle size of about 150μm were obtained ( Fig.10 ).

[0126] It was determined that the magnetic separation time of the magnetic microspheres was less than 10 s, and the epoxy content of the magnetic microspheres was 62 μmol / g.

[0127] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention.

Claims

1. A method for preparing shell-controllable magnetic agarose gel microspheres, characterized in that: The following steps are involved: S1. Preparation of micron-sized core agarose gel microspheres: The first agarose solution is added to the mixed oil phase of Span 80 and liquid paraffin under high-speed stirring conditions for emulsification under high-speed stirring. After the emulsification is completed, the emulsion is cooled to room temperature under stirring conditions and then solidified in an ice water bath; after the solidification is completed, the emulsion is demulsified; The lower layer of precipitate is added with distilled water and washed multiple times to obtain the first agarose microspheres; S2. Preparation of shell-controllable magnetic agarose gel microspheres: The obtained first agarose microspheres are placed in the device, a first airflow is introduced to make the first agarose microspheres suspended, and then a second agarose solution is sprayed into the reaction chamber to make a layer of agarose solution adhere to the surface of the first agarose microspheres; The magnetic powder suspension is sprayed into the reaction chamber of the equipment to make a layer of magnetic particles adhere to the surface of the first agarose microsphere; the third agarose solution is then sprayed into the reaction chamber to make a layer of agarose solution adhere to the outermost surface of the agarose microsphere, and then a second air flow is introduced to introduce the agarose magnetic microspheres into deionized water to obtain magnetic agarose gel microspheres; wherein the first agarose microspheres are sprayed with the second agarose solution, and the magnetic powder suspension and the second agarose solution are repeated as needed.

2. The preparation method according to claim 1, characterized in that In the step S1, the concentration of the first agarose solution is 2-6 w / v%; and / or The Span80 concentration is 1-5 w / v%.

3. The preparation method according to claim 1, characterized in that: In the step S1, the water-oil ratio in the emulsified system is 1:10 to 9:10; and / or The emulsification under high-speed stirring is upper stirring emulsification and lower stirring emulsification; wherein the rate of the upper stirring emulsification is 16000rpm-24000rpm, and the rate of the lower stirring emulsification is 800rpm-1600rpm; and / or The emulsification temperature is 70-100° C. and the emulsification time is 5-30 minutes.

4. The preparation method according to claim 1, characterized in that: In the step S1, the stirring rate of the curing is 800 rpm to 1200 rpm; and / or The particle size of the first agarose microspheres is 1 to 10 μm.

5. The preparation method according to claim 1, characterized in that: In the step S2, the concentration of the second agarose solution is 0.1 w / v% to 0.5 w / v%; and / or The concentration of the magnetic powder suspension is 5 w / v% to 20 w / v%; and / or The concentration of the third agarose solution is 2 w / v% to 6 w / v%.

6. The preparation method according to claim 1, characterized in that: In the step S2, the magnetic powder in the magnetic powder suspension is at least one of ferroferric oxide powder and ferrous oxide powder; and / or The magnetic powder has a particle size of 10 to 100 nm and a shape of rod, polyhedron or hollow sphere; and / or The magnetic saturation intensity of the magnetic powder is greater than 80emu / g.

7. The preparation method according to claim 1, characterized in that: In the step S2, the temperature of the first airflow is 60-100° C.; and / or The spraying temperature of the second agarose solution is 60-100° C.; and / or The spray temperature of the magnetic powder suspension is 90 to 120°C; and / or The spray temperature of the third agarose solution is 80-100° C.; and / or The temperature of the second air flow is 0-25°C.

Citation Information

Patent Citations

  • Preparation method of magnetic agarose bead

    CN103980519A

  • Preparation method of magnetic chitosan composite with adsorption characteristic

    CN108057423A

  • Preparation method of agar polysaccharide magnetic microspheres

    CN108912412A

  • Preparation method of chitosan-based magnetic microsphere adsorbent for efficiently adsorbing cationic dyes

    CN111111631A

  • Method for preparing super paramagnetic high polymer homogeneous microball

    CN1640921A