Preparation method of black niobium oxide photocatalytic material and product prepared by same
The preparation of NbOyHx+NbO2.5 biphase structure niobium oxide photocatalyst through solvent thermal reaction and hydrogen calcination method, solving the problems of reducing the bandwidth of niobium oxide band-extraction and improving the photocatalytic efficiency in the prior art, achieving efficient photocatalytic activity, and providing New preparation approach for black niobium oxide photocatalyst.
Patent Information
- Application Number
- CN202410953275.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The prior art is difficult to effectively reduce the band gap width of niobium oxide and improve its photocatalytic efficiency. Especially during the H doping process, the method of preparing black niobium oxide photocatalyst is relatively low, which is limited by the preparation process and conditions.
Using niobium oxide nanopowder, NbCl5 and NaH or CaH2 as raw materials, the NbHxCl5-x precursor was formed through solvent-thermal reaction, and calcined in a hydrogen atmosphere at low temperature to prepare black niobium oxide photocatalysis with NbOyHx+NbO2.5 biphasic structure Material.
The photocatalytic activity of niobium oxide is significantly improved, and the hydrogen evolution rate reaches 25 to 35 times that of pure NbO2.5. The preparation method is simple and fast, the conditions are mild, and it is easy to achieve.
Smart Images

Figure CN118904326A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalyst materials, and in particular to a method for preparing an H-doped black niobium oxide photocatalytic material and a product obtained therefrom. Background Art
[0002] Niobium oxide is a wide bandgap intrinsic semiconductor with a white powder appearance. It is a non-toxic and highly efficient photocatalyst that can decompose water to produce hydrogen or organic matter in the air (formaldehyde, toluene, etc.). In order to reduce the bandgap of niobium oxide and improve its photocatalytic efficiency so that it responds to visible light, people use various synthetic methods to prepare niobates (such as KNbO3, InNbO3), and use some ions to dope niobium oxide and test its effect. A large number of research results show that (1) wide bandgap niobates have very weak absorption of visible light; (2) doping niobium oxide with anions can effectively reduce its bandgap. For example, when N is doped into niobium oxide at a certain concentration, niobium oxide can appear yellow, which effectively improves its absorption rate of visible light; when H is doped into niobium oxide at a certain concentration, niobium oxide can be transformed into blue-gray (near black), and the bandgap of niobium oxide can be reduced to 0.5eV, which greatly improves the photoelectric conversion efficiency of niobium oxide. H-doped oxides, such as titanium oxide and niobium oxide, can not only improve the conductivity of oxides and significantly reduce the bandgap of oxides, but also significantly improve the photoelectric conversion efficiency of oxides. At present, the high-pressure hydrogen reaction method is widely used in industry to prepare hydrides, such as MgH2, CaH2, TiH2, and ZrH2. The use of high-pressure hydrogen to dope titanium oxide with H has achieved great success. The prepared black titanium oxide has good photocatalytic properties in the ultraviolet region. However, when this method is applied to niobium oxide materials, H doping is difficult to achieve (Nb-O chemical bonds are relatively stable). At present, a method for preparing black niobium oxide photocatalysts by palladium reduction has been reported abroad, but it is limited by the equipment or preparation conditions in the preparation process and has low efficiency. For this reason, it is necessary to seek a new method for preparing black niobium oxide photocatalysts that is simple, fast, and easy to implement. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a black niobium oxide photocatalytic material. The method uses niobium oxide nanopowder, NbCl5, NaH or CaH2 as raw materials, and reacts NbCl5 with NaH or CaH2 to form NbH x Cl 5-x The precipitate is uniformly deposited on the surface of nano-niobium oxide particles, and then after hydrolysis and ethanol washing, the resulting precipitate is low-temperature calcined in a hydrogen atmosphere to prepare NbO y H2+NbO 2.5The dual-phase structure niobium oxide photocatalytic material can significantly improve the photocatalytic activity of the niobium oxide material. Another object of the present invention is to provide a product prepared by the above preparation method.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] The present invention provides a method for preparing a black niobium oxide photocatalytic material, comprising the following steps:
[0006] (1) mixing niobium oxide nanopowder: NbCl5: NaH or CaH2: anhydrous toluene at a mass volume ratio of 10-30 g: 1-5 g: 0.2-1 g: 100-200 mL at room temperature to obtain a reaction solution;
[0007] (2) The reaction solution is placed in a reaction kettle, and a solvent thermal reaction is carried out at 180 to 220° C. for 5 to 15 hours to dissolve NbCl5 in anhydrous toluene and react with NaH or CaH2. After the reaction is completed, the mixture is filtered and collected to obtain NbH x Cl 5-x (x = 0.1-2) precursor powder uniformly deposited on the surface of niobium oxide particles;
[0008] (3) Add the precursor powder to an aqueous NH3 solution with a concentration of 0.5 to 2 mol / L to make NbH x Cl 5-x (x = 0.1-2) was hydrolyzed, and the obtained precipitate was washed with anhydrous ethanol and then moved to a hydrogen furnace for heat treatment at 250-350°C in a hydrogen atmosphere for 1-2 hours to obtain NbO y H x +NbO 2.5 (x=0.1~2) Dual-phase structure niobium oxide photocatalytic material.
[0009] The product prepared by the above-mentioned method for preparing black niobium oxide photocatalytic material, the NbO y H x +NbO 2.5 The hydrogen evolution rate of the dual-phase niobium oxide photocatalytic material in the photocatalytic water decomposition reaction is much faster than that of pure NbO 2.5 25 to 35 times of.
[0010] The present invention has the following beneficial effects:
[0011] The present invention uses a simple solvent thermal reaction and chemical precipitation method, changes the ratio of NbCl5, NaH or CaH2, and niobium oxide nanopowder in the reactants, and performs low-temperature calcination in a hydrogen atmosphere, thereby preparing a nano black niobium oxide photocatalyst with a dual-phase structure, and significantly improving the photocatalytic activity of niobium oxide. The preparation method of the present invention is simple and fast, has mild conditions, is easy to implement, and provides a new way to prepare black niobium oxide photocatalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:
[0013] Figure 1 The NbO prepared in the embodiment of the present invention y H2+NbO 2.5 Transmission electron microscope photo of dual-phase structure niobium oxide photocatalytic material;
[0014] Figure 2 It is pure NbO 2.5 and NbO y H 0.5 、NbO y H, NbO y XRD spectrum of H2;
[0015] Figure 3 is ω%NbO y H2+NbO 2.5 (ω=0,3,5) XRD spectra of dual-phase structure powders (ω=3: Example 1, Example 3; ω=5: Example 2);
[0016] Figure 4 The NbO prepared in the embodiment of the present invention y H2+NbO 2.5 High-resolution Nb3dXPS spectrum of dual-phase niobium oxide photocatalytic materials;
[0017] Figure 5 The NbO prepared in the embodiment of the present invention y H2+NbO 2.5 UV-visible absorption spectrum of dual-phase niobium oxide photocatalytic material. (3% NbO y H2+NbO 2.5 : Example 1, Example 3; 5% NbO y H2+NbO 2.5 :Example 2) DETAILED DESCRIPTION
[0018] Embodiment 1:
[0019] This embodiment provides a method for preparing a black niobium oxide photocatalytic material, and the steps are as follows:
[0020] (1) adding 13.3 g of niobium oxide nanopowder, 1.8 g of NbCl5, and 0.5 g of NaH into 100 mL of anhydrous toluene, and mixing at room temperature to obtain a reaction solution;
[0021] (2) the reaction solution is placed in a polytetrafluoroethylene-lined reactor, and moved to an oven to react at 180° C. for 10 h, so that NbCl5 is dissolved in anhydrous toluene and reacts with NaH. After the reaction is completed, the precursor powder is filtered and collected to obtain NbH2Cl3 uniformly deposited on the surface of niobium oxide particles;
[0022] (3) The above precursor powder was added to an NH3 aqueous solution with a concentration of 1 mol / L to hydrolyze NbH2Cl3. The resulting precipitate was washed with anhydrous ethanol and then moved to a hydrogen furnace for heat treatment at 300°C in a hydrogen atmosphere for 1 h to obtain NbO y H2+NbO 2.5 Dual-phase structured niobium oxide photocatalytic materials.
[0023] Embodiment 2:
[0024] This embodiment provides a method for preparing a black niobium oxide photocatalytic material, and the steps are as follows:
[0025] (1) adding 13.3 g of niobium oxide nanopowder, 3 g of NbCl5, and 0.8 g of NaH into 100 mL of anhydrous toluene, and mixing at room temperature to obtain a reaction solution;
[0026] (2) The reaction solution is placed in a polytetrafluoroethylene-lined reactor, and moved to an oven to react at 200° C. for 8 h to dissolve NbCl5 in anhydrous toluene and react with NaH. After the reaction is completed, the precursor powder is filtered and collected to obtain NbH2Cl3 uniformly deposited on the surface of niobium oxide particles;
[0027] (3) The above precursor powder was added to an NH3 aqueous solution with a concentration of 1 mol / L to hydrolyze NbH2Cl3. The resulting precipitate was washed with anhydrous ethanol and then moved to a hydrogen furnace for heat treatment at 350°C in a hydrogen atmosphere for 1.5 h to obtain NbO y H2+NbO 2.5 Dual-phase structured niobium oxide photocatalytic materials.
[0028] Embodiment three:
[0029] This embodiment provides a method for preparing a black niobium oxide photocatalytic material, and the steps are as follows:
[0030] (1) adding 13.3 g of niobium oxide nanopowder, 1.8 g of NbCl5, and 0.7 g of CaH2 into 100 mL of anhydrous toluene, and mixing at room temperature to obtain a reaction solution;
[0031] (2) the reaction solution is placed in a polytetrafluoroethylene-lined reactor, and moved to an oven to react at 220° C. for 8 h, so that NbCl5 is dissolved in anhydrous toluene and reacts with CaH2. After the reaction is completed, the precursor powder is filtered and collected to obtain NbH2Cl3 uniformly deposited on the surface of niobium oxide particles;
[0032] (3) The above precursor powder was added to an NH3 aqueous solution with a concentration of 1 mol / L to hydrolyze NbH2Cl3. The resulting precipitate was washed with anhydrous ethanol and then moved to a hydrogen furnace for heat treatment at 300°C in a hydrogen atmosphere for 2 h to obtain NbO y H2+NbO 2.5 Dual-phase structured niobium oxide photocatalytic materials.
[0033] NbO prepared in the embodiment of the present invention y H2+NbO 2.5 Dual-phase structure niobium oxide photocatalytic materials such as Figure 1 As shown, the test of its photocatalytic water decomposition reaction to produce hydrogen is as follows:
[0034] At 20°C, with a 300W xenon lamp as the light source, 100mL of 20% (volume ratio) methanol aqueous solution and 0.3g of catalyst were added to a 150mL quartz reactor, the distance between the light source and the quartz tube was 8cm, the stirring speed was 500rpm, and the light was turned on for 4h before sampling and analyzing the reaction raw materials and products by gas chromatography. The reaction data are listed in Table 1.
[0035] Table 1 Photocatalytic materials and pure NbO in the examples of the present invention 2.5 Photocatalytic hydrogen production activity
[0036]
[0037] The above results show that the hydrogen evolution rate of the niobium oxide photocatalytic material of the embodiment of the present invention is 2.5 25 to 35 times of.
[0038] Figure 2 Pure NbO shown 2.5 and NbO y H 0.5 、NbO y H, NbO y From the XRD spectrum of H2, we can see that pure NbO 2.5The crystal form is intact, and the diffraction peaks are consistent with the standard card JCPDS 005-0352; NbO prepared by solvent thermal assisted heat treatment 2.5- y H 0.5 、NbO 2.5-y The H crystal form is complete, and its diffraction peaks are consistent with the monoclinic NbO in the standard card (JCPDS 30–0872). 2.5 The diffraction peaks of (100), (011), (013), (113), and (202) crystal planes of NbO are consistent. This shows that H doping makes NbO 2.5 The crystal structure has changed. And with the increase of H doping, NbO 2.5 The crystal structure is gradually destroyed until an amorphous structure (such as NbO y H2). Figure 3 As shown, a small amount of amorphous NbO y H2 coated onto NbO 2.5 The surface of niobium oxide catalysts 2.5 The crystal structure was not affected.
[0039] like Figure 4 As shown, Nb 3d 5 / 2 and Nb 3d 3 / 2 The binding energies are 207.5eV and 210.1eV, respectively, indicating that Nb in the sample is +5. However, a small splitting peak can be clearly observed at about 206.2eV, which may be the Nb-H bond (Nb 3d 5 / 2 The binding energy is located at 203 eV). The UV-visible absorption spectrum of the product obtained in the embodiment of the present invention is as follows: Figure 5 As shown, it is shown that the prepared black niobium oxide has a strong absorption phenomenon of visible light (absorbance is 0.8-0.9).
Claims
1. A method for preparing a black niobium oxide photocatalytic material, Features The following steps are involved: (1) According to the mass volume ratio of niobium oxide nanopowder: NbCl 5 ∶NaH or CaH 2 ∶anhydrous toluene=10-30 g:1-5 g:0.2-1 g:100-200 mL, mix at room temperature to obtain a reaction solution; (2) The reaction solution is placed in a reaction kettle and subjected to a solvent thermal reaction at 180 to 220° C. for 5 to 15 hours to obtain NbCl 5 Dissolve in anhydrous toluene and mix with NaH or CaH 2 After the reaction, the NbH x Cl 5-x (x = 0.1-2) precursor powder uniformly deposited on the surface of niobium oxide particles; (3) Add the precursor powder to NH 3 In aqueous solution, NbH x Cl 5-x (x = 0.1-2) was hydrolyzed, and the obtained precipitate was washed with anhydrous ethanol and then moved to a hydrogen furnace for heat treatment at 250-350°C in a hydrogen atmosphere for 1-2 hours to obtain NbO y H x +NbO 2.5 (x=0.1~2) Dual-phase structure niobium oxide photocatalytic material.
2. A product obtained by the method for preparing the black niobium oxide photocatalytic material according to claim 1.
3. The product according to claim 2, Features: The NbO y H x +NbO 2.5 The hydrogen evolution rate of the dual-phase niobium oxide photocatalytic material in the photocatalytic water decomposition reaction is much faster than that of pure NbO 2.5 25 to 35 times of.
Citation Information
Patent Citations
Process for manufacturing metal containing powder