Catalyst precursor as well as preparation method and application thereof

By designing Cu and M metal oxide catalyst precursors, using Al2O3 and MgO support materials to control acidic alkaline sites, the problem of DMA selective hydrogenation is solved, and high efficiency and economicality is achieved production, suitable for industrial applications.

CN118904345AActive Publication Date: 2024-11-08SHANGHAI HUAFON NEW MATERIAL R&D TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410948561.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The prior art is difficult to achieve DMA selective hydrogenation to prepare methyl 6-hydroxyhexanoate, resulting in high raw material prices, poor process economy, and low selectivity and efficiency of catalysts, which limits industrial applications.

Method used

A catalyst precursor, including oxides of Cu and M metals, is designed, and the support material is a mixture of Al2O3 and MgO, by controlling the Cu, M, Al, Mg atomic ratio and the acidic alkaline position of the support material in the catalyst precursor. Point concentration ensures that the formation of highly selective and efficient catalysts after CuO reduction.

Benefits of technology

The efficient production of methyl 6-hydroxyhexanoate is achieved by selective hydrogenation of DMA, reducing the raw material price, simplifying the process, suitable for large-scale production, and improving the selectivity and conversion rate of the catalyst.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a catalyst precursor as well as a preparation method and application thereof. The catalyst precursor comprises an active component and a carrier material; the active components are oxides of CuO and M; m is selected from at least one of IVA group metal ions, IB group metal ions, IIB group metal ions, IVB group metal ions, VIB group metal ions, VIIB group metal ions or VIII group metal ions, and M is not Cu; the carrier material is a mixture comprising Al2O3 and MgO. The composition of the catalyst precursor is designed, CuO in the catalyst precursor is reduced into Cu, the catalyst which is excellent in performance and high in selectivity and can be used for preparing the methyl 6-hydroxyhexanoate through DMA selective hydrogenation is obtained, the condition for preparing the methyl 6-hydroxyhexanoate by using the catalyst is mild, and the production process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic synthesis, and specifically relates to a catalyst precursor and a preparation method and application thereof, and more specifically relates to a catalyst precursor for preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA and a preparation method and application thereof. Background Art

[0002] 6-Hydroxycaproic acid ester can efficiently cyclize to synthesize ε-caprolactone, and after ring-opening polymerization, it can obtain polycaprolactone or polycaprolactone polyol. The former is used in biomedicine, degradable materials and other fields, and the latter is used to synthesize high-performance polyurethane.

[0003] There are few research reports on the synthesis of 6-hydroxyhexanoic acid esters. The methods used in the literature are mostly the reaction of caprolactone with alcohol or the esterification of 6-hydroxyhexanoic acid, but these two raw materials are expensive and the process economy is poor. CN101945847A discloses a method for preparing 6-hydroxyhexanoic acid ester, which comprises the following steps: a) oxidizing cyclohexane with molecular oxygen or a mixture of molecular oxygen and a gas that is inert under reaction conditions to generate a reaction mixture containing the following components as main components: cyclohexyl hydroperoxide, cyclohexanol, cyclohexanone, unconverted cyclohexane, 6-hydroperoxycaproic acid, 6-hydroxycaproic acid, 5-formylvaleric acid and α,ω-dicarboxylic acids having 4 to 6 carbon atoms, b) separating the reaction mixture from step a) into an organic phase containing cyclohexane and cyclohexane compounds and an aqueous phase containing carboxylic acids after adding water, c) catalytically hydrogenating the aqueous phase from step b), d) reacting the carboxylic acid present in the aqueous phase with an alcohol containing 1 to 10 carbon atoms to produce the corresponding carboxylic acid ester, and e) obtaining 6-hydroxyhexanoic acid ester from the esterification mixture from step d) by distillation, wherein the catalytic hydrogenation in step c) comprises at least hydrogenating 5-formylvaleric acid to 6-hydroxyhexanoic acid. It can be seen from this that this technical solution uses 5-formylvaleric acid, a by-product mixture produced during the oxidation of cyclohexane to cyclohexanone and cyclohexanol, as a raw material, prepares 6-hydroxyhexanoic acid through a hydrogenation reaction, and further esterifies to obtain 6-hydroxyhexanoic acid ester. This method has limited raw material supply and cannot be mass-produced.

[0004] CN101379019A discloses a method for producing 6-hydroxycaproic acid ester and a method for producing trialkylamine. The technical scheme uses nylon 6 and an amide compound based on ε-caprolactam and an alcohol in a supercritical state to prepare 6-hydroxycaproic acid ester and trialkylamine under conditions of 330-370°C and 27-36MPa, but the reaction conditions are harsh, and the equipment investment and operating energy consumption are too high.

[0005] Using DMA (full name: dimethyl 1,6-adipate) as raw material, 6-hydroxyhexanoic acid methyl ester can theoretically be obtained through selective unilateral hydrogenation. DMA raw materials are inexpensive and widely available. If effective unilateral hydrogenation can be achieved, this route has excellent industrial prospects.

[0006] However, the current difficulty is how to achieve efficient and selective unilateral hydrogenation, that is, during the synthesis, it is required to control only one of the ester bonds in DMA to be hydrogenated and converted into hydroxyl groups, and the other ester bond is retained. It is relatively easy to achieve efficient full hydrogenation of DMA, that is, the two ester bonds are indifferently converted into hydroxyl groups during the hydrogenation process, but how to prepare 6-hydroxyhexanoic acid methyl ester by selective hydrogenation using DMA as a raw material has become the focus of current research. How to provide an efficient catalyst that can achieve selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester has become a technical problem that needs to be solved urgently. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a catalyst precursor and a preparation method and application thereof, and more specifically to a catalyst precursor for preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA and a preparation method and application thereof. In the present invention, by designing the composition of the catalyst precursor, after CuO in the catalyst precursor is reduced to Cu, a catalyst with excellent performance and high selectivity is obtained, which can realize the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conditions for preparing 6-hydroxyhexanoic acid methyl ester by using the catalyst are relatively mild, the production process is relatively simple, the raw material price is low, the source is wide, and large-scale production can be carried out.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a catalyst precursor, the catalyst precursor comprising an active component and a support material;

[0010] The active ingredients are Cu and M;

[0011] The M is selected from at least one of Group IVA, Group IB, Group IIB, Group IVB, Group VIB, Group VIIB or Group VIII metals, and M is not Cu;

[0012] The support material comprises Al 2 O 3 A mixture of MgO and MgO;

[0013] The acidic site concentration of the carrier material is 0.5 to 2 mmol / g, and the basic site concentration is 1 to 5 mmol / g;

[0014] The atomic ratio of Cu, M, Al and Mg in the catalyst precursor is 5-15:0.5-1.5:15-65:20-80, and the sum of the atomic ratios of Cu, Al and Mg in the catalyst precursor is 100.

[0015] In the present invention, the composition of the catalyst precursor is designed, and the atomic ratio of Cu, M, Al, and Mg in the catalyst precursor is controlled within a specific range, and the Al 2 O 3 A mixture of CuO and MgO is used as a carrier material, and the acid site concentration and the basic site concentration of the carrier material are controlled within a specific range. After CuO in the catalyst precursor is reduced to Cu, a catalyst with excellent performance and high selectivity is obtained, and the catalyst can realize the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conditions for preparing 6-hydroxyhexanoic acid methyl ester using the catalyst are relatively mild, the production process is relatively simple, the raw material price is low, the source is wide, and large-scale production can be carried out.

[0016] In the present invention, the Cu in the catalyst can make H 2 The molecules are adsorbed and dissociated into active H atoms to achieve catalytic ester bond hydrogenation. Therefore, Cu-based catalysts are usually selected for DMA hydrogenation. In order to make the Cu nanoparticles have a smaller particle size (XRD) and better dispersion (N 2 O titration method), the present invention designs the Cu atomic ratio in the catalyst precursor to be 5-15%, so that the Cu atomic ratio in the catalyst after subsequent hydrogenation is 5-15%. The prior art usually has a high Cu loading, mostly above 20%. The higher the copper content, the stronger the catalytic hydrogenation activity and the higher the conversion rate of DMA. However, the inventors found that an excessively high Cu loading leads to extremely high selectivity for hexanediol, and basically no selective unilateral hydrogenation product 6-hydroxyhexanoic acid methyl ester is generated.

[0017] The catalyst carrier used in DMA hydrogenation in the prior art is mostly SiO 2 、Al 2 O 3 Or porous materials such as molecular sieves as carriers are conducive to obtaining catalysts with high specific surface areas and selectively generating hexanediol. However, the surface of such carriers is acidic. When used for selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester, DMA and 6-hydroxyhexanoic acid methyl ester will easily undergo oligomerization reaction under hydrogenation conditions, and the target product 6-hydroxyhexanoic acid methyl ester cannot be obtained with high selectivity.

[0018] The catalyst precursor provided by the present invention and the carrier material of the catalyst after hydrogenation contain acidic Al 2 O 3With alkaline MgO, the acid-base sites created can interact with the oxygen atom and π* orbital of C=O in DMA, promote the adsorption and activation of DMA on the catalyst surface, and facilitate the selective hydrogenation reaction. 2 O 3 The surface hydroxyl group interacts with the carbonyl group in DMA to promote the adsorption of DMA on the catalyst; the basic site provided by MgO can interact with the hydroxyl group in 6-hydroxyhexanoic acid methyl ester, stabilize the intermediate product, and slow down the further hydrogenation of 6-hydroxyhexanoic acid methyl ester to produce 1,6-hexanediol, which has an effect that cannot be replaced by other alkali metal or alkaline earth metal oxides. At the same time, in the present invention, by designing the molar ratio of Al and Mg within a specific range, the acid site concentration and the basic site concentration of the carrier material can be controlled within a specific range, which can effectively improve the selectivity of 6-hydroxyhexanoic acid methyl ester.

[0019] In the present invention, the carrier material comprises acidic Al 2 O 3 A mixture of alkaline MgO and the acidic Al 2 O 3 Acidic Al is independent of basic MgO 2 O 3 Particles and independent alkaline MgO particles. Acidic Al 2 O 3 The alkaline MgO particles and the alkaline MgO particles have independent surfaces to obtain the ideal distribution and concentration of acid and base sites that promote selective hydrogenation. 2 O 3 Surface or acidic Al 2 O 3 Loading on the alkaline MgO surface destroys the ideal distribution of acid and base sites, and cannot obtain the ideal acid and base site concentration, which ultimately leads to low selectivity of methyl 6-hydroxyhexanoate.

[0020] The acidic site concentration of the support material can be 0.5mmol / g, 0.6mmol / g, 0.7mmol / g, 0.8mmol / g, 0.9mmol / g, 1mmol / g, 1.1mmol / g, 1.2mmol / g, 1.3mmol / g, 1.4mmol / g, 1.5mmol / g, 1.6mmol / g, 1.7mmol / g, 1.8mmol / g, 1.9mmol / g or 2mmol / g, etc.

[0021] The basic site concentration of the support material can be 1 mmol / g, 1.5 mmol / g, 2 mmol / g, 2.5 mmol / g, 3 mmol / g, 3.5 mmol / g, 4 mmol / g, 4.5 mmol / g or 5 mmol / g, etc.

[0022] The atomic ratio of Cu, M, Al and Mg in the catalyst precursor is 5-15:0.5-1.5:15-65:20-80, for example, 5:0.5:15:80, 10:1:20:70, 15:1.5:65:20, 10:1:30:60, 15:0.5:15:70, 5:0.5:65:30, 10:1:15:75, 10:1:25:65, 10:1:50:40, 10:1:65:25, etc.

[0023] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0024] As a preferred technical solution of the present invention, M in the catalyst precursor is selected from any one of Fe, Zn, Co, Mn, and Zr, or a combination of at least two thereof.

[0025] As a preferred technical solution of the present invention, the ratio of the acid site concentration to the basic site concentration of the carrier material is 0.2 to 0.8:1, for example, it can be 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1 or 0.8:1.

[0026] In the present invention, the selectivity of methyl 6-hydroxyhexanoate can be further improved by further controlling the ratio of the acid site concentration to the basic site concentration of the carrier material within a specific range.

[0027] As a preferred technical solution of the present invention, the average pore diameter of the catalyst precursor is ≥15 nm, for example, it can be 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm or 25 nm.

[0028] In the present invention, by controlling the average pore size of the catalyst precursor within a specific range, it is ensured that the subsequent corresponding catalyst has a suitable average pore size, so that the generated product can be diffused in time, and 6-hydroxyhexanoic acid methyl ester with a high yield can be prepared. If the pore size of the catalyst precursor is too small, the pore size of the corresponding catalyst is too small, and when the diffusion capacity of the product molecule is insufficient, it is easy to cause the other side of the 6-hydroxyhexanoic acid methyl ester to be hydrogenated and converted into 1,6-hexanediol, resulting in a low selectivity of 6-hydroxyhexanoic acid methyl ester, and ultimately resulting in a low yield of 6-hydroxyhexanoic acid methyl ester.

[0029] As a preferred technical solution of the present invention, the average particle size of CuO in the catalyst precursor is 3 to 5 nm, for example, it can be 3 nm, 3.2 nm, 3.4 nm, 3.6 nm, 3.8 nm, 4 nm, 4.2 nm, 4.4 nm, 4.6 nm, 4.8 nm or 5 nm.

[0030] Preferably, the dispersion degree of CuO in the catalyst precursor is 30-35%, for example, it can be 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5% or 35%.

[0031] It is known that the smaller the particle size of the active component, the higher the dispersion. The present invention can avoid sintering of the active component, resulting in reduced catalyst activity and decreased DMA conversion rate, by controlling the particle size and dispersion of the active component in the catalyst precursor within a specific range.

[0032] As a preferred technical solution of the present invention, the catalyst precursor also includes a dehydrating agent.

[0033] Preferably, the water scavenger comprises CaO.

[0034] Preferably, based on the sum of the mass percentages of the active ingredient and the carrier material as 100%, the mass percentage content of the dehydrating agent is 0.5-1%, for example, it can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%.

[0035] The dehydrating agent can react with the trace amount of water in the raw material DMA to inhibit the hydrolysis of DMA and avoid the formation of monomethyl adipate or adipic acid. CaO reacts with the trace amount of water in the raw material DMA to generate Ca(OH) 2 It can also react with trace amounts of adipic acid or monomethyl adipic acid in the raw material to prevent the acidic substance from catalyzing oligomerization side reactions, which is beneficial to prolonging the life of the catalyst. If the content of the dehydrating agent in the catalyst is too low, the effect on the life of the catalyst is not significant; if the content of the dehydrating agent in the catalyst precursor is too high, it will significantly change the surface alkaline sites of the catalyst, causing side reactions, resulting in poor selectivity of 6-hydroxyhexanoic acid methyl ester and low yield.

[0036] In a second aspect, the present invention provides a method for preparing the catalyst precursor as described in the first aspect, wherein the preparation method specifically comprises the following steps:

[0037] (1) mixing a soluble copper salt, a soluble salt containing M, a soluble magnesium salt, a soluble aluminum salt and water to obtain a solution A;

[0038] Mixing the precipitant and water to obtain solution B;

[0039] (2) adding the solution B dropwise into the solution A, and precipitating Cu, M, Al, and Mg in the form of basic carbonates to obtain a mixture;

[0040] (3) aging the mixture obtained in step (2);

[0041] (4) calcining the aged mixture in step (3) to obtain catalyst precursor embryos, and then grinding the obtained embryos to obtain the catalyst precursor.

[0042] It should be noted that in the present invention, there is no special restriction on the specific selection of soluble copper salts, soluble salts containing M, soluble magnesium salts, and soluble aluminum salts, and the soluble copper salts, soluble salts containing M, soluble magnesium salts, and soluble aluminum salts commonly used in the art are all applicable. Among them, soluble copper salts exemplarily include but are not limited to: copper nitrate, copper oxalate, copper sulfate, and copper chloride, preferably copper nitrate and copper oxalate; soluble salts containing M exemplarily include but are not limited to: nitrates of M, oxalates of M, sulfates of M, chlorides of M, preferably nitric acid of M, oxalic acid of M; soluble magnesium salts exemplarily include but are not limited to: magnesium nitrate, magnesium oxalate, magnesium sulfate, and magnesium chloride, preferably magnesium nitrate and magnesium oxalate; soluble aluminum salts exemplarily include but are not limited to: aluminum nitrate, aluminum oxalate, aluminum sulfate, and aluminum chloride, preferably aluminum nitrate and aluminum oxalate.

[0043] The precipitant is a conventional alkaline substance that can precipitate the soluble metal salt in the form of basic carbonate, usually a mixture of a weak alkaline substance and a strong alkaline substance; the molar ratio of the weak alkaline substance to the strong alkaline substance is adjusted according to the principle of completely precipitating the metal particles, for example, the molar ratio can be 1 / 3 to 1 / 5.

[0044] The weak alkaline substance is selected from any one of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonia water, and ammonium bicarbonate, or a combination of at least two thereof;

[0045] The strong alkaline substance is selected from sodium hydroxide and / or lithium hydroxide;

[0046] In the present invention, there is no special restriction on the concentration of soluble salts (including soluble copper salts, soluble M salts, soluble magnesium salts, soluble aluminum salts, the same below) in solution A and the concentration of precipitant in solution B, and the concentration ranges commonly used in the art are applicable. If the precipitation process in step (2) is carried out in an overly dilute solution, the supersaturation is small, which is conducive to crystal growth, but the yield of the synthetic catalyst precursor per unit volume is low; if the precipitation process in step (2) is carried out in a concentrated solution, the supersaturation is large, the crystallization rate is fast, but it is also easy to contain impurities. The selection of the target molar concentrations of solution A and solution B should take into account the result of forming a precipitate at an appropriate supersaturation. Exemplarily, for example, a solution A having a soluble salt concentration of 0.5 to 2 mol / L (e.g., 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, or 2 mol / L, etc.) and a solution B having a total alkali (including strong alkaline substances and weak alkaline substances) concentration of 0.5 to 2 mol / L (e.g., 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, or 2 mol / L, etc.). The target molar concentration of solution B and its volume ratio with solution A should be selected to achieve the desired Cu 2+ , M, Al 3+ Mg 2+ As a result of complete precipitation, illustratively, the pH at the end point of dropwise addition is controlled to be 9.0 to 10.5 (eg, 9.0, 9.2, 9.5, 9.7, 10.0, 10.2 or 10.5, etc.).

[0047] In the present invention, the purpose of aging in step (3) is to obtain a precipitate with uniform particle size and stable structure. It should be noted that there is no special restriction on the process conditions for aging in the present invention, and the process conditions commonly used in the art are applicable, and aging is performed by stirring at 80 to 100° C. (for example, 80° C., 82° C., 84° C., 86° C., 88° C., 90° C., 92° C., 94° C., 96° C., 98° C. or 100° C., etc.) for 12 to 24 hours (for example, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours or 24 hours, etc.).

[0048] In the present invention, step (3) further includes a post-treatment step after aging, and the post-treatment method includes filtering, washing, and drying.

[0049] As a preferred technical solution of the present invention, the calcination temperature is 400-550°C, for example, it can be 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C or 550°C.

[0050] Preferably, the calcination time is ≥ 3 h, for example, it can be 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.

[0051] In the present invention, by controlling the calcination temperature within a specific range, a catalyst precursor with excellent performance can be prepared. As the calcination temperature increases, the average pore size of the catalyst precursor will increase, but the acid-base site concentration will simultaneously decrease. The suitable calcination temperature is 400-550°C, and the optimum calcination temperature is 450°C; if the calcination temperature is too low, the acid-base site concentration of the prepared catalyst precursor is high, but the average pore size is too small; if the calcination temperature is too high, a catalyst precursor with a larger pore size can be prepared, but the acid-base site concentration will be too low.

[0052] Meanwhile, the calcination time in step (4) of the present invention is ≥ 3 h, otherwise the catalyst precursor is difficult to be completely converted into CuO, M oxides, Al 2 O 3 and MgO.

[0053] It should be noted that if the catalyst precursor contains a dehydrating agent, after the catalyst precursor green particles are obtained by roasting in step (4), the catalyst precursor green particles are mixed with the dehydrating agent and ground together to obtain the catalyst precursor.

[0054] In the present invention, the grinding in step (4) further comprises the steps of tableting, grinding and screening, and after grinding and screening, a catalyst precursor with a mesh size of 20 to 60 is obtained.

[0055] In the preparation method of the present invention, the process means adopted is to co-precipitate a soluble magnesium salt and a soluble aluminum salt to obtain a catalyst precursor having a specific acid site concentration and a specific basic site concentration, thereby ensuring that the acid site concentration and the specific basic site concentration of the activated catalyst are suitable for improving the selectivity of 6-hydroxyhexanoic acid methyl ester. 2 O 3 or Al 2 O 3 Precursors (such as aluminum hydroxide, pseudo-boehmite, etc.) are used to precipitate MgO on Al 2 O 3 The surface is partially covered with surface acid and basic sites to improve the selectivity of the target product 1,6-hexanediol. As mentioned above, MgO is precipitated on Al 2 O 3When the surface is exposed to the sun, it is impossible to obtain a suitable distribution of acid and base sites, which not only fails to improve the selectivity of unilateral hydrogenation, but instead increases the selectivity of 1,6-hexanediol.

[0056] In the preparation method of the present invention, the precipitation product of Cu salt is small-sized nanoparticles, while the precipitation products of Mg salt and Al salt are large-sized carriers with high specific surface area. Nano-sized CuO is randomly dispersed in the system. 2 O 3 In a mixture system with alkaline MgO.

[0057] As a preferred technical solution of the present invention, the method for preparing the catalyst precursor specifically comprises the following steps:

[0058] (1) mixing a soluble copper salt, a soluble salt containing M, a soluble magnesium salt, a soluble aluminum salt and water to obtain a solution A;

[0059] Mixing the precipitant and water to obtain solution B;

[0060] (2) adding the solution B dropwise into the solution A, and precipitating Cu, M, Al, and Mg in the form of basic carbonates to obtain a mixture;

[0061] (3) stirring the mixture obtained in step (2) at 80-100° C. for 12-24 h, aging, filtering, washing, and drying;

[0062] (4) The aged mixture obtained in step (3) is calcined at 400-550° C. for ≥3 h to obtain catalyst precursor embryonic particles, which are then mixed with an optional dehydrating agent, ground, formed into tablets, and ground and sieved to obtain a catalyst precursor with a mesh size of 20-60 meshes.

[0063] In a third aspect, the present invention provides a method for preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA, the method comprising the following steps:

[0064] (S1) performing a reduction treatment on the catalyst precursor described in the first aspect until all CuO in the catalyst precursor is reduced to Cu, thereby obtaining a catalyst having catalytic activity;

[0065] (S2) placing the catalyst obtained after reduction treatment in step (S1) in a reaction system, introducing hydrogen, and adding DMA to the reaction system under a hydrogen atmosphere to react to obtain methyl 6-hydroxyhexanoate.

[0066] In the present invention, by designing the composition of the catalyst precursor, a catalyst with excellent performance and high selectivity is obtained, which can realize the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester, and the conditions for preparing 6-hydroxyhexanoic acid methyl ester using the catalyst are relatively mild.

[0067] The reduction treatment of the catalyst precursor in step (S1) of the present invention is a prior art, and its process conditions are not particularly limited. For example: using a mixed gas containing hydrogen to reduce the catalyst precursor so that CuO in the catalyst precursor is reduced to Cu, and other oxides will not be reduced in the reduction treatment of the mixed gas containing hydrogen; using a nitrogen-hydrogen mixed gas (hydrogen volume concentration of 10-50%, for example, 10%, 15%, 20%) , 25%, 30%, 35%, 40%, 45% or 50%, etc.) at 200-230°C (for example, it can be 200°C, 203°C, 206°C, 210°C, 212°C, 215°C, 217°C, 220°C, 223°C, 225°C, 228°C or 230°C, etc.) for 4-12h (for example, it can be 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h, etc.).

[0068] As a preferred technical solution of the present invention, after the reaction in step (S2), a post-treatment step is also included, and the post-treatment method includes the following steps:

[0069] The mixture obtained after the reaction is placed in a gas-liquid separator for separation to obtain a liquid product containing residual DMA, 6-hydroxyhexanoic acid methyl ester and 1,6-hexanediol; the hydrogen is returned to the reaction system for repeated use.

[0070] In industrial production, the method for preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA using the catalyst precursor provided by the present invention includes the following exemplary steps:

[0071] (S1) loading the prepared catalyst precursor into a fixed bed reactor, and performing a reduction treatment on the catalyst precursor until all CuO is reduced to Cu element;

[0072] (S2) After the catalyst precursor reduction treatment is completed, the reaction temperature of the fixed bed reactor is adjusted to 200° C., the replacement atmosphere is a hydrogen atmosphere, the hydrogen flow rate is controlled and the pressure of the fixed bed reactor is adjusted to 2 MPa, DMA is vaporized in the vaporization chamber and then enters the reactor to react with hydrogen, and the reaction mixture discharged from the fixed bed reactor is placed in a gas-liquid separator for separation to obtain a liquid phase product containing residual DMA, 6-hydroxyhexanoic acid methyl ester and 1,6-hexanediol, thereby obtaining 6-hydroxyhexanoic acid methyl ester;

[0073] The molar ratio of hydrogen to DMA is 40:1, and the mass space velocity of DMA is 1.0 kg / (kg·h); the hydrogen is returned to the reaction system for repeated use.

[0074] In a fourth aspect, the present invention provides a catalyst, wherein the catalyst is obtained by subjecting the catalyst precursor described in the first aspect to a reduction treatment, wherein the CuO in the catalyst is reduced to Cu, and other metal oxides remain in an oxidized state.

[0075] Compared with the prior art, the present invention has the following beneficial effects:

[0076] (1) The catalyst precursor for preparing 6-hydroxyhexanoic acid methyl ester from DMA provided by the present invention comprises an acidic Al 2 O 3 A mixture of alkaline MgO and acidic Al 2 O 3 The use of alkaline MgO can regulate the acid site concentration and basic site concentration of the catalyst precursor within a specific range, so that it maintains a suitable acid-base site ratio, thereby ensuring that the acid site concentration and specific basic site concentration of the catalyst after activation (i.e., after CuO reduction) are appropriate, which can effectively improve the selectivity of 6-hydroxyhexanoic acid methyl ester.

[0077] (2) The present invention uses a dehydrating agent, which reacts with trace amounts of water and acidic impurities in the raw materials to inhibit the occurrence of oligomerization side reactions during DMA hydrogenation and improve the selectivity of 6-hydroxyhexanoic acid methyl ester.

[0078] (3) Compared with the existing method, the catalyst precursor preparation method of the present invention does not require additional equipment, has a simple process, and is easier to industrialize.

[0079] (4) In the process of using the catalyst precursor provided by the present invention to catalyze the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester, the reduction reaction of the catalyst precursor can be carried out directly in the reactor without external reduction, saving costs; in specific application scenarios, it can also be carried out outside the reactor. The catalyst provided by the present invention can achieve a relatively high conversion rate of DMA and a relatively high selectivity of 6-hydroxyhexanoic acid methyl ester at a relatively low reaction pressure and a relatively high liquid mass space velocity, which can save fixed asset investment, reduce operating costs, and increase production capacity. It has a good application prospect, the conversion rate of DMA is 90-98%, the selectivity of 6-hydroxyhexanoic acid methyl ester is 86-99%, the yield of 6-hydroxyhexanoic acid methyl ester is 82-93%, and the degree of hydrolysis of DMA is ≤0.2%. DETAILED DESCRIPTION

[0080] For ease of understanding of the present invention, the present invention enumerates the following embodiments. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. The raw materials in the present invention can all be purchased from the market, and the experimental methods for which specific conditions are not indicated in the examples are usually carried out under conventional conditions.

[0081] The performance of the catalyst precursor provided in the embodiments and comparative examples of the present invention or the DMA selective hydrogenation provided in the application examples and comparative application examples to prepare 6-hydroxyhexanoic acid methyl ester was tested, and the specific test method is as follows:

[0082] 1. Concentration of acidic sites on the catalyst precursor surface

[0083] The NH 3 -TPD was measured. The test method is as follows: 100 mg of the catalyst precursor of 20-60 mesh was placed in a U-shaped quartz tube, pretreated in a helium atmosphere of 30 mL / min, heated from room temperature to 400°C at a rate of 10°C / min, kept constant for 2 hours, and then naturally cooled to 50°C to remove water and other pollutants; then a 10 vol% NH 3 The ammonia-helium mixture is then heated to 600℃ at a rate of 10℃ / min for desorption. During the heating process, the NH adsorbed on the acidic sites is desorbed. 3 It will gradually separate, and at 600℃, all acidic sites will separate from ammonia. The higher the ammonia desorption temperature, the stronger the acidity. 3 -The signal acquisition in the TPD test process uses a thermal conductivity cell detector (TPD), which can use the difference in thermal conductivity between the carrier gas and the gas to be tested to reflect the change in ammonia concentration during the heating process, and convert this chemical signal into a voltage signal and feed it back on the spectrum. The horizontal axis of the spectrum is temperature (℃), and the vertical axis is voltage (mV). Through the correspondence between the ammonia content and the integrated area of ​​the desorption peak in the spectrum, according to the ratio that 1 mol of acid sites can adsorb 1 mol of ammonia, the ammonia adsorption amount can be converted to the acid site content. At this point, the peak area data can be converted to the acid site content, and divided by the mass of the catalyst precursor to obtain the acid site concentration.

[0084] 2. Basic site concentration on the catalyst precursor surface

[0085] The instrument and testing principle used are consistent with the testing principle of acid site content. 2 -TPD test. The test method is as follows: take 100 mg of 20-60 mesh catalyst precursor into a U-shaped quartz tube, pre-treat in a 30 mL / min helium atmosphere, heat from room temperature to 400°C at a rate of 10°C / min, keep the temperature constant for 2 hours, and then naturally cool to 50°C; then pass a 10 vol% CO 2The alkaline sites on the sample to be tested will chemically combine with CO2. After 30 minutes of adsorption, all alkaline sites will be chemically combined with CO2. 2 reaction; then, helium was used to purge and remove the unreacted CO 2 ; Then, the temperature was raised to 600℃ at a rate of 10℃ / min for desorption, and CO was detected. 2 -TPD spectrum, from CO 2 The basic site concentration of the catalyst precursor sample was calculated based on the correspondence between the content and the integrated area of ​​the desorption peak in the spectrum.

[0086] 3. Average pore size of catalyst precursor

[0087] The average pore size of the catalyst precursor can be obtained by using a physical adsorption instrument model BSD-PM1 / 2 produced by Best Instrument Technology Co., Ltd. The test method is as follows: 120 mg of a catalyst precursor with a mesh size of 20 to 60 is placed in a quartz tube and degassed at 200°C for 24 hours to remove water and other impurities, and then an adsorption-desorption experiment is performed at -196°C.

[0088] 4. Average particle size of CuO in catalyst precursor

[0089] The average particle size of CuO was characterized by an X-ray diffractometer model Advance D8 from Bruker, Germany. 3 g of the catalyst precursor was taken and ground into a mortar with a mesh size of less than 300. The powder sample was added to the groove of the sample holder and the surface was pressed with a glass slide to keep the entire surface even and flat and consistent with the height of the groove plane. The sample holder was inserted into the sample card slot of the instrument. Cu K α X-ray, tube voltage and tube current are 40 kV and 40 mA respectively, scanning speed is 5° / min, and scanning range 2θ is 10°~80°. The average particle size of CuO particles in the sample is calculated using Scherrer formula, and its expression is as follows: d=Kλ / (βCosθ), where K is Scherrer constant, which is 0.89, λ is X-ray wavelength, Cu K α The wavelength is β is the half-height width of the sample diffraction peak, and θ is the diffraction angle.

[0090] 5. Dispersion of CuO in catalyst precursor

[0091] Tianjin Xianquan TP-5080B chemical adsorption instrument was used to analyze the N 2 O titration method. The test method is as follows: take 50 mg of 20-60 mesh catalyst precursor in a U-shaped quartz tube and use 5 vol% H 2The CuO in the catalyst precursor was reduced to Cu by a mixture of hydrogen and nitrogen with a gas flow rate of 30 mL / min and a heating rate of 10 °C / min. The temperature was kept at 400 °C for 60 min for the first reduction. H 2 -TPR spectrum, the reduction peak area can be obtained by software integration; when the bed temperature drops below 50°C, the gas flow is switched to nitrogen purge for 60 minutes, with a gas flow rate of 30 mL / min; after the nitrogen purge is completed, the gas flow is switched to 5 vol% N 2 O mixed with laughing gas and nitrogen, kept at 50℃ for 60min to oxidize the surface copper of the sample, the chemical equation is: 2Cu+N 2 O(g)=Cu 2 O+N 2 (g) Switch the gas flow to nitrogen purge for 60 min to remove the unreacted and adsorbed N 2 O; then 5 vol% H 2 The catalyst precursor was reduced for the second time under the same conditions by a mixture of hydrogen and nitrogen. The chemical equation is: Cu 2 O+H 2 (g) = 2Cu + H 2 O(g); The calculation formula for the CuO dispersion on the catalyst precursor surface is: D = 2A 2 / A 1 *100%, of which A 1 With A 2 N 2 The reduction peak areas of the first and second temperature-programmed reduction in the O titration experiment.

[0092] 6. Evaluation of selective hydrogenation effect

[0093] The catalyst provided by the present invention is activated after the catalyst precursor is used in the process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA. The obtained liquid phase product is analyzed by gas chromatography, the detector is FID, and the conversion rate of DMA, the selectivity of 6-hydroxyhexanoic acid methyl ester, the yield of 6-hydroxyhexanoic acid methyl ester (conversion rate of DMA*selectivity of 6-hydroxyhexanoic acid methyl ester) and the degree of hydrolysis of DMA (referring to the sum of the selectivity of generated monomethyl adipic acid, 6-hydroxycaproic acid and adipic acid) are calculated by external standard standard curve method. The process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA is as follows:

[0094] (S1) loading the prepared catalyst precursor into a fixed bed reactor, and performing a reduction treatment on the catalyst precursor until all CuO is reduced to Cu element;

[0095] (S2) After the catalyst precursor reduction treatment is completed, the reaction temperature of the fixed bed reactor is adjusted to 200° C., the replacement atmosphere is a hydrogen atmosphere, the hydrogen flow rate is controlled and the pressure of the fixed bed reactor is adjusted to 2 MPa, DMA is vaporized in the vaporization chamber and then enters the reactor to react with hydrogen, and the reaction mixture discharged from the fixed bed reactor is placed in a gas-liquid separator for separation to obtain a liquid phase product containing residual DMA, 6-hydroxyhexanoic acid methyl ester and 1,6-hexanediol, thereby obtaining 6-hydroxyhexanoic acid methyl ester;

[0096] The molar ratio of hydrogen to DMA is 40:1, and the mass space velocity of DMA is 1.0 kg / (kg·h); the hydrogen is returned to the reaction system for repeated use.

[0097] It should be noted that the deionized water used in the above method can also be replaced by other water with similar functions or utilities. The replacements and modifications made by those skilled in the art based on the above disclosure are all within the protection scope of the present invention.

[0098] Example 1

[0099] This embodiment provides a catalyst precursor and a preparation method thereof, wherein the catalyst precursor comprises an active component, a carrier material and a dehydrating agent CaO; the active component is an oxide of Cu and Zn, and the carrier material is Al 2 O 3 A mixture of MgO and MgO;

[0100] In the catalyst precursor, the atomic ratio of Cu, Zn, Al and Mg is 10:1:30:60;

[0101] The added amount of CaO is 1 wt % of the total amount of the mixture.

[0102] The preparation method of the above catalyst precursor is as follows:

[0103] (1) copper nitrate, zinc nitrate, aluminum nitrate, magnesium nitrate and deionized water are mixed and stirred to obtain a solution A; wherein the total concentration of the above metal salts in the solution A is 1 mol / L, and the atomic ratio of Cu, Zn, Al and Mg is 10:1:30:60;

[0104] Sodium carbonate, sodium hydroxide and deionized water are mixed and stirred to obtain a solution B; the total concentration of sodium carbonate and sodium hydroxide in the solution B is 1 mol / L, and the molar ratio of sodium carbonate to sodium hydroxide is 1:3;

[0105] (2) adding the solution B dropwise into the solution A, controlling the pH at the end point of the addition to be 9.5, so that Cu, Zn, Al, and Mg are precipitated in the form of basic carbonates to obtain a mixture;

[0106] (3) stirring the mixture obtained in step (2) at 80° C. for 12 h, aging, filtering, washing, and drying;

[0107] (4) The aged mixture obtained in step (3) is calcined at 450° C. for 3 h to obtain catalyst precursor embryonic particles, which are then mixed with CaO in an amount of 1 wt% of the total amount of the mixture, ground into powder, formed into tablets, and ground and sieved to obtain a catalyst precursor with a mesh size of 20 to 60.

[0108] The catalyst precursor provided in this embodiment has an acid site concentration of 1.2 mmol / g, a basic site concentration of 3 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.4:1; the average pore size of the catalyst precursor is 22 nm, of which the average particle size of CuO is 4 nm, and the dispersion of CuO is 32%.

[0109] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 94%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 99%, the yield of 6-hydroxyhexanoic acid methyl ester was 93%, and the degree of hydrolysis of DMA was 0.01%.

[0110] Example 2

[0111] This embodiment provides a catalyst precursor and a preparation method thereof, wherein the catalyst precursor comprises an active component, a carrier material and a dehydrating agent CaO; the active component is Cu and Fe, the carrier material is Al 2 O 3 A mixture of MgO and MgO;

[0112] In the catalyst precursor, the atomic ratio of Cu, Fe, Al and Mg is 5:0.5:15:80;

[0113] The added amount of CaO is 0.6 wt % of the total amount of the mixture.

[0114] The preparation method of the above catalyst precursor is as follows:

[0115] (1) copper oxalate, iron oxalate, aluminum oxalate, magnesium oxalate and deionized water are mixed and stirred to obtain a solution A; wherein the total concentration of the above metal salts in the solution A is 1 mol / L, and the atomic ratio of Cu, Fe, Al and Mg is 5:0.5:15:80;

[0116] Sodium carbonate, sodium hydroxide and deionized water are mixed and stirred to obtain a solution B; the total concentration of sodium carbonate and sodium hydroxide in the solution B is 1 mol / L, and the molar ratio of sodium carbonate to sodium hydroxide is 1:4;

[0117] (2) adding the solution B dropwise into the solution A, controlling the pH at the end point of the addition to be 9, so that Cu, Fe, Al, and Mg are precipitated in the form of basic carbonates to obtain a mixture;

[0118] (3) stirring the mixture obtained in step (2) at 85° C. for 15 h, aging, filtering, washing, and drying;

[0119] (4) The aged mixture obtained in step (3) is calcined at 450° C. for 4 h to obtain catalyst precursor embryonic particles, which are then mixed with CaO in an amount of 0.6 wt % of the total amount of the mixture, ground into powder, formed into tablets, and ground and sieved to obtain a catalyst precursor with a mesh size of 20 to 60.

[0120] The catalyst precursor provided in this embodiment has an acid site concentration of 0.5 mmol / g, a basic site concentration of 5 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.01:1; the average pore size of the catalyst precursor is 22.3 nm, of which the average particle size of CuO is 3.6 nm, and the dispersion of CuO is 34%.

[0121] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 90%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 94%, the yield of 6-hydroxyhexanoic acid methyl ester was 85%, and the degree of hydrolysis of DMA was 0.02%.

[0122] Example 3

[0123] This embodiment provides a catalyst precursor and a preparation method thereof, wherein the catalyst precursor comprises an active component, a carrier material and a dehydrating agent CaO; the active component is Cu and Co, and the carrier material is Al 2 O 3 A mixture of MgO and MgO;

[0124] In the catalyst precursor, the atomic ratio of Cu, Co, Al and Mg is 15:0.5:15:70;

[0125] The added amount of CaO is 0.5 wt % of the total amount of the mixture.

[0126] The preparation method of the above catalyst precursor is as follows:

[0127] (1) copper chloride, cobalt chloride, aluminum chloride, magnesium chloride and deionized water are mixed and stirred to obtain a solution A; wherein the total concentration of the above metal salts in the solution A is 1 mol / L, and the atomic ratio of Cu, Co, Al and Mg is 15:0.5:15:70;

[0128] Sodium carbonate, sodium hydroxide and deionized water are mixed and stirred to obtain a solution B; the total concentration of sodium carbonate and sodium hydroxide in the solution B is 1 mol / L, and the molar ratio of sodium carbonate to sodium hydroxide is 1:3;

[0129] (2) adding the solution B to the solution A by dropwise addition, controlling the pH at the end point of the dropwise addition to be 10.5, so that Cu, Co, Al, and Mg are precipitated in the form of basic carbonates to obtain a mixture;

[0130] (3) stirring the mixture obtained in step (2) at 95° C. for 20 h, aging, filtering, washing, and drying;

[0131] (4) The aged mixture obtained in step (3) is calcined at 440° C. for 3 h to obtain catalyst precursor embryonic particles, which are then mixed with CaO in an amount of 0.5 wt % of the total amount of the mixture, ground into powder, formed into tablets, and ground and sieved to obtain a catalyst precursor with a mesh size of 20 to 60.

[0132] The catalyst precursor provided in this embodiment has an acid site concentration of 0.7 mmol / g, a basic site concentration of 4.3 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.16:1; the average pore size of the catalyst precursor is 22.1 nm, wherein the average particle size of CuO is 4.5 nm, and the dispersion of CuO is 30.8%.

[0133] The catalyst precursor provided in this example was used to evaluate its effect in the process of selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 96%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 94%, the yield of 6-hydroxyhexanoic acid methyl ester was 90%, and the degree of hydrolysis of DMA was 0.04%.

[0134] Example 4

[0135] This embodiment provides a catalyst precursor and a preparation method thereof, wherein the catalyst precursor comprises an active component, a carrier material and a dehydrating agent CaO; the active component is Cu and Zr, and the carrier material is Al 2 O 3 A mixture of MgO and MgO;

[0136] In the catalyst precursor, the atomic ratio of Cu, Zr, Al and Mg is 5:1.5:65:30;

[0137] The added amount of CaO is 0.8 wt % of the total amount of the mixture.

[0138] The preparation method of the above catalyst precursor is as follows:

[0139] (1) copper sulfate, zirconium sulfate, aluminum sulfate, magnesium sulfate and deionized water are mixed and stirred to obtain a solution A; wherein the total concentration of the above metal salts in the solution A is 1 mol / L, and the atomic ratio of Cu, Zr, Al and Mg is 5:1.5:65:30;

[0140] Sodium carbonate, sodium hydroxide and deionized water are mixed and stirred to obtain a solution B; the total concentration of sodium carbonate and sodium hydroxide in the solution B is 1 mol / L, and the molar ratio of sodium carbonate to sodium hydroxide is 1:5;

[0141] (2) adding the solution B to the solution A by dropwise addition, controlling the pH at the end point of the dropwise addition to be 10, so that Cu, Zr, Al, and Mg are precipitated in the form of basic carbonates to obtain a mixture;

[0142] (3) stirring the mixture obtained in step (2) at 90° C. for 18 h, aging, filtering, washing, and drying;

[0143] (4) The aged mixture obtained in step (3) is calcined at 450° C. for 5 h to obtain catalyst precursor embryonic particles, which are then mixed with CaO in an amount of 0.8 wt % of the total amount of the mixture, ground into powder, formed into tablets, and ground and sieved to obtain a catalyst precursor with a mesh size of 20 to 60.

[0144] The acid site concentration of the carrier material in the catalyst precursor provided in this embodiment is 1.8 mmol / g, the basic site concentration is 1.7 mmol / g, and the ratio of the acid site concentration to the basic site concentration is 1.06:1; the average pore size of the catalyst precursor is 21.9 nm, of which the average particle size of CuO is 3.5 nm, and the dispersion of CuO is 34.5%.

[0145] The catalyst precursor provided in this example was used to evaluate its effect in the process of selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 92%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 92%, the yield of 6-hydroxyhexanoic acid methyl ester was 85%, and the degree of hydrolysis of DMA was 0.01%.

[0146] Example 5

[0147] This embodiment provides a catalyst precursor and a preparation method thereof, wherein the catalyst precursor comprises an active component, a carrier material and a dehydrating agent CaO; the active component is Cu and Mn, and the carrier material is Al 2 O 3 A mixture of MgO and MgO;

[0148] In the catalyst precursor, the atomic ratio of Cu, Mn, Al and Mg is 15:1.5:65:20;

[0149] The added amount of CaO is 0.9 wt % of the total amount of the mixture.

[0150] The preparation method of the above catalyst precursor is as follows:

[0151] (1) copper nitrate, manganese nitrate, aluminum nitrate, magnesium nitrate and deionized water are mixed and stirred to obtain a solution A; wherein the total concentration of the above metal salts in the solution A is 1 mol / L, and the atomic ratio of Cu, Mn, Al and Mg is 15:1.5:65:20;

[0152] Sodium carbonate, sodium hydroxide and deionized water are mixed and stirred to obtain a solution B; the total concentration of sodium carbonate and sodium hydroxide in the solution B is 1 mol / L, and the molar ratio of sodium carbonate to sodium hydroxide is 1:3;

[0153] (2) adding the solution B dropwise into the solution A, controlling the pH at the end point of the addition to be 9.5, so that Cu, Mn, Al, and Mg are precipitated in the form of basic carbonates to obtain a mixture;

[0154] (3) stirring the mixture obtained in step (2) at 100° C. for 24 h, aging, filtering, washing, and drying;

[0155] (4) The aged mixture obtained in step (3) is calcined at 465° C. for 3 h to obtain catalyst precursor embryonic particles, which are then mixed with CaO in an amount of 0.9 wt % of the total amount of the mixture, ground into powder, formed into tablets, and ground and sieved to obtain a catalyst precursor with a mesh size of 20 to 60.

[0156] The acid site concentration of the carrier material in the catalyst precursor provided in this embodiment is 2 mmol / g, the basic site concentration is 1.2 mmol / g, and the ratio of the acid site concentration to the basic site concentration is 1.67:1; the average pore size of the catalyst precursor is 21.8 nm, of which the average particle size of CuO is 4.7 nm, and the dispersion of CuO is 31%.

[0157] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 98%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 87%, the yield of 6-hydroxyhexanoic acid methyl ester was 85%, and the degree of hydrolysis of DMA was 0.02%.

[0158] Example 6

[0159] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0160] In the catalyst precursor, the atomic ratio of Cu, Zn, Al and Mg is 10:1:15:75;

[0161] Other conditions are the same as in Example 1.

[0162] The acid site concentration of the carrier material in the catalyst precursor provided in this embodiment is 0.6 mmol / g, the basic site concentration is 4.6 mmol / g, and the ratio of the acid site concentration to the basic site concentration is 0.13:1; the average pore size of the catalyst precursor is 22.5 nm, of which the average particle size of CuO is 4.1 nm, and the dispersion of CuO is 31.8%.

[0163] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 95%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 93%, the yield of 6-hydroxyhexanoic acid methyl ester was 88%, and the degree of hydrolysis of DMA was 0.01%.

[0164] Example 7

[0165] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0166] In the catalyst precursor, the atomic ratio of Cu, Zn, Al and Mg is 10:1:25:65;

[0167] Other conditions are the same as in Example 1.

[0168] The acidic site concentration of the support material in the catalyst precursor provided in this embodiment is 0.8 mmol / g, the basic site concentration is 3.9 mmol / g, and the ratio of the acidic site concentration to the basic site concentration is 0.21.

[0169] The average pore size of the catalyst precursor provided in this embodiment is 22.2 nm, wherein the average particle size of CuO is 4.1 nm, and the dispersion degree of CuO is 32%.

[0170] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 95%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 96%, the yield of 6-hydroxyhexanoic acid methyl ester was 91%, and the degree of hydrolysis of DMA was 0.01%.

[0171] As can be seen from Examples 6-7, the atomic ratio of Al to Mg in the catalyst precursor affects the acidic site concentration and basic site concentration of the catalyst precursor. If the atomic ratio of Al to Mg in the catalyst precursor is relatively small (Examples 6-7), the acidic site concentration of the catalyst precursor will decrease, and the basic site concentration will increase, which will eventually lead to a slight decrease in the selectivity of methyl 6-hydroxyhexanoate.

[0172] Example 8

[0173] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0174] In the catalyst precursor, the atomic ratio of Cu, Zn, Al and Mg is 10:1:50:40;

[0175] Other conditions are the same as in Example 1.

[0176] The acid site concentration of the carrier material in the catalyst precursor provided in this embodiment is 1.6 mmol / g, the basic site concentration is 1.9 mmol / g, and the ratio of the acid site concentration to the basic site concentration is 0.84; the average pore size of the catalyst precursor is 21.9 nm, of which the average particle size of CuO is 4.0 nm, and the dispersion of CuO is 32.1%.

[0177] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 95%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 95%, the yield of 6-hydroxyhexanoic acid methyl ester was 90%, and the degree of hydrolysis of DMA was 0.01%.

[0178] Example 9

[0179] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0180] In the catalyst precursor, the atomic ratio of Cu, Zn, Al and Mg is 10:1:65:25;

[0181] Other conditions are the same as in Example 1.

[0182] The acid site concentration of the carrier material in the catalyst precursor provided in this embodiment is 1.9 mmol / g, the basic site concentration is 1.3 mmol / g, and the ratio of the acid site concentration to the basic site concentration is 1.46; the average pore size of the catalyst precursor is 21.6 nm, of which the average particle size of CuO is 4.0 nm, and the dispersion of CuO is 32.1%.

[0183] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 94%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 89%, the yield of 6-hydroxyhexanoic acid methyl ester was 84%, and the degree of hydrolysis of DMA was 0.01%.

[0184] As can be seen from Examples 8-9, the atomic ratio of Al to Mg in the catalyst precursor affects the acidic site concentration and basic site concentration of the catalyst precursor. If the atomic ratio of Al to Mg in the catalyst precursor is relatively large (Examples 8-9), the acidic site concentration of the catalyst precursor will increase, and the basic site concentration will decrease, which will eventually lead to a slight decrease in the selectivity and yield of methyl 6-hydroxyhexanoate.

[0185] At the same time, it can be seen from the contents of Example 1 and Examples 6-9 that the present invention can adjust the acid site concentration and the basic site concentration of the support material by regulating the atomic ratio of Cu, M, Al, and Mg in the catalyst precursor, and further control the ratio of the acid site concentration and the basic site concentration of the support material within a specific range (Example 1), which can further improve the selectivity of 6-hydroxyhexanoic acid methyl ester.

[0186] Example 10

[0187] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0188] The calcination temperature in step (4) is 400°C;

[0189] Other conditions are the same as in Example 1.

[0190] The acid site concentration of the carrier material in the catalyst precursor provided in this embodiment is 1.6 mmol / g, the basic site concentration is 3.6 mmol / g, and the ratio of the acid site concentration to the basic site concentration is 0.44; the average pore size of the catalyst precursor is 15 nm, of which the average particle size of CuO is 3.8 nm, and the dispersion of CuO is 34.5%.

[0191] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 96%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 86%, the yield of 6-hydroxyhexanoic acid methyl ester was 83%, and the degree of hydrolysis of DMA was 0.01%.

[0192] It can be seen from Example 10 that if the calcination temperature of the catalyst precursor is reduced, the average pore size of the catalyst precursor will also decrease, which will lead to lower selectivity and yield of methyl 6-hydroxyhexanoate.

[0193] Embodiment 11

[0194] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0195] The calcination temperature in step (4) is 550°C;

[0196] Other conditions are the same as in Example 1.

[0197] The catalyst precursor provided in this embodiment has an acid site concentration of 1 mmol / g, a basic site concentration of 2.6 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.38; the average pore size of the catalyst precursor is 25 nm, of which the average particle size of CuO is 4.3 nm, and the dispersion of CuO is 31.2%.

[0198] The catalyst precursor provided in this example was used to evaluate its effect in the process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA. The conversion rate of DMA was 85%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 94%, the yield of 6-hydroxyhexanoic acid methyl ester was 80%, and the degree of hydrolysis of DMA was 0.01%.

[0199] It can be seen from this embodiment that if the calcination temperature of the catalyst precursor is increased, the average pore size of the catalyst precursor will also increase accordingly, but the concentrations of acidic and basic sites of the catalyst precursor are low, resulting in a decrease in the conversion rate of DMA, the selectivity and yield of methyl 6-hydroxyhexanoate.

[0200] Example 12

[0201] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0202] The calcination temperature in step (4) is 380°C;

[0203] Other conditions are the same as in Example 1.

[0204] The catalyst precursor provided in this embodiment has an acid site concentration of 1.8 mmol / g, a basic site concentration of 5 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.36; the average pore size of the catalyst precursor is 12 nm, of which the average particle size of CuO is 3.7 nm, and the dispersion of CuO is 37%.

[0205] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 95%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 80%, the yield of 6-hydroxyhexanoic acid methyl ester was 76%, and the degree of hydrolysis of DMA was 0.01%.

[0206] It can be seen from this embodiment that if the calcination temperature of the catalyst precursor is too low, the average pore size of the catalyst precursor will be too small, thereby causing a significant decrease in the selectivity and yield of methyl 6-hydroxyhexanoate.

[0207] Embodiment 13

[0208] This embodiment provides a catalyst precursor and a preparation method thereof, which differs from Embodiment 1 only in that:

[0209] The catalyst precursor does not contain a dehydrating agent, CaO;

[0210] Other conditions are the same as in Example 1.

[0211] The acid site concentration of the carrier material in the catalyst precursor provided in this embodiment is 1.3 mmol / g, the basic site concentration is 2.9 mmol / g, and the ratio of the acid site concentration to the basic site concentration is 0.45; the average pore size of the catalyst precursor is 22 nm, of which the average particle size of CuO is 4 nm, and the dispersion of CuO is 32%.

[0212] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 93%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 88%, the yield of 6-hydroxyhexanoic acid methyl ester was 82%, and the degree of hydrolysis of DMA was 0.20%.

[0213] The dehydrating agent can react with the trace amount of water in the raw material DMA, inhibit the hydrolysis of DMA, and avoid the formation of monomethyl adipate or adipic acid. As can be seen from this embodiment, if the dehydrating agent is not used, the degree of hydrolysis of DMA is high, and the hydrolysis of DMA will generate monomethyl adipate or adipic acid, etc., which will lead to a decrease in the selectivity and yield of methyl 6-hydroxycaproate.

[0214] Comparative Example 1

[0215] This comparative example provides a catalyst precursor and a preparation method thereof, which differs from Example 1 only in that:

[0216] In the catalyst precursor, the atomic ratio of Cu, Zn, Al and Mg is 10:1:5:85;

[0217] Other conditions are the same as in Example 1.

[0218] The catalyst precursor provided in this comparative example has an acid site concentration of 0.2 mmol / g, a basic site concentration of 5.5 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.04; the average pore size of the catalyst precursor is 22.8 nm, wherein the average particle size of CuO is 4.1 nm, and the dispersion of CuO is 32.3%.

[0219] The catalyst precursor provided in this comparative example was used to evaluate its effect in the process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA. The conversion rate of DMA was 86%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 75%, the yield of 6-hydroxyhexanoic acid methyl ester was 65%, and the degree of hydrolysis of DMA was 0.01%.

[0220] It can be seen from this comparative example that if the Al:Mg atomic ratio in the catalyst precursor is too small, the acid site concentration of the catalyst precursor carrier material will be too small and the basic site concentration will be too large, which will lead to a low conversion rate of DMA and a low selectivity and yield of methyl 6-hydroxyhexanoate.

[0221] Comparative Example 2

[0222] This comparative example provides a catalyst precursor and a preparation method thereof, which differs from Example 1 only in that:

[0223] In the catalyst precursor, the atomic ratio of Cu, Zn, Al and Mg is 10:1:85:5;

[0224] Other conditions are the same as in Example 1.

[0225] The catalyst precursor provided in this comparative example has an acid site concentration of 2.8 mmol / g, a basic site concentration of 0.3 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 9.33; the average pore size of the catalyst precursor is 22.5 nm, of which the average particle size of CuO is 3.9 nm, and the dispersion of CuO is 32.5%.

[0226] The catalyst precursor provided in this comparative example was used to evaluate its effect in the process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA. The conversion rate of DMA was 89%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 68%, the yield of 6-hydroxyhexanoic acid methyl ester was 61%, and the degree of hydrolysis of DMA was 0.01%.

[0227] It can be seen from this comparative example that if the Al:Mg atomic ratio in the catalyst precursor is too large, the acidic site concentration of the catalyst precursor carrier material will be too high and the basic site concentration will be too low, which will lead to a low conversion rate of DMA and a low selectivity and yield of methyl 6-hydroxyhexanoate.

[0228] Comparative Example 3

[0229] This comparative example provides a catalyst precursor and a preparation method thereof, wherein the catalyst precursor comprises an active component and a carrier material; the active component is CuO and ZnO, and the carrier material is Al2O3 modified by MgO. 2 O 3The atomic ratio of Cu, Zn, Al and Mg in the catalyst precursor is 10:1:30:60.

[0230] The preparation method of the above catalyst precursor is as follows:

[0231] (1) mixing a prescribed amount of aluminum hydroxide dry gel and water to prepare an aluminum hydroxide dry gel suspension, stirring at 70° C. to uniformly disperse the mixture, to obtain a solution A, wherein the concentration of aluminum hydroxide in the solution A is 0.3 mol / L;

[0232] Copper nitrate, zinc nitrate, magnesium nitrate and deionized water are mixed and stirred to obtain a solution B; wherein the total concentration of the nitrates in the solution B is 1 mol / L, and the atomic ratio of Cu, Zn, Al and Mg is controlled to be 10:1.0:30:60;

[0233] Mixing sodium carbonate, sodium hydroxide and deionized water to obtain a solution and stirring it evenly to obtain a solution C; the total concentration of sodium carbonate and sodium hydroxide in the solution C is 1 mol / L, and the molar ratio of sodium carbonate to sodium hydroxide is 1:3;

[0234] (2) adding solution B and solution C to solution A simultaneously under stirring at 80° C., controlling the pH at the end point of the addition to be 9-10, so that Cu, M, and Mg are precipitated on the surface of aluminum hydroxide in the form of basic carbonates to obtain a mixture;

[0235] (3) stirring the mixture obtained in step (2) at 90° C. for 15 h, aging, filtering, washing, and drying;

[0236] (4) The aged mixture obtained in step (3) is calcined at 450° C. for 5 h to obtain catalyst precursor embryonic particles, which are then mixed with CaO in an amount of 1 wt% of the total amount of the mixture, ground into powder, formed into tablets, and ground and sieved to obtain a catalyst precursor with a mesh size of 20 to 60.

[0237] The catalyst precursor provided in this comparative example has an acid site concentration of 0.2 mmol / g, a basic site concentration of 2 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.10; the average pore size of the catalyst precursor is 17 nm, of which the average particle size of CuO is 3.5 nm, and the dispersion of CuO is 34.2%.

[0238] The catalyst precursor provided in this comparative example was used to evaluate its effect in the process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA. The conversion rate of DMA was 75%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 60%, the yield of 6-hydroxyhexanoic acid methyl ester was 45%, and the degree of hydrolysis of DMA was 0.01%.

[0239] From this comparative example, it can be seen that the alkaline MgO is loaded on the acidic Al 2 O 3 The surface will destroy the ideal distribution of acid and base sites, resulting in the catalyst precursor support material having an acid site concentration that is too low and an alkaline site concentration that is too high, which in turn leads to a low conversion rate of DMA and a low selectivity and yield of methyl 6-hydroxyhexanoate.

[0240] Comparative Example 4

[0241] This comparative example provides a catalyst precursor and a preparation method thereof, wherein the catalyst precursor comprises an active component, a carrier material and a dehydrating agent CaO; the active component is an oxide of Cu and Ba, and the carrier material is Al 2 O 3 A mixture of MgO and MgO;

[0242] In the catalyst precursor, the atomic ratio of Cu, Ba, Al, and Mg is 10:1:30:60;

[0243] The added amount of CaO is 1 wt % of the total amount of the mixture.

[0244] The only difference between the preparation method of the catalyst precursor and Example 1 is that the zinc nitrate in step (1) is replaced by calcium nitrate, so that the atomic ratio of Cu, Ba, Al, and Mg in solution A is 10:1:30:60;

[0245] Other conditions are the same as in Example 1.

[0246] The catalyst precursor provided in this comparative example has an acid site concentration of 1.4 mmol / g, a basic site concentration of 3.3 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.42; the average pore size of the catalyst precursor is 22.4 nm, wherein the average particle size of CuO is 3.9 nm, and the dispersion of CuO is 32.3%.

[0247] The catalyst precursor provided in this comparative example was used to evaluate its effect in the process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA. The conversion rate of DMA was 89%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 65%, the yield of 6-hydroxyhexanoic acid methyl ester was 58%, and the degree of hydrolysis of DMA was 0.01%.

[0248] It can be seen from this comparative example that if other metal oxides (such as Ca oxide) are selected as the active component of the catalyst precursor, the conversion rate of DMA will be lower, and the selectivity and yield of methyl 6-hydroxyhexanoate will also be lower.

[0249] Comparative Example 5

[0250] This comparative example provides a catalyst precursor and a preparation method thereof, which is different from Example 1 only in that the carrier material of the catalyst precursor is only Al 2 O 3 ;

[0251] In the catalyst precursor, the atomic ratio of Cu, Zn and Al is 10:1.0:30;

[0252] Magnesium nitrate is not used in step (1);

[0253] Other conditions are the same as in Example 1.

[0254] The catalyst precursor provided in this comparative example has an acid site concentration of 1.3 mmol / g, a basic site concentration of 0.1 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 13.00; the average pore size of the catalyst precursor is 215 nm, wherein the average particle size of CuO is 3.8 nm, and the dispersion of CuO is 32.9%.

[0255] The catalyst precursor provided in this comparative example was used to evaluate its effect in the process of preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA. The conversion rate of DMA was 99%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 30%, the yield of 6-hydroxyhexanoic acid methyl ester was 30%, and the degree of hydrolysis of DMA was 0.01%.

[0256] It can be seen from this comparative example that if only Al 2 O 3 As a carrier material of the catalyst precursor, the basic site concentration of the catalyst precursor is too low, which ultimately leads to too low selectivity and yield of 6-hydroxyhexanoic acid methyl ester.

[0257] Comparative Example 6

[0258] This comparative example provides a catalyst precursor and a preparation method thereof, which differs from Example 1 only in that:

[0259] The calcination temperature in step (4) is 600°C;

[0260] Other conditions are the same as in Example 1.

[0261] The catalyst precursor provided in this comparative example has an acid site concentration of 0.3 mmol / g, a basic site concentration of 0.8 mmol / g, and a ratio of the acid site concentration to the basic site concentration of 0.38; the average pore size of the catalyst precursor is 30 nm, of which the average particle size of CuO is 5.1 nm, and the dispersion of CuO is 29%.

[0262] The catalyst precursor provided in this example was used to evaluate its effect in the selective hydrogenation of DMA to prepare 6-hydroxyhexanoic acid methyl ester. The conversion rate of DMA was 80%, the selectivity of 6-hydroxyhexanoic acid methyl ester was 85%, the yield of 6-hydroxyhexanoic acid methyl ester was 68%, and the degree of hydrolysis of DMA was 0.01%.

[0263] It can be seen from this comparative example that if the calcination temperature is too high during the preparation of the catalyst precursor, the acid site concentration and the basic site concentration of the catalyst precursor will be low, the average pore size of the catalyst precursor will be too high, the average particle size of CuO in the catalyst precursor will be slightly larger, and the dispersion will be slightly lower, which will lead to a lower conversion rate of DMA and a lower selectivity and yield of methyl 6-hydroxyhexanoate.

[0264] In summary, the present invention designs the composition of the catalyst precursor, further controls the atomic ratio of Cu, M, Al, and Mg in the catalyst precursor within a specific range, and includes Al 2 O 3 A mixture of MgO and MgO is used as a carrier material, and the acid site concentration and the basic site concentration of the carrier material are controlled within a specific range. After the catalyst precursor is activated, a catalyst with excellent performance and high selectivity is obtained, and DMA selective hydrogenation can be used to prepare 6-hydroxyhexanoic acid methyl ester. The conditions for preparing 6-hydroxyhexanoic acid methyl ester using the catalyst are relatively mild, the process is simple, and industrialization is easier to carry out.

[0265] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A catalyst precursor, It is characterized in that The catalyst precursor includes an active component and a support material; The active ingredients are oxides of CuO and M; The M is selected from at least one of Group IVA, Group IB, Group IIB, Group IVB, Group VIB, Group VIIB or Group VIII metal ions, and M is not Cu; The support material comprises Al 2 O 3 A mixture of MgO and MgO; The acidic site concentration of the carrier material is 0.5 to 2 mmol / g, and the basic site concentration is 1 to 5 mmol / g; The atomic ratio of Cu, M, Al and Mg in the catalyst precursor is 5-15:0.5-1.5:15-65:20-80, and the sum of the atomic ratios of Cu, Al and Mg in the catalyst precursor is 100.

2. The catalyst precursor according to claim 1, It is characterized in that The M is selected from any one of Fe, Zn, Co, Mn and Zr, or a combination of at least two thereof.

3. The catalyst precursor according to claim 1 or 2, It is characterized in that The ratio of the acid site concentration to the basic site concentration of the carrier material is 0.2 to 0.8:

1.

4. The catalyst precursor according to any one of claims 1 to 3, It is characterized in that The average pore diameter of the catalyst precursor is ≥15 nm.

5. The catalyst precursor according to any one of claims 1 to 4, It is characterized in that The average particle size of CuO in the catalyst precursor is 3 to 5 nm; Preferably, the dispersion degree of CuO in the catalyst precursor is 30-35%.

6. The catalyst precursor according to any one of claims 1 to 5, It is characterized in that The catalyst precursor also includes a dehydrating agent; Preferably, the dehydrating agent comprises CaO; Preferably, based on the sum of the mass percentages of the active ingredient and the carrier material being 100%, the mass percentage content of the water remover is 0.5-1%.

7. A method for preparing a catalyst precursor according to any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: (1) mixing a soluble copper salt, a soluble salt containing M, a soluble magnesium salt, a soluble aluminum salt and water to obtain a solution A; Mixing the precipitant and water to obtain solution B; (2) adding the solution B dropwise into the solution A, and precipitating Cu, M, Al, and Mg in the form of basic carbonates to obtain a mixture; (3) aging the mixture obtained in step (2); (4) calcining the aged mixture in step (3) to obtain catalyst precursor embryos, and then grinding the obtained embryos to obtain the catalyst precursor.

8. The preparation method according to claim 7, It is characterized in that The calcination temperature is 400-550°C; Preferably, the calcination time is ≥3h.

9. A method for preparing 6-hydroxyhexanoic acid methyl ester by selective hydrogenation of DMA, It is characterized in that The method comprises the following steps: (S1) reducing the catalyst precursor according to any one of claims 1 to 6 until all CuO is reduced to Cu; (S2) placing the catalyst obtained by reduction treatment in step (S1) in a reaction system, introducing hydrogen, and adding DMA to the reaction system under a hydrogen atmosphere to react to obtain methyl 6-hydroxyhexanoate.

10. A catalyst, It is characterized in that The catalyst is obtained by subjecting the catalyst precursor according to any one of claims 1 to 6 to reduction treatment, wherein the CuO in the catalyst is reduced to Cu, and other metal oxides are still in an oxidized state.

Citation Information

Patent Citations

  • Catalyst for hydrogenation of adipate to produce 1,6-hexanediol, and preparation method thereof

    CN110560072A

  • Supported CO2 hydrogenation catalyst and preparation method thereof

    CN112403474A

  • Method for producing 1,6-hexanediol and 6-hydroxycaproic acid or their esters

    CN1257470A

  • Method for producing aldehyde

    US20160289151A1

  • Catalyst for catalytically hydrogenating co2 to methanol and preparation thereof

    WO2012040977A1