Method for synthesizing P / Cd0. 25Zn0. 75S composite material by hydrothermal method

By doping P elements in sulfhydryl zinc cadmium catalyst and synthesizing P/Cd0.25Zn0.75S composite material by hydrothermal method, the photocorrosion and carrier recombination of the catalyst were solved, and efficient and stable photocatalytic hydrogen production effect was achieved. , has promoted the development of renewable energy technology.

CN118904367AInactive Publication Date: 2024-11-08NANCHANG HANGKONG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410924473.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The unmodified Cd1-xZnxS catalyst has rapid carrier recombination and severe photocorrosion problems, resulting in undesirable catalytic activity and poor stability, which limits its application in photocatalytic decomposition of water to produce hydrogen.

Method used

The P element is doped into the Cd0.25Zn0.75S nanorod by hydrothermal method, and the structural morphology of sulfhydryl zinc cadmium material is regulated, and the efficient and stable P/Cd0.25Zn0.75S composite material is synthesized to improve the conductivity of the photocatalyst and Electron-hole separation efficiency.

Benefits of technology

The photocatalytic hydrogen production efficiency and stability are significantly improved, and the hydrogen production rate of the 0.3-P/Cd0.25Zn0.75S composite material reaches three times that of pure Cd0.25Zn0.75S, and has good cycling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904367A_ABST
    Figure CN118904367A_ABST
Patent Text Reader

Abstract

The invention discloses a method for synthesizing a P / Cd0. 25Zn0. 75S composite material by using a hydrothermal method. The P element is doped into a Cd0. 25Zn0. 75S nanorod by using the hydrothermal method, the P / Cd0. 25Zn0. 75S composite material is synthesized, and the photocatalytic hydrogen production performance of the P / Cd0. 25Zn0. 75S composite material is researched. The photocatalytic hydrogen production performance of the 3-P / Cd < 0.25 > Zn < 0.75 > S composite material synthesized by the method can reach 2343.75 [mu] mol g <-1 > h <-1 >, and is about 3 times that of pure Cd < 0.25 > Zn < 0.75 > S (781.25 [mu] mol g <-1 > h <-1 >).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for synthesizing P / Cd by hydrothermal method. 0.25 Zn 0.75 The invention relates to a method for preparing a photocatalytic hydrogen-producing composite material, and belongs to the technical field of photocatalytic hydrogen production. Background Art

[0002] Sulfur zinc cadmium (Cd 1-x Zn x Cd(S) is a semiconductor catalyst. It has become one of the most promising metal sulfide materials for photocatalytic water decomposition to produce hydrogen due to its unique catalytic properties such as narrow band gap and good visible light response. 1-x Zn x S catalysts have problems of rapid carrier recombination and severe photocorrosion, which lead to unsatisfactory catalytic activity and poor stability, limiting their further application. 1-x Zn x The performance of S can be theoretically improved by changing Cd 1-x Zn x The microstructure of S can achieve better separation of photogenerated electron-hole pairs, and more effective charge separation can be achieved by building a heterojunction to expand the light absorption range. The present invention explores the method of P element doping to regulate the structural morphology of sulfur-zinc-cadmium materials to synthesize a photocatalyst with excellent hydrogen evolution performance.

[0003] Studies have shown that P doping can improve material performance. P doping can not only improve the conductivity of photocatalysts, but also reduce the bandgap and effectively inhibit the recombination of electron-hole pairs, promoting the generation of photogenerated electrons. Therefore, the development of P / CdZnS composite materials and further achieving a good combination with co-catalysts will hopefully improve the efficiency and stability of photocatalytic hydrogen production materials and promote the development of renewable energy technologies.

[0004] Taking all the above into consideration, we doped P into Cd by a simple hydrothermal method. 0.25 Zn 0.75 S nanorods, synthesized efficient and stable composite hydrogen production photocatalyst. When the P doping amount is 0.3%, P / Cd 0.25 Zn 0.75 The hydrogen production efficiency of the S(P / CdZnS) composite material is the highest, which is higher than that of pure Cd 0.25 Zn 0.75 Therefore, this innovation provides a new way to synthesize photocatalysts characterized by improved electron-hole separation efficiency. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a hydrothermal method for synthesizing P / Cd0.25 Zn 0.75 The method of preparing S composite materials is used to solve the shortcomings of the previous technology such as complex synthesis process and high overall cost of catalysts, and provides a new idea of ​​heteroatom doping for the synthesis of efficient and stable photocatalytic water decomposition hydrogen production system without precious metals.

[0006] The present invention is achieved by the following scheme: a hydrothermal method for synthesizing P / Cd 0.25 Zn 0.75 The method for preparing a composite material of S comprises the following steps:

[0007] Step 1: 1.0 mmol CdCl 2 ·5H 2 O was dissolved in 27 mL C 2 H 8 N 2 The solution was stirred for 10 min.

[0008] Step 2: Add 3.0 mmol ZnCl 2 6H 2 O and continued stirring for 25 min, then 4.0 mmol C 2 H 5 NS and continue stirring for 30 min;

[0009] Step 3: Transfer the mixed solution to a 50 ml Teflon-lined stainless steel autoclave and hydrotherm at 180°C for 24 h. After the product is cooled to room temperature, wash it three times with deionized water and ethanol respectively, and finally place the sample in a vacuum drying oven at 60°C to dry overnight. 0.25 Zn 0.75 S powder;

[0010] Step 4: Weigh 0.5 mmol Cd 0.25 Zn 0.75 S monomer was dissolved in a beaker containing 30 mL of deionized water and stirred for 10 min;

[0011] Step 5: Add 1.49 mg, 2.24 mg, and 2.99 mg of NaHCO3 to the doping ratio of P element at 0.2%, 0.3%, and 0.4%, respectively. 2 PO 2 ·H 2 O, and continue stirring for 30 min;

[0012] Step 6. Transfer the mixed solution to a 50 ml Teflon-lined stainless steel autoclave and hydroheat at 160°C for 12 h. After the product is cooled to room temperature, wash it three times with deionized water and ethanol respectively. Finally, place the sample in a vacuum drying oven at 60°C and dry it overnight. According to the doping content of the P element, they are named 0.2-P / CdZnS, 0.3-P / CdZnS and 0.4-P / CdZnS respectively.

[0013] The CdCl 2 ·5H 2 O, provided by MACKLIN; the ZnCl 2 6H 2 O, provided by MACKLIN; the C 2 H 8 N 2 , provided by MACKLIN; the C 2 H 5 NS, provided by MACKLIN; the NaH 2 PO 2 ·H 2 O, provided by MACKLIN.

[0014] The NaH 2 PO 2 ·H 2 O, provided by MACKLIN.

[0015] In the step 4, the hydrothermal reaction was carried out at 180°C for 24 hours to obtain Cd 0.25 Zn 0.75 S monomer.

[0016] In the step six, the obtained samples are named as 0.2-P / CdZnS, 0.3-P / CdZnS and 0.4-P / CdZnS according to the mass percentage of the doping elements P and CdZnS.

[0017] In the step 6, the P element is added and maintained at a high temperature of 160°C. The heating reaction time is 12 hours to obtain P / Cd 0.25 Zn 0.75 S(P / CdZnS) composite materials,

[0018] The beneficial effects of the present invention are:

[0019] The present invention starts from the perspective of doping non-precious metal element photocatalytic materials, and uses a hydrothermal method to dope P element into Cd 0.25 Zn 0.75S nanorods, by reducing the band gap, promoting the generation of photogenerated electrons; and effectively inhibiting the recombination of electron-hole pairs. At the same time, the amount of P used is very small, only 0.3% content, the cost is low, but the resulting 0.3-P-CdZnS composite material shows significantly improved photocatalytic activity, and the hydrogen production rate under 300W xenon light is about the same as that of pure Cd 0.25 Zn 0.75 S is 3 times, and 0.3-P / Cd 0.25 Zn 0.75 The S composite material has good stability, and the hydrogen production rate per cycle is 2343.75 μmol g -1 h -1 The secondary cycle hydrogen production rate is as high as 2053.27 μmol g -1 h -1 , which can be recycled many times. Therefore, this work provides a new way to synthesize photocatalysts characterized by improving the efficiency of electron-hole separation. At the same time, this work also provides a new idea of ​​heteroatom doping for the synthesis of efficient photocatalytic water decomposition and hydrogen production system without precious metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The xP / Cd prepared in Example 1 0.25 Zn 0.75 S hydrogen production rate diagram under simulated sunlight;

[0021] Figure 2 The 0.3-P / Cd prepared in Example 1 0.25 Zn 0.75 S hydrogen production performance cycle diagram under simulated sunlight. DETAILED DESCRIPTION

[0022] The present invention is further described below by way of examples. The composites prepared in Examples 1-2 are prepared by using xP / Cd 0.25 Zn 0.75 S represents, x represents doping elements P and Cd 0.25 Zn 0.75 Mass percentage of S.

[0023] Example 1

[0024] (1) Cd 0.25 Zn 0.75 Synthesis of S(CdZnS) Nanorods

[0025] 1) 1.0mmol CdCl 2 ·5H 2 O was dissolved in 27 mL C 2 H 8 N 2The solution was stirred for 10 min.

[0026] 2) Add 3.0 mmol ZnCl 2 6H 2 O and continued stirring for 25 min. Then 4.0 mmol C 2 H 5 NS and continue stirring for 30 min.

[0027] 3) The mixed solution was transferred to a 50 ml Teflon-lined stainless steel autoclave and hydrothermal at 180 °C for 24 h. After the product cooled to room temperature, it was washed three times with deionized water and ethanol respectively, and finally the sample was placed in a vacuum drying oven at 60 °C and dried overnight. 0.25 Zn 0.75 S monomer.

[0028] (2)P / Cd 0.25 Zn 0.75 Synthesis of S(P / CdZnS) Composites

[0029] 4) Weigh 0.5mmol Cd 0.25 Zn 0.75 S monomer was dissolved in a beaker containing 30 mL of deionized water and stirred for 10 min.

[0030] 5) According to the doping ratio of P element 0.2%, 0.3%, and 0.4%, 1.49 mg, 2.24 mg, and 2.99 mg of NaH were added respectively. 2 PO 2 ·H 2 O and continue stirring for 30 min.

[0031] 6) The mixed solution was transferred to a 50 ml Teflon-lined stainless steel autoclave and hydrothermal at 160°C for 12 h. After the product cooled to room temperature, it was washed three times with deionized water and ethanol respectively, and finally the sample was placed in a vacuum drying oven at 60°C and dried overnight. According to the doping content of P element, it was named 0.2-P / Cd 0.25 Zn 0.75 S, 0.3-P / Cd 0.25 Zn 0.75 S and 0.4-P / Cd 0.25 Zn 0.75 S.

[0032] Weigh 10 mg of catalyst (0.3-P / Cd 0.25 Zn 0.75S) was evenly dispersed in a reactor containing 8 mL of deionized water and 2 mL of triethanolamine, and then argon was continuously injected into the reactor for 30 min while stirring to ensure that the reactor was filled with argon. A 300 W xenon lamp was used as the light source. After the reaction process lasted for 2 h, the efficiency of generating hydrogen was 2343.75 μmol g -1 h -1 .

[0033] The product obtained in Example 1 produces hydrogen under light (λ≥380nm) to evaluate Cd 0.25 Zn 0.75 S and 0.3-P / Cd 0.25 Zn 0.75 The photocatalytic performance of S is shown in Figure 1 Among them, pure Cd 0.25 Zn 0.75 The hydrogen production rate of S is 781.25 μmol g -1 h -1 , and the 0.3-P / Cd synthesized by the hydrothermal method described in the present invention 0.25 Zn 0.75 The hydrogen production performance of S was significantly improved, reaching 2343.75 μmol g -1 h -1 This shows that this method can dope P into CdZnS, and P acts as a catalyst to effectively increase the 0.25 Zn 0.75 The photocatalytic hydrogen production performance of S. And 0.3-P / Cd 0.25 Zn 0.75 The S composite material exhibited good hydrogen production cycle stability.

[0034] Although the technical solutions of the present invention have been described and listed in detail, it should be understood that it is obvious to those skilled in the art to make modifications to the above embodiments or adopt equivalent alternatives. These modifications or improvements made without departing from the spirit of the present invention are within the scope of protection required by the present invention.

Claims

1. A hydrothermal method for the synthesis of P / Cd 0.25 Zn 0.75 The method for preparing a composite material of S comprises the following steps: Step 1: Dissolve 1.0 mmol CdCl2·5H2O in 27 mL C2H8N2 solution and continue stirring for 10 min; Step 2: Add 3.0 mmol ZnCl2·6H2O and continue stirring for 25 min, then add 4.0 mmol C2H5NS to the solution and continue stirring for 30 min; Step 3: Transfer the mixed solution to a 50 ml Teflon-lined stainless steel autoclave and hydrotherm at 180°C for 24 h. After the product is cooled to room temperature, wash it three times with deionized water and ethanol respectively, and finally place the sample in a vacuum drying oven at 60°C to dry overnight. 0.25 Zn 0.75 S powder; Step 4: Weigh 0.5mmolCd 0.25 Zn 0.75 S monomer was dissolved in a beaker containing 30 mL of deionized water and stirred for 10 min; Step 5: Add 1.49 mg, 2.24 mg, and 2.99 mg of NaH2PO2·H2O respectively according to the doping ratio of P element 0.2%, 0.3%, and 0.4%, and continue stirring for 30 minutes; Step 6. Transfer the mixed solution to a 50 ml Teflon-lined stainless steel autoclave and hydroheat at 160°C for 12 h. After the product is cooled to room temperature, wash it three times with deionized water and ethanol respectively. Finally, place the sample in a vacuum drying oven at 60°C and dry it overnight. According to the doping content of the P element, they are named 0.2-P / CdZnS, 0.3-P / CdZnS and 0.4-P / CdZnS respectively.

2. A hydrothermal synthesis of P / Cd according to claim 1 0.25 Zn 0.75 S composite material method, characterized in that: The CdCl2·5H2O is provided by MACKLIN; the ZnCl2·6H2O is provided by MACKLIN; the C2H8N2 is provided by MACKLIN; the C2H5NS is provided by MACKLIN; and the NaH2PO2·H2O is provided by MACKLIN.

3. A hydrothermal synthesis of P / Cd according to claim 1 0.25 Zn 0.75 S composite material method, characterized in that: The NaH2PO2·H2O is provided by MACKLIN Company.

4. A hydrothermal synthesis of P / Cd according to claim 1 0.25 Zn 0.75 S composite material method, characterized in that: In the step 4, the hydrothermal reaction was carried out at 180°C for 24 hours to obtain Cd 0.25 Zn 0.75 S monomer.

5. A hydrothermal synthesis of P / Cd according to claim 1 0.25 Zn 0.75 S composite material method, characterized in that: In the step six, the obtained samples are named as 0.2-P / CdZnS, 0.3-P / CdZnS and 0.4-P / CdZnS according to the mass percentage of the doping elements P and CdZnS.

6. A hydrothermal synthesis of P / Cd according to claim 1 0.25 Zn 0.75 S composite material method, characterized in that: In the step 6, the P element is added and maintained at a high temperature of 160°C. The heating reaction time is 12 hours to obtain P / Cd 0.25 Zn 0.75 S (P / CdZnS) composite materials.