Method for improving quality and reducing fluorine of copper-sulfur concentrate product

Through pretreatment, flotation, neutralization reaction and precipitation treatment, the fluorine content in copper-sulfur concentrate is reduced, and the problems of fluoride pollution and smelting difficulty in traditional copper-sulfur concentrate are solved, thus achieving low-cost and low-fluorine content Copper-sulfur concentrate products improve smelting efficiency and environmental protection.

CN118904524APending Publication Date: 2024-11-08GUANGDONG PROVINCE DABAOSHAN MINING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410904994.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional copper-sulfur concentrates contain higher fluoride, which increases the difficulty of smelting and may cause pollution to the environment. It also reacts less heat during the smelting process, and additional fuel needs to be supplemented to maintain energy balance.

Method used

A method for improving the quality of copper sulfur concentrate products is adopted, including pretreatment, flotation removal, neutralization reaction to reduce fluorine, precipitation reaction to reduce fluorine, filtration, washing and drying steps, using sodium hydroxide solution and calcium salt solution The fluoride is produced separately and the fluoride content is reduced by precipitation and filtration.

Benefits of technology

It significantly reduces the fluorine content in copper-sulfur concentrate to below 0.1%, improves the quality of mineral products, is simple to operate and low cost, and is suitable for the smelting process of copper-sulfur concentrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904524A_ABST
    Figure CN118904524A_ABST
Patent Text Reader

Abstract

The invention discloses a quality-improving and fluorine-reducing method for a copper-sulfur concentrate product, and relates to the field of mineral processing. Comprising the following steps: pretreatment: crushing and grinding copper-sulfur concentrate; flotation impurity removal is conducted, specifically, the pretreated copper-sulfur concentrate is added into a flotation machine, a collecting agent and a foaming agent are added, and flotation impurity removal is conducted; the flotation concentrate is added into a neutralization reaction tank, a sodium hydroxide solution is added for a neutralization reaction, fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate water-soluble sodium fluoride, and the fluorine content in the copper-sulfur concentrate is reduced; and performing precipitation reaction to reduce fluorine, and after the neutralization reaction is completed, adding a calcium salt solution into the reaction tank to perform precipitation reaction. The fluorine content in the copper-sulfur concentrate can be remarkably reduced to 0.1% or below, meanwhile, the quality of the copper-sulfur concentrate is remarkably improved, and the method has the advantages of being easy to operate, low in cost, remarkable in effect and the like and can be widely applied to the smelting process of the copper-sulfur concentrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mineral processing, and in particular to a method for improving the quality and reducing fluorine in copper-sulfur concentrate products. Background Art

[0002] Copper sulfide concentrate, also known as chalcopyrite or copper sulfide ore, is an important mineral resource.

[0003] Copper sulfide concentrate has the characteristics of high copper grade, which enables a higher metal recovery rate to be obtained during the smelting process, whether using pyrometallurgical or hydrometallurgical smelting process.

[0004] The S / Cu ratio of copper sulfide concentrate is lower, which means that during the smelting process, the reaction is less exothermic and additional fuel may be needed to maintain energy balance.

[0005] The Fe / SiO2 ratio in the copper concentrate is also low, which helps reduce impurity levels during the smelting process.

[0006] The smelting process of copper sulfide concentrate mainly includes pyrometallurgy and hydrometallurgy. Pyrometallurgy usually does not require matte smelting, and can be directly blown into crude copper or reduced into crude copper by electric furnace after roasting and desulfurization. Hydrometallurgy requires converting copper sulfide into water-soluble copper oxide, and then extracting metallic copper by electrolysis and other methods.

[0007] However, traditional copper-sulfur concentrates often contain high levels of fluoride, which not only increases the difficulty of smelting but also may cause environmental pollution.

[0008] To this end, the present invention proposes a method for improving the quality of copper-sulfur concentrate products and reducing fluorine. Summary of the invention

[0009] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for improving the quality of copper-sulfur concentrate products and reducing fluorine.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0012] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0013] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0014] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0015] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0016] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0017] Preferably: in the step S2, the concentration of the flotation pulp is 25%-30%, and the aeration volume is 0.2-0.3m 3 / min, the flotation stirring speed is 150-200r / min.

[0018] Preferably: in the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

[0019] Preferably, the xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0020] Preferably: the foaming agent in step S2 is any one or more combinations of saponins, pine oil, butanol, octanol, propanol and pentanol.

[0021] Preferably: in the step S3, the concentration of the sodium hydroxide solution is 10%-15%, and the reaction time is 1-2h.

[0022] Preferably: in the step S4, the calcium salt solution is any one or more combinations of calcium chloride, calcium nitrate, calcium sulfate, calcium hydrogen phosphate, and calcium hydrogen carbonate, the concentration of the calcium salt solution is 20%-30%, and the reaction time is 0.5h-1h.

[0023] Preferably: in the step S5, the filtering pressure is 0.4MPa-0.6MPa, deionized water is used for washing until the fluoride ion concentration in the washing liquid is lower than 10mg / L, and a heat sealing dryer is used for drying, the drying temperature is 100-120 degrees Celsius, and the drying time is 2h-3h.

[0024] Preferably: in step S5, the fluoride ion concentration is detected by an ion selective electrode method.

[0025] Preferably, the ion selective electrode method for detecting the fluoride ion concentration in deionized water comprises the following steps:

[0026] S51: Calibrate ion selective electrode: Wipe the electrode surface with deionized water to avoid contamination; Soak the electrode and reference electrode with standard fluoride ion solution to ensure that the electrodes are in equilibrium; Adjust the potential of the potentiometer to zero; Add standard fluoride ion solutions of different concentrations to the water sample, record the potential readings, and make a calibration curve;

[0027] S52: Test the water sample by placing the water sample to be tested into a cuvette using a pipette; clean the ion-selective electrode to avoid contamination; insert the electrode into the cuvette so that the electrode contacts the water sample and record the potential reading.

[0028] The beneficial effects of the present invention are:

[0029] 1. The fluorine content in the copper-sulfur concentrate of the present invention can be significantly reduced to below 0.1%, and the quality of the copper-sulfur concentrate is significantly improved. The method has the advantages of simple operation, low cost, and significant effect, and can be widely used in the smelting process of copper-sulfur concentrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention provides a flow chart of a method for improving the quality of copper-sulfur concentrate products and reducing fluorine. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0032] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "set" should be understood in a broad sense, for example, they can be fixedly connected or set, or detachably connected or set, or integrally connected or set. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0033] Embodiment 1:

[0034] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0035] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0036] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0037] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0038] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0039] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0040] In the step S2, the collector is xanthate and carboxylic acid.

[0041] The xanthate is ethyl xanthate, and the carboxylic acid is oleic acid.

[0042] In the step S2, the foaming agent is saponin.

[0043] Embodiment 2:

[0044] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0045] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0046] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0047] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0048] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0049] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0050] In the step S2, the collector is fatty amine, black medicine and benzothiazolyl mercaptan.

[0051] The fatty amine is dodecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0052] In the step S2, the foaming agent is butanol, octanol, propanol and pentanol.

[0053] Embodiment 3:

[0054] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0055] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0056] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0057] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0058] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0059] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0060] In the S2 step, the flotation pulp concentration is 25%-30%, and the aeration volume is 0.2-0.3m 3 / min, the flotation stirring speed is 150-200r / min.

[0061] In the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

[0062] The xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0063] In the step S2, the foaming agent is any one or more combinations of saponins, pine oil, butanol, octanol, propanol and pentanol.

[0064] Embodiment 4:

[0065] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0066] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0067] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0068] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0069] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0070] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0071] In the S2 step, the flotation pulp concentration is 27.5%, and the aeration volume is 0.25m 3 / min, and the flotation stirring speed is 175r / min.

[0072] In the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

[0073] The xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0074] In the step S2, the foaming agent is any one or more combinations of saponins, pine oil, butanol, octanol, propanol and pentanol.

[0075] Embodiment 5:

[0076] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0077] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0078] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0079] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0080] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0081] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0082] In the S2 step, the flotation pulp concentration is 27.5%, and the aeration volume is 0.25m 3 / min, and the flotation stirring speed is 175r / min.

[0083] In the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

[0084] The xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0085] In step S2, the foaming agent is any one or more combinations of saponins, pine oil, butanol, octanol, propanol, and amyl alcohol.

[0086] In the step S3, the concentration of the sodium hydroxide solution is 12.5%, and the reaction time is 1.5 h.

[0087] Embodiment 6:

[0088] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0089] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0090] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0091] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0092] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0093] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0094] In the S2 step, the flotation pulp concentration is 27.5%, and the aeration volume is 0.25m 3 / min, and the flotation stirring speed is 175r / min.

[0095] In the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

[0096] The xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0097] In step S2, the foaming agent is any one or more combinations of saponins, pine oil, butanol, octanol, propanol, and amyl alcohol.

[0098] In the step S3, the concentration of the sodium hydroxide solution is 10%-15%, and the reaction time is 1-2h.

[0099] In the step S4, the calcium salt solution is a combination of calcium chloride, calcium nitrate, calcium sulfate, calcium hydrogen phosphate, and calcium hydrogen carbonate. The concentration of the calcium salt solution is 25%, and the reaction time is 0.75 h.

[0100] Embodiment 7:

[0101] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0102] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0103] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0104] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0105] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0106] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0107] In the S2 step, the flotation pulp concentration is 25%-30%, and the aeration volume is 0.2-0.3m 3 / min, the flotation stirring speed is 150-200r / min.

[0108] In the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

[0109] The xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0110] In step S2, the foaming agent is any one or more combinations of saponins, pine oil, butanol, octanol, propanol, and amyl alcohol.

[0111] In the step S3, the concentration of the sodium hydroxide solution is 10%-15%, and the reaction time is 1-2h.

[0112] In the step S4, the calcium salt solution is any one or more combinations of calcium chloride, calcium nitrate, calcium sulfate, calcium hydrogen phosphate, and calcium hydrogen carbonate. The concentration of the calcium salt solution is 20%-30%, and the reaction time is 0.5h-1h.

[0113] In the step S5, the filtering pressure is 0.5 MPa, and deionized water is used for washing until the fluoride ion concentration in the washing liquid is lower than 10 mg / L. A heat sealing dryer is used for drying, the drying temperature is 110 degrees Celsius, and the drying time is 2.5 hours.

[0114] Embodiment 8:

[0115] A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, comprising the following steps:

[0116] S1: Pretreatment, crushing and grinding of copper-sulfur concentrate;

[0117] S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal;

[0118] S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate;

[0119] S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water;

[0120] S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

[0121] In the S2 step, the flotation pulp concentration is 25%-30%, and the aeration volume is 0.2-0.3m 3 / min, the flotation stirring speed is 150-200r / min.

[0122] In the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

[0123] The xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

[0124] In step S2, the foaming agent is any one or more combinations of saponins, pine oil, butanol, octanol, propanol, and amyl alcohol.

[0125] In the step S3, the concentration of the sodium hydroxide solution is 10%-15%, and the reaction time is 1-2h.

[0126] In the step S4, the calcium salt solution is any one or more combinations of calcium chloride, calcium nitrate, calcium sulfate, calcium hydrogen phosphate, and calcium hydrogen carbonate. The concentration of the calcium salt solution is 20%-30%, and the reaction time is 0.5h-1h.

[0127] In the step S5, the filtering pressure is 0.4MPa-0.6MPa, and deionized water is used for washing until the fluoride ion concentration in the washing liquid is lower than 10mg / L. A heat sealing dryer is used for drying, the drying temperature is 100-120 degrees Celsius, and the drying time is 2h-3h.

[0128] In step S5, the fluoride ion concentration is detected by an ion selective electrode method.

[0129] The ion selective electrode method for detecting the fluoride ion concentration in deionized water comprises the following steps:

[0130] S51: Calibrate ion selective electrode: Wipe the electrode surface with deionized water to avoid contamination; Soak the electrode and reference electrode with standard fluoride ion solution to ensure that the electrodes are in equilibrium; Adjust the potential of the potentiometer to zero; Add standard fluoride ion solutions of different concentrations to the water sample, record the potential readings, and make a calibration curve;

[0131] S52: Test the water sample by placing the water sample to be tested into a cuvette using a pipette; clean the ion-selective electrode to avoid contamination; insert the electrode into the cuvette so that the electrode contacts the water sample and record the potential reading.

[0132] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for improving the quality of copper-sulfur concentrate products and reducing fluorine, characterized in that: The following steps are involved: S1: Pretreatment, crushing and grinding of copper-sulfur concentrate; S2: flotation and impurity removal, adding the pretreated copper-sulfur concentrate into the flotation machine, adding collector and frother to carry out flotation and impurity removal; S3: Neutralization reaction to reduce fluorine, adding the flotation concentrate to the neutralization reaction tank, adding sodium hydroxide solution to carry out neutralization reaction, so that the fluoride in the copper-sulfur concentrate reacts with sodium hydroxide to generate sodium fluoride that is easily soluble in water, thereby reducing the fluorine content in the copper-sulfur concentrate; S4: precipitation reaction to reduce fluorine. After the neutralization reaction is completed, a calcium salt solution is added to the reaction tank for precipitation reaction, so that sodium fluoride reacts with calcium ions to generate calcium fluoride precipitate which is insoluble in water; S5: filtering, washing and drying, filtering, washing and drying the precipitate to obtain a copper-sulfur concentrate product with a low fluorine content.

2. The method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 1, characterized in that: In the S2 step, the flotation pulp concentration is 25%-30%, and the aeration volume is 0.2-0.3m 3 / min, the flotation stirring speed is 150-200r / min.

3. The method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 1, characterized in that: In the step S2, the collector is any one or more combinations of xanthate, carboxylic acid, fatty amine, black medicine, and benzothiazolyl mercaptan.

4. A method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 3, characterized in that: The xanthate is ethyl xanthate or butyl xanthate, the carboxylic acid is oleic acid or fatty acid, the fatty amine is dodecylamine or hexadecylamine, and the black medicine is sodium diethyldithiocarbamate.

5. The method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 1, characterized in that: In the step S2, the foaming agent is any one or more combinations of saponins, pine oil, butanol, octanol, propanol and pentanol.

6. The method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 1, characterized in that: In the step S3, the concentration of the sodium hydroxide solution is 10%-15%, and the reaction time is 1-2h.

7. The method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 1, characterized in that: In the step S4, the calcium salt solution is any one or more combinations of calcium chloride, calcium nitrate, calcium sulfate, calcium hydrogen phosphate, and calcium hydrogen carbonate. The concentration of the calcium salt solution is 20%-30%, and the reaction time is 0.5h-1h.

8. The method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 1, characterized in that: In the step S5, the filtering pressure is 0.4MPa-0.6MPa, and deionized water is used for washing until the fluoride ion concentration in the washing liquid is lower than 10mg / L. A heat sealing dryer is used for drying, the drying temperature is 100-120 degrees Celsius, and the drying time is 2h-3h.

9. A method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 8, characterized in that: In step S5, the fluoride ion concentration is detected by an ion selective electrode method.

10. A method for improving the quality of copper-sulfur concentrate products and reducing fluorine according to claim 9, characterized in that: The ion selective electrode method for detecting the fluoride ion concentration in deionized water comprises the following steps: S51: Calibrate ion selective electrode: Wipe the electrode surface with deionized water to avoid contamination; Soak the electrode and reference electrode with standard fluoride ion solution to ensure that the electrode is in a balanced state; Adjust the potential of the potentiometer to zero; add standard fluoride ion solutions of different concentrations to the water sample, record the potential readings, and prepare a calibration curve; S52: Test the water sample by placing the water sample to be tested into a cuvette using a pipette; clean the ion-selective electrode to avoid contamination; insert the electrode into the cuvette so that the electrode contacts the water sample and record the potential reading.

Citation Information

Patent Citations

  • Flotation method for low-grade copper sulphide ore difficult to treat

    CN112156895A

  • Flotation process for reducing fluorine content in copper sulfide concentrate

    CN114798186A

  • Comprehensive recovery method of low-grade sulphide ore type fluorite mine

    CN116618183A

  • Flotation method of copper sulfide ore

    CN117943212A