Metal surface treatment process and application thereof
By combining normal pressure plasma and low pressure plasma treatment and interface activation process, the problems of high cost of metal surface treatment and insufficient adhesion in the prior art are solved, and efficient and environmentally friendly metal surface treatment is achieved, which significantly improves the coating and metal The adhesion force of the product reduces the contact angle and avoids film decomposition.
Patent Information
- Application Number
- CN202411003762.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The existing metal surface treatment process is high, the environment is unfriendly, the process is complicated and the adhesion between the metal surface and the coating cannot be improved for a long time, especially during the adhesion of the topcoat, such as film removal, etc.
Using a process that combines normal pressure plasma treatment and low pressure plasma treatment, the aqueous interface treatment formula is used for interface activation, remove grease and dirt on the metal surface, establish free radicals such as hydroxyl and carboxyl groups, improve surface energy, and form intermediate layers to enhance Adhesion of the coating to the metal and saves resources through the recycling filtration system of the cleaning section.
It significantly improves the adhesion of the metal surface, reduces the surface contact angle, avoids film defiling, and has a long-lasting treatment effect. It is suitable for a variety of coating processes, is environmentally friendly, does not contain organic polymers, and is suitable for plastic surface treatment.
Smart Images

Figure CN118904692A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal material surface treatment, and in particular to a metal surface treatment process and application thereof. Background Art
[0002] During the process of coating the metal surface, the adhesion between the metal and the coating will be seriously affected due to the great differences in the metal surface roughness, microstructure, surface oxide layer and chemical properties of the coating. In addition, due to the changes in the metal surface properties under environmental exposure, the contact angle of the metal surface becomes larger, which will also affect the adhesion between the metal and the coating.
[0003] At present, polyurethane primer, alkyd primer, epoxy resin primer, acrylic resin primer and other primers are generally used to improve the adhesion of topcoat, but due to the high cost, long baking time, complex baking process and high VOC content of the above primers, they not only consume a lot of resources but are also not environmentally friendly. Therefore, there is an urgent need for a process that is low in cost, environmentally friendly, simple in process, highly adaptable and can permanently improve the adhesion between metal surface and coating. Summary of the invention
[0004] In view of the defects in the prior art, the present invention proposes a metal surface treatment process and application thereof.
[0005] The present invention provides a metal surface treatment process, comprising the following steps:
[0006] Cleaning section: spraying, roller brushing, vacuum roller drying, baking, and winding;
[0007] Interface processing section:
[0008] a) plasma treatment;
[0009] b) Interface activation: unwinding, spraying, roller coating, baking, and winding;
[0010] The plasma treatment includes normal pressure plasma treatment and low pressure plasma treatment; the water-based interface treatment formula used in the spraying process includes the following components:
[0011] Water 0-50 parts by weight, such as 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50 parts; solvent 0-50 parts by weight, such as 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50 parts; interface treatment agent 0.5-5 parts by weight, such as 0.1, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 parts; auxiliary agent 0.5-3 parts by weight, such as 0.5, 1, 1.5, 2, 2.5, 3 parts.
[0012] In order to maintain the surface quality of metal coils in the cleaning section, the spraying and roller brushing time must be controlled within 1.5-5 minutes. If the time is too short, oil stains, impurities, etc. will remain on the metal surface. If the time is too long, the working hours and cleaning agents will be increased, thereby increasing costs. After cleaning, the metal surface needs to be tested for dyne value to ensure that the dyne value is greater than 30.
[0013] The atmospheric pressure plasma treatment system consists of a plasma generator, a gas delivery pipeline and a plasma spray gun. The plasma generator generates high-voltage and high-frequency energy, and generates low-temperature plasma in the glow discharge that is activated and controlled in the nozzle steel pipe. The plasma is sprayed onto the surface of the workpiece with the help of compressed air. When the plasma meets the surface of the treated object, chemical reactions and physical changes occur, the surface is cleaned, hydrocarbon dirt such as grease, auxiliary additives, etc. are removed, and free radicals such as hydroxyl and carboxyl are established. These radicals promote the adhesion of various coating materials and are optimized during bonding and paint applications. The low-pressure plasma cleaning system consists of a vacuum chamber and a high-frequency plasma power supply, a vacuum pump, an air filling system, an automatic control system, etc. The vacuum pump is used to evacuate the studio to a vacuum degree of 30-50Pa, and then the gas is ionized under the action of the alternating electric field of the high-frequency generator to form plasma (the fourth state of matter). Its notable characteristics are high uniformity glow discharge, and the emission of colored visible light from blue to dark purple according to different gases, and the material processing temperature is close to room temperature. During the low-pressure plasma treatment process, the active plasma performs a dual role of physical bombardment and chemical reaction on the object to be cleaned, so that the surface material of the object to be cleaned becomes particles and gaseous materials, which are discharged through vacuuming, thereby achieving the purpose of cleaning. The surface energy of the metal can be significantly improved by plasma treatment, and the surface contact angle can be reduced, which can improve the adhesion effect of primers and topcoats, etc., and avoid abnormal phenomena such as film stripping. At the same time, the metal surface will be modified, such as hydrophilicity, low friction, high cleaning, activation, etching, etc. For example, surface etching is the formation of plasma by gas exposed to the electron area, and the ionized gas and the gas composed of released high-energy electrons are generated, thereby forming plasma or ions. When the ionized gas atoms are accelerated by the electric field, they will release enough power to etch the surface. The present invention adopts the method of coordinated treatment of normal pressure plasma treatment and low pressure plasma treatment, which can significantly improve the surface energy of the metal compared with single plasma treatment, and significantly improve the effective time of the surface energy.
[0014] During the interface activation stage, a special interface treatment formula is used to form an intermediate layer between the metal and the coating. The intermediate layer can significantly improve the interface energy of the metal. The coating and the metal are bonded together through the combined forces of chemical bonding, diffusion force, van der Waals force, hydrogen bonding, etc., thereby improving the adhesion between the organic coating and the metal surface. In addition, the interface activation section has simple configuration, low baking temperature (low energy consumption), does not contain polymer compounds, and is low in VOC (environmentally friendly). After activation, the metal surface energy can be maintained at a high level for a long time, is irreversible, has strong coating adaptability, and significantly improves adhesion. Compared with the use of plasma treatment alone, it also has the effect of permanently improving the interface energy of the metal surface. The interface activation process of the present invention is not only suitable for metal but also for surface treatment of plastics, and is also suitable for different coating processes, such as roller coating, spraying, etc.
[0015] The cleaning process of the present invention can remove grease, dirt, rust, paint, etc. attached to the surface of metal materials, which is convenient for later interface treatment; plasma treatment can significantly increase the surface energy of the metal, reduce the surface contact angle, and avoid the problem of incomplete cleaning in the cleaning process; the interface activation stage can significantly reduce the contact angle of the metal surface, and enhance and improve the adhesion between the coating film and the substrate. Through the mutual cooperation between the various process sections, the metal surface energy can be permanently improved to ensure that there will be no abnormal phenomena such as film peeling after the coating is applied.
[0016] The special surface treatment process of the present invention is not affected by the metal manufacturing process and the metal storage environment. The treated metal surface has a low contact angle and high surface energy, which can significantly improve the adhesion of the coating on the metal surface. The treatment effect is irreversible and will not reduce the surface energy over time. In addition, compared with other primers and connecting paints, the method of improving the adhesion between the metal surface and the coating of the present invention does not contain organic polymers such as resins, which is friendly to the environment and the human body.
[0017] Furthermore, the cleaning agent used in the cleaning section is any one of an aqueous acid cleaning agent, an aqueous alkaline cleaning agent or a solvent-based cleaning agent. The cleaning section also includes a filtration system for recovering and filtering the cleaning agent, so that the cleaning agent can be reused to save resources.
[0018] Aqueous acid cleaning agents include one or more acidic cleaning agents such as hydrochloric acid, sulfuric acid, citric acid, formic acid, and hydrofluoric acid, and a small amount of surfactants, chelating agents, corrosion inhibitors, etc. are added; aqueous alkaline cleaning agents include one or more alkaline cleaning agents such as caustic soda, soda ash, sodium phosphate, sodium sulfite, etc., and a small amount of surfactants, chelating agents, corrosion inhibitors, etc. are added; solvent-based cleaning agents include one or more hydrocarbon cleaning agents such as chlorinated hydrocarbons, brominated hydrocarbons, fluorinated hydrocarbons, etc., and a small amount of surfactants, chelating agents, corrosion inhibitors, etc. are added.
[0019] The cleaning process can make targeted choices of cleaning agents based on the characteristics of the metal. For example, the acid pickling method is suitable for acid-resistant materials such as stainless steel, and the alkaline cleaning method is suitable for materials such as steel. The cleanliness of the metal surface can be improved by combining chemical and physical methods, which can improve the subsequent plasma treatment effect.
[0020] Furthermore, the solvent is an alcohol organic solvent, including but not limited to one or more of methanol, ethanol, propylene glycol, butanediol, polyols, etc.
[0021] Furthermore, the interface treatment agent is one or more of a silane coupling agent, isopropyl tri(dioctyl pyrophosphate) titanate, diisopropoxy diacetylacetonate titanate, isopropyl tristearate titanate, an aluminate coupling agent, a lignin coupling agent or a bimetallic coupling agent, wherein the silane coupling agent includes but is not limited to any one or more of vinyl silane, aminosilane, and epoxy silane, and the bimetallic coupling agent includes but is not limited to any one or more of an aluminum-titanium composite coupling agent and an aluminum-zirconate coupling agent.
[0022] Furthermore, the interface treatment agent is a combination of diisopropoxy diacetylacetonate titanate and a bimetallic coupling agent.
[0023] Furthermore, the gas used for the atmospheric pressure plasma treatment is any one of argon, helium, oxygen or nitrogen.
[0024] Furthermore, the auxiliary agent is one or more of a dispersant, a wetting agent, a defoaming agent, a leveling agent, and a corrosion inhibitor.
[0025] The present invention also provides a metal treated by the metal surface treatment process, wherein the metal surface energy is higher than 70 mN / m.
[0026] The present invention also provides the use of the metal in preparing copper-clad plates and automobiles, especially in preparing automobile products that need to be sprayed.
[0027] In summary, compared with the prior art, the present invention achieves the following technical effects:
[0028] (1) The surface-treated metal provided by the present invention has a high surface energy for a long time;
[0029] (2) The surface-treated metal provided by the present invention has a low surface contact angle;
[0030] (3) The surface-treated metal provided by the present invention has high adhesion to the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 This is a diagram showing the effect of metal after low-pressure plasma treatment in Example 4 of the present invention;
[0033] Figure 2 Schematic diagram of the interface activation process of the metal interface treatment section in Examples 1-4 of the present invention;
[0034] Figure 3 This is a schematic diagram of the metal atmospheric pressure plasma treatment process in Examples 1-4 of the present invention;
[0035] Figure 4 Effect diagram of the metal after normal pressure plasma treatment in Examples 1-4 of the present invention. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0037] Example
[0038] The present invention is further described below in conjunction with specific examples and comparative examples. The following specific examples are all preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the following examples, and are particularly not limited to the types of the various component raw materials used in the following specific examples.
[0039] 1. The sources of raw materials for the embodiments and comparative examples are as follows:
[0040] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present invention are commercially available.
[0041] Among them, the present application uses aluminum as the metal substrate and soda ash as the cleaning agent;
[0042] The gas used in the atmospheric pressure plasma treatment process is nitrogen;
[0043] The additives in the aqueous interface treatment formula include 0.3 parts by weight of a defoaming agent GPE type polyoxyethylene (polyoxypropylene) ether, 0.3 parts by weight of a leveling agent polydimethylsiloxane, 0.3 parts by weight of a dispersant polyacrylate, 0.3 parts by weight of a wetting agent polyether modified silicone oil, and 0.3 parts by weight of a corrosion inhibitor sulfonated lignin.
[0044] 2. Various performance test methods
[0045] (1) Metal surface energy test: The surface energy is measured using the dyne pen test method, and the dyne value is the surface energy.
[0046] (2) Metal surface contact angle test: The contact angle is measured using a contact angle meter using the sessile drop method.
[0047] (3) Metal surface and coating adhesion test: Test according to ISO2409-1992 standard.
[0048] Example 1
[0049] The metal surface treatment process of Example 1 comprises the following steps:
[0050] Cleaning section: spraying, roller brushing, vacuum roller drying, baking, and winding;
[0051] Interface processing section:
[0052] a) Plasma treatment: atmospheric pressure plasma treatment + low pressure plasma treatment;
[0053] b) Interface activation: unwinding, spraying, roller coating, baking, and winding;
[0054] The aqueous interface treatment formula in the spraying process includes the following components:
[0055] 5 parts by weight of water, 40 parts by weight of butanediol, 4 parts by weight of vinyl silane, and 1.5 parts by weight of auxiliary agent.
[0056] Example 2
[0057] The metal surface treatment process of Example 2 comprises the following steps:
[0058] Cleaning section: spraying, roller brushing, vacuum roller drying, baking, and winding;
[0059] Interface processing section:
[0060] a) Plasma treatment: atmospheric pressure plasma treatment + low pressure plasma treatment;
[0061] b) Interface activation: unwinding, spraying, roller coating, baking, and winding;
[0062] The aqueous interface treatment formula in the spraying process includes the following components:
[0063] 40 parts by weight of water, 5 parts by weight of butanediol, 1 part by weight of vinyl silane, and 1.5 parts by weight of auxiliary agent.
[0064] Example 3
[0065] The metal surface treatment process of Example 3 comprises the following steps:
[0066] Cleaning section: spraying, roller brushing, vacuum roller drying, baking, and winding;
[0067] Interface processing section:
[0068] a) Plasma treatment: atmospheric pressure plasma treatment + low pressure plasma treatment;
[0069] b) Interface activation: unwinding, spraying, roller coating, baking, and winding;
[0070] The aqueous interface treatment formula in the spraying process includes the following components:
[0071] 30 parts by weight of water, 30 parts by weight of methanol, 2 parts by weight of diisopropoxy diacetylacetonate titanate, and 1.5 parts by weight of auxiliary agent.
[0072] Example 4
[0073] The metal surface treatment process of Example 4 comprises the following steps:
[0074] Cleaning section: spraying, roller brushing, vacuum roller drying, baking, and winding;
[0075] Interface processing section:
[0076] a) Plasma treatment: atmospheric pressure plasma treatment + low pressure plasma treatment;
[0077] b) Interface activation: unwinding, spraying, roller coating, baking, and winding;
[0078] The aqueous interface treatment formula in the spraying process includes the following components:
[0079] 30 parts by weight of water, 30 parts by weight of methanol, 1 part by weight of diisopropoxy diacetylacetonate titanate, 1 part by weight of bimetallic coupling agent aluminum-titanium composite coupling agent, and 1.5 parts by weight of auxiliary agent.
[0080] Comparative Example 1
[0081] Compared with Example 4, the metal surface treatment process of Comparative Example 1 does not include a cleaning section.
[0082] Comparative Example 2
[0083] Compared with Example 4, the metal surface treatment process of Comparative Example 2 includes only atmospheric pressure plasma treatment in the plasma treatment process.
[0084] Comparative Example 3
[0085] Compared with Example 4, the metal surface treatment process of Comparative Example 3 does not include an interface activation step.
[0086] Comparative Example 4
[0087] Compared with Example 4, the metal surface treatment process of Comparative Example 4 does not include a plasma treatment step.
[0088] Table 1 Effects of Examples and Comparative Examples
[0089]
[0090]
[0091] The metal surface treatment process of Examples 1-4 includes a clearing section and an interface treatment section, and includes a normal pressure plasma treatment process, a low pressure plasma treatment process and an interface activation process. The treated metals have high surface energy, low surface contact angle and high adhesion with the coating. The surface energy of the metals after treatment in Examples 1-4 is all above 70mN / m, the surface contact angle is all below 10°, and the peeling level between the metals and the coating is also level 1 or below. Obviously, the metal surface treatment process of the present invention can replace the polymer compound primer to improve the adhesion between the metal surface and the coating, and at the same time has environmental protection performance.
[0092] Comparative Examples 1-4 are all compared with Example 4. The surface treatment process of Comparative Example 1 does not include a cleaning process, so that foreign matter such as oil, impurities, etc. remain on the metal surface, affecting the effect of subsequent plasma treatment and interface activation; the plasma treatment of Comparative Example 2 only includes normal pressure plasma treatment, so that hydrocarbon dirt, such as grease, auxiliary additives, etc., remain on the metal surface, affecting the effect of subsequent low-pressure plasma treatment and interface activation; the surface treatment process of Comparative Example 3 does not include an interface activation process, so that the metal surface energy will gradually decrease with the extension of time, affecting the subsequent adhesion; Comparative Example 4 does not include a plasma treatment process, resulting in a reduction in active groups such as hydroxyl groups on the metal surface, affecting the effect of subsequent surfactants. None of the above comparative examples can make the metal after surface treatment have high surface energy, low contact angle, and high adhesion with the coating, and cannot maintain high surface energy for a long time.
[0093] Based on the test data of metal surface energy, metal surface contact angle and adhesion between metal and coating in Table 1 and Table 2, the polyamide / polyolefin composite materials prepared by Examples 1-4 have obvious advantages over the comparative examples and can effectively meet the high standards of customers and the market.
[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A metal surface treatment process, characterized in that: The steps include: Cleaning section: spraying, roller brushing, vacuum roller drying, baking, and winding; Interface processing section: a) plasma treatment; b) Interface activation: unwinding, spraying, roller coating, baking, and winding; Wherein, the plasma treatment includes normal pressure plasma treatment and low pressure plasma treatment; The water-based interface treatment formula used in the spraying process includes the following components: Water 0-50 parts by weight, solvent 0-50 parts by weight, interface treatment agent 0.5-5 parts by weight, auxiliary agent 0.5-3 parts by weight.
2. The metal surface treatment process according to claim 1, characterized in that: The cleaning agent used in the cleaning section is any one of an aqueous acid cleaning agent, an aqueous alkaline cleaning agent or a solvent cleaning agent.
3. The metal surface treatment process according to claim 1, characterized in that: The solvent is an alcohol organic solvent.
4. The metal surface treatment process according to claim 1, characterized in that: The interface treatment agent is any one or more of a silane coupling agent, isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, diisopropoxy diacetylacetonate titanate, isopropyl tristearate titanate, an aluminate coupling agent, a lignin coupling agent or a bimetallic coupling agent.
5. The metal surface treatment process according to claim 4, characterized in that: The interface treatment agent is a combination of diisopropoxy diacetylacetonate titanate and a bimetallic coupling agent.
6. The metal surface treatment process according to claim 1, characterized in that: The gas for the atmospheric pressure plasma treatment is any one of argon, helium, oxygen or nitrogen.
7. The metal surface treatment process according to claim 1, characterized in that: The auxiliary agent is one or more of a dispersant, a wetting agent, a defoamer, a leveling agent, and a corrosion inhibitor.
8. The metal treated by the metal surface treatment process according to any one of claims 1 to 7, characterized in that: The metal surface energy is higher than 70 mN / m.
9. Use of the metal according to claim 8 in the preparation of copper clad laminates and automobiles.
Citation Information
Cited By
Surface treatment process and system for GIS (gas insulated switchgear) tubular insulation structural member
CN121131351A