Recycled polyester chip, superfine denier fiber and preparation method of superfine denier fiber

By cutting and high-temperature compacting waste polyester filaments and PET bottle flakes, the intrinsic viscosity fluctuation of recycled polyester chips is controlled, solving the fiber quality problem caused by intrinsic viscosity fluctuations during the recycling process of waste filaments and PET bottle flakes, and improving the production stability and performance of ultrafine denier fibers.

CN118906287APending Publication Date: 2024-11-08JIANGSU HENGKE ADVANCED MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411285485.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the recycling process of waste filaments and PET bottle flakes, fluctuations in intrinsic viscosity lead to poor mechanical properties and processing stability of the recycled fibers. In particular, in the production of ultrafine denier fibers, uneven melting of chips causes problems such as spinning breakage, uneven linear density, hard ends, and uneven dyeing.

Method used

Recycled polyester chips are prepared by cutting and high-temperature compacting polyester waste filament granules and PET bottle flakes, followed by mixing and compacting, controlling the bulk density deviation of the mixture, ensuring the uniformity of the material before entering the screw extruder, and using specific parameters such as the temperature of the rotating mixing container, the vacuum degree, and the temperature of the screw extruder.

Benefits of technology

This method achieves a small intrinsic viscosity fluctuation range and high molecular weight in recycled polyester chips, reduces material degradation, ensures excellent fiber performance, solves the melt inhomogeneity problem in the production of ultrafine denier fibers, and improves spinning stability and fiber quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043617680000111
    Figure BDA0005043617680000111
Patent Text Reader

Abstract

The invention relates to a regenerated polyester chip, a superfine denier fiber and a preparation method thereof.The preparation method of the regenerated polyester chip comprises the steps that firstly, waste polyester yarn particles and PET bottle chips are subjected to cutting and high-temperature compaction, then the compacted waste polyester yarn particles and the compacted bottle chips are subjected to cutting and high-temperature mixed compaction again, and the regenerated polyester chip is obtained; the deviation range of the stacking density of the finally-compacted mixed material is reduced, and the finally-compacted mixed material can still keep a good mixing effect after entering the first screw extruder, so that the stable screw filling degree is ensured, the intrinsic viscosity fluctuation range of the obtained regenerated polyester chip is smaller, the b value is smaller, and the quality of the regenerated polyester chip is improved. Therefore, the production requirements of subsequent superfine denier fibers are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of regenerated polyester fibers, and in particular to a regenerated polyester chip, an ultrafine denier fiber and a preparation method thereof. Background Art

[0002] As the main renewable raw materials for polyester fiber, the recycling of waste silk and PET bottle flakes is particularly important. Waste silk mainly comes from unqualified products and scraps in the textile production process, while PET bottle flakes mainly come from discarded polyester beverage bottles. Through reasonable recycling processes, these wastes can not only effectively reduce environmental pollution, but also realize the recycling of resources, which has significant economic and environmental significance.

[0003] However, there are some technical difficulties in the recycling process of waste silk and PET bottle flakes. In the recycling process of waste silk, since the waste silk has been processed and treated many times, its molecular chain is damaged to a certain extent, resulting in a low intrinsic viscosity of the recycled chips. In the recycling process of PET bottle flakes, since the PET bottle flakes are affected by environmental factors such as ultraviolet rays and oxygen during use, their molecular chains may undergo cross-linking or oxidation reactions, resulting in a high intrinsic viscosity of the recycled chips. The intrinsic viscosity is an important indicator to measure the molecular weight of the polymer. A low intrinsic viscosity means a decrease in molecular weight, which will directly affect the mechanical properties and processing stability of the regenerated fiber, thereby reducing the fiber quality. A high intrinsic viscosity will not only increase the flow resistance of the melt, making the processing process more difficult, but may also affect the uniformity and dyeing properties of the regenerated fiber.

[0004] Especially in the process of ultra-fine fiber production and processing, the fluctuation range of the intrinsic viscosity of the regenerated chips seriously affects the quality of ultra-fine fibers. The larger the fluctuation range of the intrinsic viscosity, the more uneven the melt obtained after the chips are melted, which in turn leads to problems such as spinning breakage, uneven linear density, hard-head yarn, difficulty in post-stretching and uneven dyeing in the subsequent spinning process. Therefore, how to develop a process method that can effectively control the intrinsic viscosity of the regenerated chips based on the different characteristics of polyester waste yarn and PET bottle chips has become a technical problem that needs to be solved urgently in the current polyester fiber regeneration field. Summary of the invention

[0005] In order to solve the above technical problems, the present application provides a regenerated polyester chip, ultrafine denier fiber and a preparation method thereof.

[0006] To achieve the above objectives, this application is implemented through the following technical solutions:

[0007] The present application provides a method for preparing recycled polyester chips, comprising the following steps:

[0008] S1. Placing the polyester waste silk particles in a first rotating mixing container with a first rotating three-dimensional knife disc for cutting and mixing, so as to compact the polyester waste silk particles to obtain compacted polyester waste silk particles, wherein the moisture content of the compacted polyester waste silk particles is less than 3%. Preferably, the compacted polyester waste silk particles have a bulk density of 60 kg / m 3 ~100kg / m 3 , the particle size of the compacted polyester waste silk particles is 2 mm to 4 mm;

[0009] S2, placing the PET bottle flakes in a second rotating mixing container with a second rotating three-dimensional blade disc for cutting and mixing, so as to compact the bottle flakes to obtain compacted bottle flakes, wherein the moisture content of the compacted bottle flakes is less than 2%, and preferably, the bulk density of the compacted bottle flakes is 220kg / m 3 ~280kg / m 3 , the particle size of the compacted bottle flakes is 3mm to 9mm;

[0010] S3, by mass percentage, placing 10% to 30% of the compacted polyester waste silk particles obtained in step S1 and 70% to 90% of the compacted bottle flakes obtained in step S2 in a third rotating mixing container with a third rotating three-dimensional knife disc for cutting and mixing, so as to achieve mixing and compacting of the compacted polyester waste silk particles and the compacted bottle flakes to obtain a compacted mixed material, wherein the moisture content of the compacted mixed material is less than 0.3%, and preferably, the bulk density of the compacted mixed material is 250 kg / m 3 ~290kg / m 3 , the particle size of the compacted mixed material is 1 mm to 3.5 mm;

[0011] S4, extruding the compacted mixed material through a first screw extruder, a first filter, a second filter, and a die extrusion device in sequence, cooling, and pelletizing to obtain recycled polyester chips.

[0012] Based on the above scheme, the polyester waste silk particles and PET bottle flakes are first cut and compacted at high temperature, and then the compacted polyester waste silk particles and compacted bottle flakes are cut and compacted at high temperature, which reduces the deviation range of the bulk density of the mixed material. When the compacted mixed material is transported to the first screw extruder, the deviation range of the bulk density of the compacted mixed material is smaller, and the mixed material is more uniform. When the screw speed of the first screw extruder is increased, a good mixing effect can still be maintained, thereby ensuring that the material has a stable filling degree in the screw extruder and that the characteristic viscosity of the obtained recycled polyester chips has a small fluctuation range. At the same time, the residence time of the compacted mixed material in the first screw extruder is shortened, reducing the material degradation caused by high temperature, and the produced recycled polyester chips have a higher molecular weight, a smaller b value, and a smaller yellowness, ensuring better performance of the later spun fibers.

[0013] As a further improvement of the present application, in step S1, the particle size of the polyester waste silk particles is 3 mm to 6 mm, the moisture content of the polyester waste silk particles is less than 10%, and the bulk density of the polyester waste silk particles is 80 kg / m 3 ~130kg / m 3 The rotation speed of the first rotating three-dimensional blade is 400 rpm / min to 500 rpm / min, and the temperature in the first rotating mixing container is 150° C. to 160° C.

[0014] As a further improvement of the present application, in step S1, the first rotating mixing container is evacuated to make the pressure in the first rotating mixing container be 5 mbar to 8 mbar.

[0015] As a further improvement of the present application, in step S2, the particle size of the PET bottle flakes is 4 mm to 12 mm, the moisture content of the PET bottle flakes is less than 5%, and the bulk density of the PET bottle flakes is 250 kg / m 3 ~350kg / m 3 The rotation speed of the second rotating three-dimensional blade disc is 90 rpm / min to 110 rpm / min, and the temperature in the second rotating mixing container is 170°C to 180°C.

[0016] As a further improvement of the present application, in step S2, the second rotating mixing container is evacuated to make the pressure in the second rotating mixing container be 5 mbar to 8 mbar.

[0017] As a further improvement of the present application, in step S3, the rotation speed of the third rotating three-dimensional blade disc is 35 rpm / min to 55 rpm / min, and the temperature in the third rotating mixing container is 190° C. to 210° C.

[0018] As a further improvement of the present application, in step S3, the third rotating mixing container is evacuated to make the pressure in the third rotating mixing container be 1 mbar to 3 mbar.

[0019] As a further improvement of the present application, in step S4, the first screw extruder includes a material entry zone and a screw extrusion zone, the temperature of the material entry zone is 195°C~205°C, the temperature of the screw extrusion zone is 275°C~285°C, the compacted mixture entering the first screw extruder is in a vacuum atmosphere of 0.1mbar~0.5mbar throughout the process, the filtration accuracy of the filter mesh of the first filter is 30μm~40μm, and the temperature of the first filter is 270°C~290°C; the filtration accuracy of the filter mesh of the second filter is 10μm~15μm, and the temperature of the second filter is 270°C~290°C.

[0020] To achieve the above objectives, the present application also provides a recycled polyester chip, which is prepared by the above-mentioned method for preparing the recycled polyester chip.

[0021] To achieve the above object, the present application also provides an ultra-fine denier fiber, which is prepared from the above-mentioned recycled polyester chips. Specifically, the recycled polyester chips are sequentially subjected to pre-crystallization, drying, a second screw extruder, a melt filter, a spinning manifold, a metering pump, a spinning assembly, side-blowing cooling and oiling, drawing, and winding processes to form the ultra-fine denier fiber.

[0022] As a further improvement of the present application, the polyester waste silk particles are prepared by subjecting the polyester waste silk to conventional crushing process, friction process, degreasing process and drying process. Among them: the degreasing rate of the conventional degreasing process can reach more than 90%. The drying process generally includes a first drying process, a second drying process and a third drying process, wherein: the first drying process and the second drying process both use a friction dryer, and the third drying process uses a fluidized bed, and the temperature of the fluidized bed is 100°C to 130°C. The moisture removal rate of the two friction dryers can reach 40% to 60%. After drying in the fluidized bed, the moisture content of the polyester waste silk particles is controlled within 10%.

[0023] The beneficial effect of the present application is that the present application provides a method of first cutting the polyester waste silk particles and the PET bottle flakes and compacting them at high temperature, and then cutting the compacted polyester waste silk particles and the compacted bottle flakes again and mixing and compacting them at high temperature, thereby reducing the deviation range of the bulk density of the final compacted mixture, and ensuring that the final compacted mixture can still maintain a good mixing effect after entering the first screw extruder, thereby ensuring a stable screw filling degree, so that the obtained recycled polyester chips have excellent characteristic viscosity and b value.

[0024] In addition, factors such as the temperature of the rotating mixing container, the vacuum degree, the temperature of the screw extruder, the moisture content of each material, etc. are all very important factors affecting the characteristic viscosity and b value of the final recycled polyester chips. Therefore, the present application sets specific parameters such as the temperature of the rotating mixing container, the vacuum degree, the temperature of the screw extruder, the moisture content of each material, etc., so that the final generated recycled polyester chips have excellent characteristic viscosity and b value. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0026] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below in conjunction with specific implementation methods.

[0027] In actual production, the screw extrusion process is a necessary process for processing slices for ultrafine denier fibers. During the processing, the inventors found that the uniformity of the material before entering the screw determines the speed of the screw, and the screw speed is positively correlated with the output of the equipment. The traditional screw extrusion process does not take into account the uniformity of the material before entering the screw. Therefore, the traditional screw extrusion process generally adopts a low screw speed for production, which leads to a corresponding increase in the plasticization time of the material, and the temperature of the material delivered to the front end of the screw is higher. The material stays in the screw for a longer time, which affects the output and also causes the degradation of the material caused by high temperature to intensify. The molecular weight of the slices produced is reduced, and the b value is too large, so that the physical properties of the fibers spun later deteriorate. In addition, if the uniformity of the material before entering the screw is poor, even if the screw speed is lowered, it is difficult to produce slices with a small characteristic viscosity fluctuation range suitable for ultrafine denier fibers. In order to solve the above technical problems, the present application designs the following embodiments:

[0028] Example 1

[0029] This embodiment provides a method for preparing a regenerated polyester chip for ultrafine denier fiber, comprising the following steps:

[0030] S1. Place the polyester waste silk particles in a first rotating mixing container with a first rotating three-dimensional blade, evacuate the first rotating mixing container, make the pressure in the first rotating mixing container 5mbar, cut and mix to compact the polyester waste silk particles, and obtain compacted polyester waste silk particles. Wherein: the particle size of the polyester waste silk particles is 3mm to 6mm, the moisture content of the polyester waste silk particles is less than 10%, and the bulk density of the polyester waste silk particles is 80kg / m3 ~130kg / m 3 The rotation speed of the first rotating three-dimensional blade is 500 rpm / min, and the temperature in the first rotating mixing container is 150°C. The bulk density of the compacted polyester waste silk particles is 60 kg / m 3 ~80kg / m 3 The moisture content of the compacted polyester waste silk particles is less than 3%, and the particle size of the compacted polyester waste silk particles is 2 mm to 3 mm.

[0031] S2, placing the PET bottle flakes in a second rotating mixing container with a second rotating three-dimensional blade, evacuating the second rotating mixing container to make the pressure in the second rotating mixing container 5mbar, cutting and mixing to achieve compaction of the PET bottle flakes to obtain compacted bottle flakes. Wherein: the particle size of the PET bottle flakes is 4mm to 12mm, the moisture content of the PET bottle flakes is less than 5%, and the bulk density of the PET bottle flakes is 250kg / m 3 ~350kg / m 3 The speed of the second rotating three-dimensional blade is 110 rpm / min, and the temperature in the second rotating mixing container is 170°C. The bulk density of the compacted bottle flakes is 220 kg / m 3 ~250kg / m 3 The moisture content of the compacted bottle flakes is less than 2%, and the particle size of the compacted bottle flakes is 3 mm to 7 mm.

[0032] S3. 10% of the polyester waste silk particles compacted in step S1 and 90% of the bottle flakes compacted in step S2 are placed in a third rotating mixing container with a third rotating three-dimensional blade disc, and the third rotating mixing container is evacuated to a pressure of 1 mbar, and the compacted polyester waste silk particles and the compacted bottle flakes are cut and mixed to obtain a compacted mixed material. The rotation speed of the third rotating three-dimensional blade disc is 55 rpm / min, the temperature in the third rotating mixing container is 210°C, and the bulk density of the compacted mixed material is 250 kg / m 3 ~260kg / m 3 The moisture content of the compacted mixed material is less than 0.3%, and the particle size of the compacted mixed material is 1 mm to 2 mm.

[0033] S4, extruding the compacted mixed material through the first screw extruder, the first filter, the second filter, and the die extrusion device in sequence, cooling, and pelletizing to obtain recycled polyester chips. Specifically: the first screw extruder includes a material entry zone and a screw extrusion zone, the temperature of the material entry zone is 195°C, the screw extrusion zone includes five zones, the temperature of each screw extrusion zone is 275°C, the compacted mixed material entering the first screw extruder is in a vacuum atmosphere of 0.1mbar throughout the process, the filtration accuracy of the filter screen of the first filter is 30μm, and the temperature of the first filter is 270°C; the filtration accuracy of the filter screen of the second filter is 10μm, and the temperature of the second filter is 270°C.

[0034] According to the test, the intrinsic viscosity of the recycled polyester chips obtained in this embodiment is 0.715 dl / g to 0.725 dl / g, the content of terminal carboxyl groups is 32.0 mol / t to 33.0 mol / t, and the b value is 2.0 to 2.5.

[0035] Example 2

[0036] This embodiment provides a method for preparing a regenerated polyester chip for ultrafine denier fiber, comprising the following steps:

[0037] S1. Place the polyester waste silk particles in a first rotating mixing container with a first rotating three-dimensional blade, evacuate the first rotating mixing container, make the pressure in the first rotating mixing container 8mbar, cut and mix to compact the polyester waste silk particles, and obtain compacted polyester waste silk particles. Wherein: the particle size of the polyester waste silk particles is 3mm to 6mm, the moisture content of the polyester waste silk particles is less than 10%, and the bulk density of the polyester waste silk particles is 80kg / m 3 ~130kg / m 3 The rotation speed of the first rotating three-dimensional blade is 400 rpm / min, and the temperature in the first rotating mixing container is 160° C. The bulk density of the compacted polyester waste silk particles is 70 kg / m 3 ~100kg / m 3 The moisture content of the compacted polyester waste silk particles is less than 3%, and the particle size of the compacted polyester waste silk particles is 2 mm to 4 mm.

[0038] S2, placing the PET bottle flakes in a second rotating mixing container with a second rotating three-dimensional blade, evacuating the second rotating mixing container to make the pressure in the second rotating mixing container 8mbar, cutting and mixing to achieve compaction of the PET bottle flakes to obtain compacted bottle flakes. Wherein: the particle size of the PET bottle flakes is 4mm to 12mm, the moisture content of the PET bottle flakes is less than 5%, and the bulk density of the PET bottle flakes is 250kg / m 3 ~350kg / m 3 The speed of the second rotating three-dimensional blade is 90 rpm / min, and the temperature in the second rotating mixing container is 180°C. The bulk density of the compacted bottle flakes is 230 kg / m 3 ~280kg / m 3 The moisture content of the compacted bottle flakes is less than 2%, and the particle size of the compacted bottle flakes is 3 mm to 9 mm.

[0039] S3. 30% of the polyester waste silk particles compacted in step S1 and 70% of the bottle flakes compacted in step S2 are placed in a third rotating mixing container with a third rotating three-dimensional blade disc, and the third rotating mixing container is evacuated to a pressure of 3 mbar, and the compacted polyester waste silk particles and the compacted bottle flakes are cut and mixed to obtain a compacted mixed material. The rotation speed of the third rotating three-dimensional blade disc is 35 rpm / min, the temperature in the third rotating mixing container is 190°C, and the bulk density of the compacted mixed material is 260 kg / m 3 ~290kg / m 3 The moisture content of the compacted mixed material is less than 0.3%, and the particle size of the compacted mixed material is 1.5 mm to 3.5 mm.

[0040] S4, extruding the compacted mixed material through the first screw extruder, the first filter, the second filter, and the die extrusion device in sequence, cooling, and pelletizing to obtain recycled polyester chips. Specifically: the first screw extruder includes a material entry zone and a screw extrusion zone, the temperature of the material entry zone is 205°C, the screw extrusion zone includes five zones, and the temperature of each screw extrusion zone is 285°C. The compacted mixed material entering the first screw extruder is in a vacuum atmosphere of 0.5mbar throughout the process, the filtration accuracy of the filter screen of the first filter is 40μm, and the temperature of the first filter is 290°C; the filtration accuracy of the filter screen of the second filter is 15μm, and the temperature of the second filter is 290°C.

[0041] According to the test, the intrinsic viscosity of the recycled polyester chips obtained in this embodiment is 0.713 dl / g to 0.727 dl / g, the content of terminal carboxyl groups is 34.0 mol / t to 35.0 mol / t, and the b value is 3.0 to 3.5.

[0042] Example 3

[0043] This embodiment provides a method for preparing a regenerated polyester chip for ultrafine denier fiber, comprising the following steps:

[0044] S1. Place the polyester waste silk particles in a first rotating mixing container with a first rotating three-dimensional blade, evacuate the first rotating mixing container, make the pressure in the first rotating mixing container 7mbar, cut and mix to compact the polyester waste silk particles, and obtain compacted polyester waste silk particles. Wherein: the particle size of the polyester waste silk particles is 3mm to 6mm, the moisture content of the polyester waste silk particles is less than 10%, and the bulk density of the polyester waste silk particles is 80kg / m 3 ~130kg / m 3 The rotation speed of the first rotating three-dimensional blade is 450 rpm / min, and the temperature in the first rotating mixing container is 155°C. The bulk density of the compacted polyester waste silk particles is 65 kg / m 3 ~90kg / m 3 The moisture content of the compacted polyester waste silk particles is less than 3%, and the particle size of the compacted polyester waste silk particles is 2 mm to 3.5 mm.

[0045] S2, placing the PET bottle flakes in a second rotating mixing container with a second rotating three-dimensional blade, evacuating the second rotating mixing container to make the pressure in the second rotating mixing container 6mbar, cutting and mixing, so as to compact the PET bottle flakes to obtain compacted bottle flakes. Wherein: the particle size of the PET bottle flakes is 4mm to 12mm, the moisture content of the PET bottle flakes is less than 5%, and the bulk density of the PET bottle flakes is 250kg / m 3 ~350kg / m 3 The speed of the second rotating three-dimensional blade is 100 rpm / min, and the temperature in the second rotating mixing container is 175°C. The bulk density of the compacted bottle flakes is 230 kg / m 3 ~270kg / m 3 The moisture content of the compacted bottle flakes is less than 2%, and the particle size of the compacted bottle flakes is 3 mm to 8 mm.

[0046] S3. According to the percentage by mass, 20% of the polyester waste silk particles compacted in step S1 and 80% of the bottle flakes compacted in step S2 are placed in a third rotating mixing container with a third rotating three-dimensional blade disc, and the third rotating mixing container is evacuated to make the pressure in the third rotating mixing container 2mbar, and cut and mix to achieve the mixed compaction of the compacted polyester waste silk particles and the compacted bottle flakes to obtain a compacted mixed material. Wherein: the rotation speed of the third rotating three-dimensional blade disc is 45rpm / min, the temperature in the third rotating mixing container is 200℃, and the bulk density of the compacted mixed material is 260kg / m 3 ~280kg / m 3 The moisture content of the compacted mixed material is less than 0.3%, and the particle size of the compacted mixed material is 1.5 mm to 3 mm.

[0047] S4, extruding the compacted mixed material through the first screw extruder, the first filter, the second filter, and the die extrusion device in sequence, cooling, and pelletizing to obtain recycled polyester chips. Specifically: the first screw extruder includes a material entry zone and a screw extrusion zone, the temperature of the material entry zone is 200°C, the screw extrusion zone includes five zones, the temperature of each screw extrusion zone is 280°C, the compacted mixed material entering the first screw extruder is in a vacuum atmosphere of 0.3mbar throughout the process, the filtration accuracy of the filter screen of the first filter is 35μm, and the temperature of the first filter is 280°C; the filtration accuracy of the filter screen of the second filter is 13μm, and the temperature of the second filter is 280°C.

[0048] According to the test, the intrinsic viscosity of the recycled polyester chips obtained in this embodiment is 0.714 dl / g to 0.726 dl / g, the content of terminal carboxyl groups is 33.0 mol / t to 34.0 mol / t, and the b value is 2.5 to 3.0.

[0049] Comparative Example 1

[0050] The difference between this comparative example and Example 3 is that the polyester waste silk particles are directly placed in a third rotating mixing container with a third rotating three-dimensional knife disc for compaction, wherein: the particle size of the polyester waste silk particles is 3 mm to 6 mm, the moisture content of the polyester waste silk particles is less than 10%, and the bulk density of the polyester waste silk particles is 80 kg / m 3 ~130kg / m 3 The pressure in the third rotating mixing container is 2 mbar, the rotation speed of the third rotating three-dimensional blade is 45 rpm / min, and the temperature in the third rotating mixing container is 200°C; the bulk density of the compacted polyester waste silk particles is 70 kg / m 3 ~120kg / m 3The moisture content of the compacted polyester waste silk particles is less than 4%, and the particle size of the compacted mixed material is 2 mm to 5 mm.

[0051] Then, the compacted polyester waste silk particles are sequentially extruded through a first screw extruder, a first filter, a second filter, and a die extrusion device, cooled, and pelletized to obtain recycled polyester chips.

[0052] After testing, the intrinsic viscosity of the recycled polyester chips obtained in this comparative example is 0.680 dl / g to 0.700 dl / g, the content of terminal carboxyl groups is 30.0 mol / t to 31.0 mol / t, and the b value is 4.5 to 5.5.

[0053] Comparative Example 2

[0054] The difference between this comparative example and Example 3 is that the PET bottle flakes are directly placed in a third rotating mixing container with a third rotating three-dimensional knife disc for compaction, wherein: the particle size of the PET bottle flakes is 4 mm to 12 mm, the moisture content of the PET bottle flakes is less than 5%, and the bulk density of the PET bottle flakes is 250 kg / m 3 ~350kg / m 3 The pressure in the third rotating mixing container is 2 mbar, the speed of the third rotating three-dimensional blade is 45 rpm / min, and the temperature in the third rotating mixing container is 200°C; the bulk density of the compacted bottle flakes is 230 kg / m 3 ~330kg / m 3 The moisture content of the compacted bottle flakes is less than 2.5%, and the particle size of the compacted bottle flakes is 3 mm to 10 mm.

[0055] The PET bottle flakes are sequentially extruded through a first screw extruder, a first filter, a second filter, and a die extrusion device, cooled, and pelletized to obtain recycled polyester chips.

[0056] After testing, the intrinsic viscosity of the recycled polyester chips obtained in this comparative example is 0.730 dl / g to 0.750 dl / g, the content of terminal carboxyl groups is 37.0 mol / t to 38.0 mol / t, and the b value is 6.0 to 7.0.

[0057] Comparative Example 3

[0058] The difference between this comparative example and Example 3 is that, by mass percentage, 20% of the polyester waste silk particles that have not been compacted in step S1 and 80% of the bottle flakes that have not been compacted in step S2 are directly placed in a third rotating mixing container with a third rotating three-dimensional knife disc, and the third rotating mixing container is evacuated to make the pressure in the third rotating mixing container 2mbar, and cutting and mixing are performed to achieve the mixed compaction of the compacted polyester waste silk particles and the compacted bottle flakes to obtain a compacted mixed material. Wherein: the rotation speed of the third rotating three-dimensional knife disc is 45rpm / min, the temperature in the third rotating mixing container is 200℃, and the bulk density of the compacted mixed material is 270kg / m 3 ~370kg / m 3 The moisture content of the compacted mixed material is less than 0.3%, and the particle size of the compacted mixed material is 2 mm to 4.5 mm. The particle size of the polyester waste silk particles is 3 mm to 6 mm, the moisture content of the polyester waste silk particles is less than 10%, and the bulk density of the polyester waste silk particles is 80 kg / m 3 ~130kg / m 3 The particle size of the PET bottle flakes is 4mm to 12mm, the moisture content of the PET bottle flakes is less than 5%, and the bulk density of the PET bottle flakes is 250kg / m 3 ~350kg / m 3 The pressure in the third rotating mixing container is 2 mbar, the rotation speed of the third rotating three-dimensional blade is 45 rpm / min, and the temperature in the third rotating mixing container is 200°C.

[0059] The compacted mixed material is sequentially extruded through a first screw extruder, a first filter, a second filter, and a die extrusion device, cooled, and pelletized to obtain recycled polyester chips.

[0060] According to the test, the intrinsic viscosity of the recycled polyester chips obtained in this comparative example is 0.700 dl / g to 0.740 dl / g, the content of terminal carboxyl groups is 36.0 mol / t to 37.0 mol / t, and the b value is 5.0 to 6.0.

[0061] The performance data of the recycled polyester chips of Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 1:

[0063] Table 1:

[0064]

[0065] In Table 1, the intrinsic viscosity of the chips suitable for producing ultrafine denier fibers is 0.720 dl / g, and the intrinsic viscosity fluctuation range refers to the difference between the intrinsic viscosity values ​​of the recycled polyester chips measured in Examples 1 to 3 and Comparative Examples 1 to 3 and 0.720 dl / g.

[0066] The melt produced by the slices with high intrinsic viscosity has high intrinsic viscosity and poor fluidity. The melt with high intrinsic viscosity has a large expansion rate when it is ejected from the spinneret, which is easy to produce injection head silk and increase the broken ends of the silk. The melt produced by the slices with low intrinsic viscosity has low intrinsic viscosity and relatively better fluidity, but too low intrinsic viscosity will lead to reduced strength of the spun silk, and it is easy to produce hairy silk and broken ends. In addition, the wide fluctuation range of the intrinsic viscosity of the slices will also increase the hairy silk and broken ends after spinning, while the product quality will decrease and the dyeing M rate will be very low. This is mainly because the intrinsic viscosity of the slices with different intrinsic viscosities is different after melting, so the rheological properties deteriorate. The closer the intrinsic viscosity of the slices is to the center value, the better the effect. In addition, the smaller the fluctuation range of the intrinsic viscosity, the better the effect.

[0067] Comparative Example 1 is a superfine fiber slice prepared by directly compacting polyester waste silk particles. Its overall viscosity is low. Although the b value is small, the strength of the spun silk is reduced, and it is easy to produce hairy silk and broken ends. Comparative Example 2 is a superfine fiber slice prepared by directly compacting PET bottle chips. Its overall viscosity is high, and the viscosity fluctuation range is also large. The b value is large. The melt with high intrinsic viscosity has a large expansion rate when it is ejected from the spinneret, which is easy to produce injection head silk, increase the broken ends of the silk, and the appearance of the spinning is not good. Comparative Example 3 is a superfine fiber slice prepared by mixing uncompacted polyester waste silk particles and PET bottle chips. Its intrinsic viscosity value is closer to 0.720dl / g, but the fluctuation range of the intrinsic viscosity value is large. The slices with different intrinsic viscosity values ​​with large differences are mixed and melt-spun, and the fluidity is poor.

[0068] In Examples 1 to 3 of the present application, the polyester waste silk particles and PET bottle flakes are mixed to control the intrinsic viscosity of the final slices to near the optimal intrinsic viscosity value, and the polyester waste silk particles and PET bottle flakes are compacted separately and then finally mixed and compacted. The fluctuation range of the bulk density of the mixed material is reduced, and then the fluctuation range of the intrinsic viscosity of the final slices is reduced, that is, the difference between the intrinsic viscosity value of the final slice and 0.720dl / g is controlled within ±0.007. The smaller the fluctuation range of the intrinsic viscosity of the slice, the smaller the b value. Therefore, compared with Comparative Example 3, the slices prepared by Examples 1 to 3 are more suitable for the production of ultrafine denier polyester fibers.

[0069] The terminal carboxyl content is also an important parameter for evaluating the quality of polyester, which reflects the unreacted PTA or degradation products. In theory, fully reacted polyester should have no terminal carboxyl groups, but in actual production, the content will be affected by many factors. The national standard stipulates that the terminal carboxyl content is in the range of 18 to 36. The higher the intrinsic viscosity, the higher the terminal carboxyl content. The content of terminal carboxyl groups (COOH number) increases with the increase of intrinsic viscosity. The intrinsic viscosity is controlled between 0.713 and 0.727, and the terminal carboxyl group is controlled between 32.0 and 35.0. This range is better, and the larger the terminal carboxyl group, the greater the degree of degradation.

[0070] The longer the residence time of the material in the screw, the greater the degree of material degradation, and the higher the b value (yellowness of the slice). The present application controls the intrinsic viscosity between 0.713 and 0.727, and the b value of the slice is 2.0 to 3.5. Because the present application takes into account the uniformity of the material before entering the screw for extrusion, the uniformity is guaranteed, which can increase the output of the equipment and reduce the residence time of the material in the screw. Therefore, the b value is very small, and the impact on the appearance of the fiber after spinning is small, which meets the requirements for slices for ultrafine denier fibers.

[0071] In summary, the present application starts from the uniformity of the material before entering the screw, and controls the uniformity of the material before entering the screw to a very small range, so that the screw speed can be increased accordingly, and the output can be increased, while reducing the time the material stays in the screw, reducing the degradation of the material due to high temperature, thereby obtaining high-quality slices suitable for ultrafine denier fibers. In addition, the present application controls the uniformity of the material before entering the screw to a very small range, and even at a high speed, slices with good characteristic viscosity uniformity suitable for ultrafine denier fibers can be produced.

[0072] Although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0073] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present application. They are not intended to limit the scope of protection of the present application. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present application should be included in the scope of protection of the present application.

Claims

1. A method for preparing a recycled polyester chip, characterized in that: The steps include: S1, placing the polyester waste silk particles in a first rotating mixing container with a first rotating three-dimensional knife disc for cutting and mixing, so as to compact the polyester waste silk particles to obtain compacted polyester waste silk particles, wherein the moisture content of the compacted polyester waste silk particles is less than 3%; S2, placing the PET bottle flakes in a second rotating mixing container with a second rotating three-dimensional knife disc for cutting and mixing, so as to compact the bottle flakes to obtain compacted bottle flakes, wherein the moisture content of the compacted bottle flakes is less than 2%; S3, by mass percentage, placing 10% to 30% of the compacted polyester waste silk particles obtained in step S1 and 70% to 90% of the compacted bottle flakes obtained in step S2 in a third rotating mixing container with a third rotating three-dimensional knife disc for cutting and mixing, so as to achieve mixing and compacting of the compacted polyester waste silk particles and the compacted bottle flakes to obtain a compacted mixed material, wherein the moisture content of the compacted mixed material is less than 0.3%; S4, extruding the compacted mixed material through a first screw extruder, a first filter, a second filter, and a die extrusion device in sequence, cooling, and pelletizing to obtain recycled polyester chips.

2. The method for preparing the recycled polyester chips according to claim 1, characterized in that: In step S1, the particle size of the polyester waste silk particles is 3 mm to 6 mm, the moisture content of the polyester waste silk particles is less than 10%, and the bulk density of the polyester waste silk particles is 80 kg / m 3 ~130kg / m 3 The rotation speed of the first rotating three-dimensional blade is 400 rpm / min to 500 rpm / min, and the temperature in the first rotating mixing container is 150°C to 160°C.

3. The method for preparing the recycled polyester chips according to claim 2, characterized in that: In step S1, the first rotating mixing container is evacuated to make the pressure in the first rotating mixing container be 5 mbar to 8 mbar.

4. The method for preparing the recycled polyester chips according to claim 1, characterized in that: In step S2, the particle size of the PET bottle flakes is 4 mm to 12 mm, the moisture content of the PET bottle flakes is less than 5%, and the bulk density of the PET bottle flakes is 250 kg / m 3 ~350kg / m 3 The rotation speed of the second rotating three-dimensional blade disc is 90 rpm / min to 110 rpm / min, and the temperature in the second rotating mixing container is 170°C to 180°C.

5. The method for preparing the recycled polyester chips according to claim 4, characterized in that: In step S2, the second rotating mixing container is evacuated to make the pressure in the second rotating mixing container be 5 mbar to 8 mbar.

6. The method for preparing the recycled polyester chips according to claim 1, characterized in that: In step S3, the rotation speed of the third rotating three-dimensional blade disc is 35 rpm / min to 55 rpm / min, and the temperature in the third rotating mixing container is 190°C to 210°C.

7. The method for preparing the recycled polyester chips according to claim 6, characterized in that: In step S3, the third rotating mixing container is evacuated to make the pressure in the third rotating mixing container be 1 mbar to 3 mbar.

8. The method for preparing the recycled polyester chips according to claim 1, characterized in that: In step S4, the first screw extruder includes a material entry zone and a screw extrusion zone, the temperature of the material entry zone is 195°C to 205°C, the temperature of the screw extrusion zone is 275°C to 285°C, the compacted mixed material entering the first screw extruder is in a vacuum atmosphere of 0.1mbar to 0.5mbar throughout the process, the filtering accuracy of the filter mesh of the first filter is 30μm to 40μm, and the temperature of the first filter is 270°C to 290°C; the filtering accuracy of the filter mesh of the second filter is 10μm to 15μm, and the temperature of the second filter is 270°C to 290°C.

9. A recycled polyester chip, characterized in that: The regenerated polyester chip is prepared by the preparation method of any one of claims 1 to 8.

10. An ultrafine fiber, characterized in that: The ultrafine denier fiber is prepared from the regenerated polyester chips described in claim 9.

Citation Information

Cited By

  • Preparation forming method and production line of high-toughness and high-flowability regenerated PET (polyethylene terephthalate) slices