Preparation process of modified non-woven fabric convenient for ink-jet printing

Through the modified non-woven fabric process, the combination of fiber and modified slurry and inkjet printing technology are used to solve the formaldehyde problem of non-woven fabrics in board decoration, improve environmental protection performance and decorative effect, and realize the traditional paint-free board replacement.

CN118906589AActive Publication Date: 2024-11-08ZHEJIANG HENGBANG NONWOVEN TECH CO LTD

Patent Information

Application Number
CN202411286010.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-08
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The existing non-woven fabrics have high formaldehyde content in the surface decoration of the board, insufficient environmental protection performance, insufficient covering, wrinkle resistance and hardness, which cannot replace the decorative effect of traditional paint-free boards.

Method used

By using the modified non-woven fabric preparation process, by mixing wood pulp fibers, resin fibers, bamboo charcoal fibers and other fibers and filling them with the modified slurry, combined with the base color coating, a surface that is easy to inkjet printing is formed, which directly replaces the technological wood veneer and Decorative paper, bonded with water-based environmentally friendly glue.

Benefits of technology

It improves the hardness, wrinkle resistance and coverability of non-woven fabrics, reduces the formaldehyde content, significantly improves the environmental protection level of the board, realizes the decorative effect of inkjet printing, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of non-woven fabrics, and discloses a preparation process of a modified non-woven fabric convenient for ink-jet printing, which comprises the following steps: S1, preparing a non-woven fabric: preparing the following fibers in parts by weight: 4-7 parts of wood pulp fibers, 5-12 parts of resin fibers, 3-5 parts of bamboo charcoal fibers and 2-3 parts of viscose fibers; the fibers are mixed, opened, combed and spun-laced or needled to be made into non-woven fabric; s2, non-woven fabric modification treatment; s3, preparing a ground color coating: roller-coating the upper surface of the modified non-woven fabric with ground color slurry, slicking the ground color slurry, and drying the ground color slurry to form the ground color coating convenient for ink-jet printing; the ground color slurry is prepared from the following components in parts by weight: 5 to 12 parts of nano titanium dioxide, 20 to 28 parts of an adhesive, 0.6 to 1.35 parts of a coupling agent and 0.3 to 0.5 part of a dispersing agent. The wood veneer is environment-friendly, can replace a technical wood veneer to be compounded with a board, and improves the environmental protection grade of the board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonwoven fabrics, and in particular to a preparation process of modified nonwoven fabrics that are convenient for inkjet printing. Background Art

[0002] In the home furnishing industry, the use of board materials (mainly wood boards) is very large. The most common paint-free board is usually made by hot-pressing a layer of technological veneer on the surface of the board, and then coating the surface of the technological veneer with a layer of decorative paper to make a paint-free board. The technological veneer is made by bonding solid wood veneers with impregnated glue. The formaldehyde content in the impregnated glue is very high. The decorative paper is also called impregnated film paper. The decorative paper is hot-pressed with the technological veneer. Since the impregnated glue content in the technological veneer and decorative paper is very high, the formaldehyde content in the paint-free board is high, which is not environmentally friendly.

[0003] For example, the Chinese patent number is 2021110423445, which discloses a preparation process of a non-woven fabric that can replace natural veneer. This non-woven fabric increases the connection strength with the decorative paper and can better prevent glue penetration. However, the strength of this non-woven fabric and the decorative paper cannot meet the requirements when bonded with aqueous environmentally friendly glue. If impregnated glue is used for bonding, the impregnated glue contains a large amount of formaldehyde, and the environmental protection performance is insufficient. Moreover, the covering and wrinkle resistance of this non-woven fabric are still defective. When it replaces the technological veneer and is compounded with the board, the decorative effect of the board surface cannot achieve the effect of the existing paint-free board: and the hardness of this non-woven fabric is insufficient, and it is easy to be partially concave after being pressed, which affects the decorative effect of the board surface. Summary of the invention

[0004] In order to solve the above-mentioned problems existing in the prior art when non-woven fabrics are applied to the surface devices of boards, the present invention provides a preparation process of a modified non-woven fabric that is convenient for inkjet printing. The modified non-woven fabric prepared by this process can directly replace natural veneer for board surface decoration. The hardness, wrinkle resistance and hiding power all meet the requirements for board surface decoration. Inkjet printing can be directly performed on the surface of the modified non-woven fabric, which directly eliminates the need for decorative paper and the use of impregnated glue, thereby having better environmental protection performance.

[0005] In order to achieve the above object, the present invention adopts the following technical solution: A process for preparing a modified nonwoven fabric that is convenient for inkjet printing comprises the following steps: S1. Preparing a nonwoven fabric: preparing fibers according to the following weight parts: 4-7 parts of wood pulp fiber, 5-12 parts of resin fiber, 3-5 parts of bamboo charcoal fiber, and 2-3 parts of viscose fiber, and mixing, opening, carding, spunlacing or needle-punching the above fibers to form a nonwoven fabric; S2, non-woven fabric modification treatment: immersing the non-woven fabric in the modified slurry so that the modified slurry fills the gaps of the non-woven fabric, and then entering the drying area for drying after double-roll extrusion to form the modified non-woven fabric; the modified slurry includes the following components by weight: 5-10 parts of calcium carbonate powder, 20-32 parts of adhesive, 0.5-2.4 parts of coupling agent, and 0.5-1.5 parts of dispersant; S3. Prepare a base color coating: Roll-coat the base color slurry on the upper surface of the modified non-woven fabric and scrape it flat. After the base color slurry dries, a base color coating that is convenient for inkjet printing is formed; the base color slurry includes the following weight components: 5-12 parts of nano titanium dioxide, 20-28 parts of adhesive, 0.6-1.35 parts of coupling agent, and 0.3-0.5 parts of dispersant.

[0006] By adopting the above technical scheme: firstly, resin fiber and bamboo charcoal fiber are added to the fiber of the non-woven fabric. The resin fiber has high strength, corrosion resistance and wear resistance, which increases the overall strength and wear resistance of the non-woven fabric. The bamboo charcoal fiber has good adsorption. When compounded with the board, it can absorb volatile formaldehyde and other toxic gases in the board and improve the environmental protection level of the board; after the non-woven fabric is modified by the modified slurry, the pores in the non-woven fabric are filled with the modified slurry, so that the hardness, strength and light-shielding property of the non-woven fabric are improved, while the ductility (to prevent stretching and cracking), air permeability and water absorption (to prevent glue penetration during subsequent use) of the non-woven fabric are reduced, and a surface layer of the modified non-woven fabric is provided with a A base coating is placed, and the nano titanium dioxide in the base coating makes the surface of the modified non-woven fabric flatter, smoother and whiter. When subsequently inkjet printing (pattern or texture) is performed, the pattern is clearer and the color is more authentic. At the same time, the adhesion performance between the ink and the base coating is also better. This modified non-woven fabric can be directly bonded to the board through water-based environmentally friendly glue, thereby directly replacing the hot pressing (impregnated glue) compounding of the technical veneer and the board. Subsequently, inkjet printing can directly replace the hot pressing impregnated decorative paper (containing formaldehyde), significantly improving the environmental protection level of the board. Moreover, the modified non-woven fabric can be rolled and bent, making production and transportation more convenient. When compounded with the board, the board can be directly hemmed at right angles.

[0007] Preferably, the fibers in step S1 further include 2-4 parts by weight of polyester fibers. The polyester fibers further improve the tensile and wrinkle resistance of the nonwoven fabric.

[0008] Preferably, the lower surface of the non-woven fabric obtained in step S1 is melt-blown, and a melt-blown layer is formed on the lower surface of the non-woven fabric after the melt-blown treatment; during melt-blowing, the polymer melt in the melt-blowing die head comprises the following components in parts by weight: 5-8 parts of polypropylene fiber and 2-3 parts of ES bonding fiber, the melt flow index of the polymer melt is 90-120 g / 10 min, the temperature of the melt-blowing die head is 195-205°C, the air flow injection angle in the melt-blowing die head is 35-40°, the pressure of the hot air flow in the melt-blowing die head is 0.1-0.18 MPa, and the polymer melt extrusion amount is 0.2-0.4 g / hole / min.

[0009] The meltblown layer is formed by meltblowing on the lower surface of the non-woven fabric. The fibers of the meltblown layer are denser and the pores are smaller, which makes the porosity of the non-woven fabric and the meltblown layer different. After subsequent immersion in the modified slurry, the non-woven fabric has a high content of modified slurry and a low content of modified slurry in the meltblown layer. Therefore, the hardness of the layer where the non-woven fabric is located is higher, smoother, and has low water absorption. The upper surface of the non-woven fabric is smoother when preparing the base color coating, which reduces ink penetration and makes the pattern clearer; while the hardness of the layer where the meltblown layer is located is relatively low, the water absorption is relatively high, and the toughness is better. When in use, the lower surface of the meltblown layer is compounded with the board through water-based environmentally friendly glue. The glue can better penetrate into the meltblown layer but cannot penetrate the non-woven fabric layer. While improving the composite strength of the meltblown layer and the board, it can effectively prevent the glue from penetrating the non-woven fabric; and the meltblown layer made of polypropylene fiber has a better sound insulation effect, which can improve the sound insulation effect of the board after compounding with the board.

[0010] Preferably, the nonwoven fabric prepared in step S1 has a gram weight of 60-150 g / ㎡, the gram weight of the meltblown layer is 30-50 g / ㎡, and the total gram weight of the nonwoven fabric after meltblowing is 90-200 g / ㎡; hot rolling is performed after meltblowing. Hot rolling makes the combination of the meltblown layer and the nonwoven fabric more stable on the one hand, and makes the fiber gaps in the nonwoven fabric and the meltblown layer smaller and more compact on the other hand, so that the overall toughness of bending can be maintained during subsequent modification treatment.

[0011] Preferably, the modified pulp in step S2 further comprises 5-20 parts by weight of bamboo pulp fibers, which enhance crack resistance and prevent surface cracking of the modified nonwoven fabric when it is rolled or bent.

[0012] Preferably, the double rollers in step S2 are configured as two groups, namely the first double roller and the second double roller, and a pre-drying zone is provided between the first double roller and the second double roller; the non-woven fabric base layer soaked in the modified slurry passes through the first double roller, the pre-drying zone, the second double roller, and the drying zone in sequence, and the modified slurry in the non-woven fabric after passing through the pre-drying zone reaches the basic hardening stage, and then enters the second double roller, and finally reaches the complete hardening stage in the drying zone.

[0013] The treatment method of primary extrusion, pre-drying, secondary extrusion and drying is adopted to eliminate the internal stress of the modified slurry during the hardening process and prevent the modified non-woven fabric from cracking. At the same time, secondary rolling is performed in the basic hardening stage to make the surface of the non-woven fabric smoother, which is conducive to the preparation of a smoother base color coating.

[0014] Preferably, the gram weight increment of the non-woven fabric after the modification treatment in step S2 is 25-45 g / ㎡. That is, the content of the modified slurry is adjusted by the rolling gap of the double rollers, and the gram weight increment of the non-woven fabric is the gram weight after the modified slurry is solidified. By limiting this gram weight, the hardness and wrinkle resistance of the modified non-woven fabric meet the requirements, and the surface layer of the modified non-woven fabric will not crack when it is rolled or bent.

[0015] Preferably, the roller surface corresponding to the lower side of the non-woven fabric in the second double roller is provided with spherical bosses distributed in an array, and the lower surface of the non-woven fabric forms spherical concave holes distributed in an array on the lower surface after passing through the second double roller. On the one hand, the spherical concave holes reduce the strength of the lower surface of the modified non-woven fabric, making it easier to bend and fold toward the lower surface; on the other hand, when the lower surface of the modified non-woven fabric is compounded with the board through glue, the spherical concave holes can increase the bonding surface bond and improve the bonding strength; thirdly, when the modified non-woven fabric is compounded with the board, the sound insulation performance of the board can be increased. Since the glue in the spherical concave holes is different from the components of the modified non-woven fabric, when the sound wave is incident from one medium (modified non-woven fabric) to another medium (solidified glue) with different acoustic properties, reflection will occur at the interface between the two media (the spherical pore wall of the spherical concave hole), and the sound will be reflected in different directions along the spherical surface, thereby greatly weakening the penetration of the sound and improving the sound insulation effect.

[0016] Preferably, the ratio of the depth of the spherical concave holes to the total thickness of the non-woven fabric after the modification treatment in step S2 is 0.25-0.35.

[0017] Preferably, in step S3, the base color slurry includes the following components by weight: 2-5 parts of precipitated barium sulfate powder and 0.15-0.35 parts of defoamer; the particle size of the nano titanium dioxide is 10-50nm, and the particle size of the precipitated barium sulfate powder is 200-400nm. The defoamer can eliminate bubbles in the slurry when stirring the base color slurry, making the base color coating smoother; the precipitated barium sulfate powder itself is white, and the difference in particle size between the precipitated barium sulfate powder and the nano titanium dioxide is used to make the surface roughness of the base color coating finally made greater than that of the nano titanium dioxide alone, and this roughness can increase the surface area of ​​inkjet printing, improve the adhesion performance of ink and base color coating, and make the inkjet printing pattern clearer and better in color.

[0018] Therefore, the present invention has the following beneficial effects: (1) the modified non-woven fabric does not contain formaldehyde, and is more environmentally friendly when used to replace technological veneer; (2) the base color coating of the modified non-woven fabric can be directly inkjet printed to form a decorative layer, eliminating the need for decorative paper and the impregnation of decorative paper, thereby further improving the loop performance; (3) the overall quality of the modified non-woven fabric is controllable and has better consistency; (4) the modified non-woven fabric can be rolled up and folded, making transportation more convenient and the size design more flexible; (5) the modified non-woven fabric can be rolled up and folded, so it can be continuously and automatically produced on a production line, greatly reducing the manufacturing cost. DETAILED DESCRIPTION

[0019] In order to make the technical problems, technical solutions and beneficial technical effects to be solved by the present invention more clearly understood, the present invention will be further described in detail below in combination with multiple exemplary embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the scope of protection of the present invention.

[0020] It should be understood that, in this document, the expressions "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance, nor should they be understood as implicitly indicating the number of technical features indicated. Features defined as "first" or "second" may explicitly or implicitly indicate that at least one of the features is included.

[0021] A preparation process of a modified non-woven fabric that is convenient for inkjet printing, comprising the following steps: S1, preparing the non-woven fabric: preparing fibers according to the following weight parts: 4-7 parts of wood pulp fiber, 5-12 parts of resin fiber, 3-5 parts of bamboo charcoal fiber, and 2-3 parts of viscose fiber, and mixing, opening, combing, spunlacing or needle-punching the above fibers to form a non-woven fabric with a gram weight of 60-150g / ㎡; S2, modifying the non-woven fabric: immersing the non-woven fabric in a modified slurry so that the modified slurry fills the gaps of the non-woven fabric, and then entering a drying area for drying after double-roll extrusion treatment to form a modified non-woven fabric; the modified slurry comprises the following weight parts: 5-10 parts of calcium carbonate powder, 20-32 parts of adhesive, 0.5-2.4 parts of coupling agent, and 0.5-1.5 parts of dispersant, and the gram weight increase of the non-woven fabric after the modification is 25-45 g / ㎡; S3. Prepare base color coating: Roll the base color slurry on the upper surface of the modified non-woven fabric and scrape it flat. After the base color slurry is dried, a base color coating that is convenient for inkjet printing is formed; the base color slurry includes the following weight components: 5-12 parts of nano titanium dioxide, 20-28 parts of adhesive, 0.6-1.35 parts of coupling agent, and 0.3-0.5 parts of dispersant.

[0022] Embodiment 1: A preparation process of a modified non-woven fabric that is convenient for inkjet printing, comprising the following steps: S1, preparing the non-woven fabric: preparing fibers according to the following weight parts: 4 parts of wood pulp fiber, 5 parts of resin fiber, 3 parts of bamboo charcoal fiber, and 2 parts of viscose fiber, mixing the above fibers, opening, combing, and spunlacing to form a non-woven fabric with a gram weight of 60g / ㎡; S2, modifying the non-woven fabric: immersing the non-woven fabric in the modified slurry so that the modified slurry fills the gaps in the non-woven fabric, and then entering a drying area for drying after double-roll extrusion to form a non-woven fabric with a gram weight of 85g / ㎡ modified non-woven fabric; the modified slurry includes the following weight parts: 5 parts of calcium carbonate powder, 20 parts of adhesive, 0.5 parts of coupling agent, and 0.5 parts of dispersant; S3, prepare the base color coating: roll the base color slurry on the upper surface of the modified non-woven fabric and scrape it flat, and the base color slurry forms a base color coating that is convenient for inkjet printing after drying; the base color slurry includes the following weight parts: 5 parts of nano titanium dioxide, 20 parts of adhesive, 0.6 parts of coupling agent, and 0.3 parts of dispersant, and the particle size of nano titanium dioxide is 10-50nm. The total gram weight of the modified non-woven fabric finally obtained is 100g / ㎡, and the total thickness is 0.2mm.

[0023] Embodiment 2: A preparation process of a modified non-woven fabric that is convenient for inkjet printing, comprising the following steps: S1, preparing the non-woven fabric: preparing fibers according to the following weight parts: 7 parts of wood pulp fiber, 12 parts of resin fiber, 5 parts of bamboo charcoal fiber, 3 parts of viscose fiber, and 4 parts of polyester fiber, mixing the above fibers, opening, combing, and needle punching to form a non-woven fabric with a gram weight of 150g / ㎡; S2, non-woven fabric modification treatment: immersing the non-woven fabric in a modified slurry so that the modified slurry fills the gaps in the non-woven fabric, and then entering a drying area for drying after double-roll extrusion treatment to form a modified non-woven fabric with a gram weight of 195g / ㎡; the modified slurry comprises the following weight parts: Components: 10 parts of calcium carbonate powder, 20 parts of bamboo pulp fiber, 32 parts of adhesive, 2.4 parts of coupling agent, 1.5 parts of dispersant; S3, prepare the base color coating: roll the base color slurry on the upper surface of the modified non-woven fabric and scrape it flat. After the base color slurry is dried, a base color coating that is convenient for inkjet printing is formed; the base color slurry includes the following weight components: 12 parts of nano titanium dioxide, 5 parts of precipitated barium sulfate powder, 0.35 parts of defoaming agent, 28 parts of adhesive, 1.35 parts of coupling agent, 0.5 parts of dispersant, the particle size of nano titanium dioxide is 10-50nm, and the particle size of precipitated barium sulfate powder is 200-400nm. The total gram weight of the modified non-woven fabric finally obtained is 225g / ㎡, and the total thickness is 0.4mm.

[0024] Embodiment 3: A preparation process of a modified non-woven fabric that is convenient for inkjet printing, comprising the following steps: S1, preparing the non-woven fabric: preparing fibers according to the following weight parts: 5.5 parts of wood pulp fiber, 8.5 parts of resin fiber, 4 parts of bamboo charcoal fiber, 2.5 parts of viscose fiber, and 3 parts of polyester fiber, mixing the above fibers, opening, combing, and spunlacing to form a non-woven fabric with a gram weight of 105g / ㎡; S2, modifying the non-woven fabric: immersing the non-woven fabric in a modified slurry so that the modified slurry fills the gaps in the non-woven fabric, and then entering a drying area for drying after double-roll extrusion treatment to form a modified non-woven fabric with a gram weight of 140g / ㎡; the modified slurry comprises: The following components by weight: 7.5 parts of calcium carbonate powder, 12 parts of bamboo pulp fiber, 26 parts of adhesive, 1.4 parts of coupling agent, and 1 part of dispersant; S3, preparation of base color coating: roll the base color slurry on the upper surface of the modified non-woven fabric and scrape it flat, and the base color slurry is dried to form a base color coating that is convenient for inkjet printing; the base color slurry includes the following weight components: 8.5 parts of nano titanium dioxide, 3.5 parts of precipitated barium sulfate powder, 0.25 parts of defoamer, 24 parts of adhesive, 1 part of coupling agent, and 0.4 parts of dispersant. The particle size of nano titanium dioxide is 10-50nm, and the particle size of precipitated barium sulfate powder is 200-400nm. The total gram weight of the modified non-woven fabric finally obtained is 160g / ㎡, and the total thickness is 0.32mm.

[0025] Embodiment 4: A preparation process of a modified non-woven fabric that is convenient for inkjet printing, comprising the following steps: S1, preparing the non-woven fabric: preparing fibers according to the following weight parts: 5.5 parts of wood pulp fiber, 8.5 parts of resin fiber, 4 parts of bamboo charcoal fiber, 2.5 parts of viscose fiber, and 2 parts of polyester fiber, and mixing, opening, combing, and spunlacing the above fibers to form a non-woven fabric with a gram weight of 110g / ㎡; S2, non-woven fabric modification treatment: immersing the non-woven fabric in a modified slurry so that the modified slurry fills the gaps in the non-woven fabric, and then entering a drying area for drying after double-roll extrusion treatment to form a modified non-woven fabric with a gram weight of 150g / ㎡; the modified slurry contains The following components are included by weight: 7.5 parts of calcium carbonate powder, 5 parts of bamboo pulp fiber, 26 parts of adhesive, 1.4 parts of coupling agent, and 1 part of dispersant; S3, preparing the base color coating: rolling the base color slurry on the upper surface of the modified non-woven fabric and scraping it flat, and the base color slurry is dried to form a base color coating that is convenient for inkjet printing; the base color slurry includes the following components by weight: 8.5 parts of nano titanium dioxide, 2 parts of precipitated barium sulfate powder, 0.15 parts of defoaming agent, 24 parts of adhesive, 1 part of coupling agent, and 0.4 parts of dispersant. The particle size of nano titanium dioxide is 10-50nm, and the particle size of precipitated barium sulfate powder is 200-400nm. The total gram weight of the modified non-woven fabric finally obtained is 165g / ㎡, and the total thickness is 0.35mm.

[0026] Embodiment 5: A process for preparing a modified non-woven fabric that is convenient for inkjet printing, comprising the following steps: S1, preparing the non-woven fabric: preparing fibers according to the following weight parts: 5.5 parts of wood pulp fiber, 8.5 parts of resin fiber, 4 parts of bamboo charcoal fiber, 2.5 parts of viscose fiber, and 3 parts of polyester fiber, mixing the above fibers, opening, combing, and spunlacing to form a non-woven fabric with a gram weight of 105 g / ㎡; performing melt-blowing treatment on the lower surface of the non-woven fabric, and forming a melt-blown layer with a gram weight of 30 g / ㎡ on the lower surface of the non-woven fabric after the melt-blowing treatment; during melt-blowing, the polymer melt in the melt-blowing die head comprises the following weight parts: 5 parts of polypropylene fiber and 2 parts of ES bonding fiber, the melt flow index of the polymer melt is 90 g / 10 min, the temperature of the melt-blowing die head is 195°C, the air flow injection angle in the melt-blowing die head is 40°, the pressure of the hot air flow in the melt-blowing die head is 0.1 Mpa, the polymer melt extrusion amount is 0.2 g / hole / min, and hot rolling treatment is performed after melt-blowing; S2. Modification of non-woven fabric: immerse the non-woven fabric in the modified slurry so that the modified slurry fills the gaps in the non-woven fabric, and then enters the drying area for drying after double-roll extrusion to form a modified non-woven fabric with a gram weight of 170g / ㎡; the modified slurry includes the following components in parts by weight: 7.5 parts of calcium carbonate powder, 12 parts of bamboo pulp fiber, 26 parts of adhesive, 1.4 parts of coupling agent, and 1 part of dispersant; S3. Preparation of base color coating: roll the base color slurry on the upper surface of the modified non-woven fabric and scrape it flat. After the base color slurry is dried, a base color coating that is convenient for inkjet printing is formed; the base color slurry includes the following components in parts by weight: 9 parts of nano titanium dioxide, 4 parts of precipitated barium sulfate powder, 0.25 parts of defoaming agent, 24 parts of adhesive, 1 part of coupling agent, and 0.4 parts of dispersant. The particle size of the nano titanium dioxide is 10-50nm, and the particle size of the precipitated barium sulfate powder is 200-400nm. The final modified nonwoven fabric has a total weight of 190 g / m2 and a total thickness of 0.38 mm.

[0027] Embodiment 6: The difference between this embodiment and embodiment 5 is that: in step S1, the lower surface of the non-woven fabric is melt-blown, and a melt-blown layer with a gram weight of 50 g / ㎡ is formed on the lower surface of the non-woven fabric after the melt-blowing treatment; during melt-blowing, the polymer melt in the melt-blowing die head includes the following components in parts by weight: 8 parts of polypropylene fiber and 3 parts of ES bonding fiber, the melt flow index of the polymer melt is 120g / 10min, the temperature of the melt-blowing die head is 205°C, the air flow injection angle in the melt-blowing die head is 35°, the pressure of the hot air flow in the melt-blowing die head is 0.18Mpa, the polymer melt extrusion amount is 0.4g / hole / min, and hot rolling treatment is performed after melt-blowing; in step S2, after double-roll extrusion treatment, it enters the drying area for drying to form a modified non-woven fabric with a gram weight of 180g / ㎡; in step S3, the total gram weight of the modified non-woven fabric finally obtained is 200g / ㎡, and the total thickness is 0.42mm.

[0028] Embodiment 7: The difference between this embodiment and embodiment 5 is that: in step S1, the lower surface of the non-woven fabric is melt-blown, and a melt-blown layer with a gram weight of 40 g / ㎡ is formed on the lower surface of the non-woven fabric after the melt-blown treatment; during melt-blowing, the polymer melt in the melt-blowing die head includes the following components in parts by weight: 6.5 parts of polypropylene fiber and 2.5 parts of ES bonding fiber, the melt flow index of the polymer melt is 105 g / 10 min, the temperature of the melt-blowing die head is 200°C, the air flow injection angle in the melt-blowing die head is 37°, the pressure of the hot air flow in the melt-blowing die head is 0.14 MPa, the polymer melt extrusion amount is 0.3 g / hole / min, and hot rolling treatment is performed after melt-blowing; The double rollers in step S2 are configured into two groups, namely the first double roller and the second double roller, and a pre-drying zone is provided between the first double roller and the second double roller; the non-woven fabric base layer soaked in the modified slurry passes through the first double roller, the pre-drying zone, the second double roller, and the drying zone in turn, and the modified slurry in the non-woven fabric after passing through the pre-drying zone reaches the basic hardening stage, and then enters the second double roller, and finally reaches the complete hardening stage in the drying zone. Among them, the roller surface corresponding to the lower side of the non-woven fabric in the second double roller is provided with spherical bosses distributed in an array, and the lower surface of the non-woven fabric is formed with spherical concave holes distributed in an array on the lower surface after passing through the second double roller, and the ratio of the depth of the spherical concave holes to the total thickness of the non-woven fabric after the modification treatment in step S2 is 0.25-0.35; after being extruded by two groups of double rollers, a modified non-woven fabric with a gram weight of 170g / ㎡ is formed; in step S3, the total gram weight of the modified non-woven fabric finally obtained is 190g / ㎡, and the total thickness is 0.4mm.

[0029] In the above seven embodiments: the adhesive is water-based acrylic resin, the coupling agent is silane coupling agent (kh550), the dispersant is ammonium salt dispersant (for example: polyacrylate ammonium salt dispersant), and the defoamer is mineral oil defoamer (for example: polyether modified silicone oil defoamer); the particle size of calcium carbonate powder is 8-12μm. The above adhesive, coupling agent, dispersant, defoamer and various other raw materials involved in the above embodiments are directly purchased.

[0030] The modified nonwoven fabric obtained by the above embodiment has better overall hardness and wrinkle resistance than ordinary nonwoven fabrics, and at the same time, its ductility, light transmittance and water absorption are reduced, so its dimensional stability and covering power are improved. When it is compounded with a plate by water-based environmentally friendly glue, the glue cannot penetrate the modified nonwoven fabric; the base color coating is white and smooth, which is very suitable for inkjet printing; the modified nonwoven fabric has toughness, can be rolled up, can be bent at right angles, and is more convenient to process and transport. This modified nonwoven fabric does not contain formaldehyde itself, and is very environmentally friendly to use. In addition, the modified nonwoven fabric contains bamboo charcoal fibers. When compounded with a plate, the bamboo charcoal fibers can absorb the volatilized formaldehyde in the plate, thereby improving the environmental protection level of the plate.

[0031] In Examples 2-7, nano titanium dioxide and precipitated barium sulfate powder are used in the base color slurry. The difference in particle size between the two particles is utilized to make the surface roughness of the final base color coating greater than the roughness of the nano titanium dioxide used alone in Example 1. This roughness can increase the surface area of ​​inkjet printing, improve the adhesion performance of ink and base color coating, and make the inkjet printed pattern clearer and the color better.

[0032] In Examples 5-7, a meltblown layer is compounded on the surface of the non-woven fabric, and the porosity of the upper and lower surfaces of the compounded non-woven fabric is different. The different porosities result in different amounts of slurry absorbed after entering the modified slurry. The non-woven fabric has a high content of modified slurry, high hardness, high flatness, and stronger hiding power. After preparing a base color coating on the surface, the inkjet printing effect is better; while the meltblown layer has a low content of modified slurry, good toughness, and relatively high water absorption. The lower surface of the meltblown layer is compounded with the sheet through a water-based environmentally friendly glue, and the glue can better penetrate into the meltblown layer but cannot penetrate the non-woven fabric layer. While improving the composite strength of the meltblown layer and the sheet, it can effectively prevent the glue from penetrating the non-woven fabric; and the meltblown layer made of polypropylene fiber has a better sound insulation effect, which can improve the sound insulation effect of the sheet after being compounded with the sheet.

[0033] In Example 7, a treatment method of primary extrusion, pre-drying, secondary extrusion, and drying is adopted to eliminate the internal stress of the modified slurry during the hardening process and prevent the modified non-woven fabric from cracking. At the same time, a secondary rolling is performed in the basic hardening stage to make the surface of the non-woven fabric smoother, which is conducive to the preparation of a smoother base color coating. During the second double-roll extrusion, spherical concave holes are formed on the lower side of the modified non-woven fabric. The spherical concave holes can enhance the bonding surface area of ​​the modified non-woven fabric and the plate when they are compounded with glue, thereby improving the bonding strength and further improving the sound insulation effect.

[0034] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by up, down, left, right, inside, outside, one end, the other end, etc. are based on the orientations or positional relationships shown, and are only for the purpose of more clearly describing the technical solution of the present invention, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific orientation, and cannot be understood as a limitation of the present invention.

[0035] Although specific embodiments of the present invention are described in detail herein, they are provided for the purpose of explanation only and should not be considered to limit the scope of the present invention. Various substitutions, changes and modifications may be conceived without departing from the spirit and scope of the present invention.

Claims

1. A process for preparing a modified nonwoven fabric that is convenient for inkjet printing, characterized in that: The following steps are involved: S1. Preparing a nonwoven fabric: preparing fibers according to the following weight parts: 4-7 parts of wood pulp fiber, 5-12 parts of resin fiber, 3-5 parts of bamboo charcoal fiber, and 2-3 parts of viscose fiber, and mixing, opening, carding, spunlacing or needle-punching the above fibers to form a nonwoven fabric; S2, non-woven fabric modification treatment: the non-woven fabric is immersed in the modified slurry so that the modified slurry fills the gaps in the non-woven fabric, and then it is subjected to double-roll extrusion treatment and then enters the drying area for drying to form the modified non-woven fabric; The modified slurry comprises the following components in parts by weight: 5-10 parts of calcium carbonate powder, 20-32 parts of adhesive, 0.5-2.4 parts of coupling agent, and 0.5-1.5 parts of dispersant; S3. Prepare a base color coating: Roll-coat the base color slurry on the upper surface of the modified non-woven fabric and scrape it flat. After the base color slurry dries, a base color coating that is convenient for inkjet printing is formed; the base color slurry includes the following weight components: 5-12 parts of nano titanium dioxide, 20-28 parts of adhesive, 0.6-1.35 parts of coupling agent, and 0.3-0.5 parts of dispersant.

2. The process for preparing a modified nonwoven fabric that is convenient for inkjet printing according to claim 1, characterized in that: The fibers in step S1 also contain 2-4 parts by weight of polyester fibers.

3. The process for preparing a modified nonwoven fabric that is convenient for inkjet printing according to claim 1, characterized in that: The lower surface of the non-woven fabric obtained in step S1 is melt-blown to form a melt-blown layer on the lower surface of the non-woven fabric after the melt-blown treatment; During melt blowing, the polymer melt in the melt blowing die head includes the following components in parts by weight: 5-8 parts of polypropylene fiber and 2-3 parts of ES bonding fiber. The melt flow index of the polymer melt is 90-120 g / 10 min. The temperature of the melt blowing die head is 195-205°C. The air flow injection angle in the melt blowing die head is 35-40°. The pressure of the hot air flow in the melt blowing die head is 0.1-0.18 MPa, and the polymer melt extrusion amount is 0.2-0.4 g / hole / min.

4. The process for preparing a modified nonwoven fabric that is convenient for inkjet printing according to claim 3, characterized in that: The nonwoven fabric prepared in step S1 has a gram weight of 60-150 g / ㎡, the gram weight of the meltblown layer is 30-50 g / ㎡, and the total gram weight of the nonwoven fabric after meltblowing is 90-200 g / ㎡; hot rolling treatment is performed after meltblowing treatment.

5. A process for preparing a modified nonwoven fabric that is convenient for inkjet printing according to claim 1, 3 or 4, characterized in that: The modified pulp in step S2 also contains 5-20 parts by weight of bamboo pulp fibers.

6. The process for preparing a modified nonwoven fabric that is convenient for inkjet printing according to claim 5, characterized in that: The double rollers in step S2 are configured into two groups, namely a first double roller and a second double roller, and a pre-drying area is provided between the first double roller and the second double roller; The non-woven fabric base layer soaked in the modified slurry passes through the first double roller, pre-drying area, second double roller and drying area in sequence. After passing through the pre-drying area, the modified slurry in the non-woven fabric reaches the basic hardening stage, and then enters the second double roller, and finally reaches the complete hardening stage in the drying area.

7. The process for preparing a modified nonwoven fabric convenient for inkjet printing according to claim 6, characterized in that: The weight gain of the nonwoven fabric after the modification treatment in step S2 is 25-45 g / ㎡.

8. The process for preparing a modified nonwoven fabric that is convenient for inkjet printing according to claim 6, characterized in that: The roller surface of the second double roller corresponding to the lower side of the non-woven fabric is provided with spherical bosses distributed in an array, and spherical concave holes distributed in an array are formed on the lower surface of the non-woven fabric after passing through the second double roller.

9. The process for preparing a composite decorative fabric according to claim 8, characterized in that: The ratio of the depth of the spherical concave holes to the total thickness of the non-woven fabric after the modification treatment in step S2 is 0.25-0.

35.

10. The process for preparing a composite decorative fabric according to claim 1, characterized in that: In step S3, the base color slurry includes the following components in parts by weight: 2-5 parts of precipitated barium sulfate powder and 0.15-0.35 parts of defoaming agent; The particle size of the nano titanium dioxide is 10-50 nm, and the particle size of the precipitated barium sulfate powder is 200-400 nm.

Citation Information

Patent Citations

  • Industrial Thang-ga cloth and preparation method thereof

    CN111074636A

  • Preparation process of non-woven fabric capable of replacing natural veneer

    CN113619233A

Cited By

  • High-barrier antibacterial and mildew-proof composite decorative plate and preparation process thereof

    CN122684118A