Decarburization reconstruction method of lithium iron phosphate battery positive electrode material

Through the crushing, primary processing, reprocessing and calcining steps, combined with metal compounds such as lithium bicarbonate and epoxy resin, the problems of fluorine element influence and performance limitations of carbon source adhesives in the prior art are solved, and efficient defluorination is achieved and decarbonization improves the capacitance and conductivity of lithium iron phosphate batteries.

CN118908172AInactive Publication Date: 2024-11-08ANHUI NANDU HUABO NEW MATERIAL TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410967021.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing decarbonization and reconstruction method of lithium iron phosphate battery positive electrode material ignores the impact of fluorine element on battery performance, resulting in side reactions and passivation film formation, reducing the reversible capacity of the battery, and the carbon removal process is complicated and lacks effective utilization. There are many types of instruments, and maintenance is difficult to concentrate. The performance of carbon source adhesives limits the improvement of battery performance.

Method used

Using a step that includes crushing, primary processing, reprocessing, calcining and secondary calcining, defluorination of metal compound lithium bicarbonate, use iron to catalyze carbon reaction, select epoxy resins, etc. as carbon source adhesive, and unify instrument operation Process to promote the formation and structural repair of carbon cladding and improve battery performance.

Benefits of technology

It achieves purer defluorination and decarbonization, saves reagents, unified instrument operation reduces operating errors, improves battery performance and capacitance, simplifies maintenance and maintenance services, and improves the conductivity and stability of carbon cladding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908172A_ABST
    Figure CN118908172A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium iron phosphate battery positive electrode material decarbonization reconstruction method, and belongs to the technical field of positive electrode material regeneration. The method is used for solving the technical problems that in the prior art, a fluorocarbon removal method is single, the reaction process is complicated, and the capacitance of a regenerated lithium iron phosphate battery positive electrode material needs to be further improved, and comprises the following steps that the lithium iron phosphate positive electrode material is smashed and then treated, and pretreatment powder is obtained; after mixing with iron powder for further processing, adding a lithium source, an iron source and phosphoric acid, mixing and calcining to obtain calcined powder; mixing and calcining the calcined powder and a carbon source adhesive, mixing with a conductive agent and an adhesive, smearing in a base material, and processing to obtain the lithium iron phosphate battery positive electrode material. The method effectively solves the technical problems that the fluorocarbon removal method is single, the reaction process is complicated, and the capacitance of the regenerated lithium iron phosphate battery positive electrode material needs to be further improved in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cathode material regeneration, and in particular to a method for decarbonizing and regenerating cathode materials for lithium iron phosphate batteries.

[0003] Lithium iron phosphate batteries have stable performance, are safe and reliable, and are widely used in electric vehicles, energy storage systems, portable electronic devices and other fields. However, as the number of battery charge and discharge cycles increases, the battery's energy storage capacity continues to weaken. This characteristic indicates the arrival of the lithium iron phosphate battery's scrap period. In the next few years, there will be an explosive wave of lithium iron phosphate battery retirements.

[0004] During the discharge process of lithium iron phosphate batteries, electrolyte decomposition products may accumulate on the surface of the positive electrode material, and some carbon particles may be released from the negative electrode material, pass through the electrolyte, and then precipitate and redisperse on the positive electrode material. The unreasonable accumulation of carbon content will affect the discharge capacity of the lithium iron phosphate battery, so the process of decarbonization and reconstruction of lithium iron phosphate batteries has extremely high application prospects.

[0005] In the prior art, the decarbonization and regeneration methods of lithium iron phosphate cathode materials ignore the influence of fluorine on battery performance, such as the destruction of the lithium iron phosphate crystal structure, the side reactions caused and the formation of passivation film, which leads to a significant decrease in the reversible capacity of the battery; the carbon removal process is mostly direct calcination to generate carbon dioxide, the process is too direct and lacks effective utilization of carbon; too many types of reaction instruments are used in the regeneration process of lithium iron phosphate cathode materials, and it is difficult to achieve centralized technical support and maintenance services; the carbon source binder used in the carbon coating treatment of the final product lithium iron phosphate is mostly glucose, which limits the further improvement of battery performance and the capacitance of the cathode material. In view of the technical defects in this regard, a solution is now proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for decarbonizing and regenerating positive electrode materials of lithium iron phosphate batteries, which is used to solve the technical problems that the existing process of removing carbon and fluorine is single, the reaction process is complicated, and the capacitance of the regenerated positive electrode materials of lithium iron phosphate batteries needs to be further improved.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries, comprising the following steps:

[0009] S1. crushing and sieving the discarded positive electrode material of lithium iron phosphate batteries to obtain lithium iron phosphate powder;

[0010] S2, performing preliminary processing on the lithium iron phosphate powder to obtain pre-treated powder;

[0011] S3, reprocessing the pre-treated powder to obtain recycled powder;

[0012] S4, mixing the regenerated powder, lithium carbonate, iron oxide powder and phosphoric acid, and calcining them once to prepare a calcined powder;

[0013] S5, placing the calcined powder and the carbon source binder into a sintering furnace for secondary calcination and post-processing to obtain regenerated lithium iron phosphate;

[0014] S6. Mix the regenerated lithium iron phosphate, conductive agent and adhesive and apply them evenly to the base material to prepare the electrode material. After cutting, use cyclic voltammetry to measure the capacitance.

[0015] Furthermore, in step S2, the primary processing includes the following steps:

[0016] A1, iron phosphate slag powder and lithium bicarbonate powder are mixed to obtain lithium iron phosphate mixed powder;

[0017] A2, activating the lithium iron phosphate mixed powder to obtain activated powder;

[0018] A3. Add activated powder and water into a reactor and stir. Set the reactor temperature to 40-60°C. After reacting for 1-2 hours, lower the temperature of the reactor to room temperature, introduce CO2 and react for 2-3 hours. Filter with suction and dry the filter cake to obtain the pre-treated powder.

[0019] Furthermore, in step A1, the weight ratio of iron phosphate slag powder to lithium bicarbonate is 1:0.5; in step A2, the activation treatment includes: after transferring the activated powder precursor to a tubular heating furnace, introducing nitrogen protection, raising the tubular heating furnace to 400±5°C at a rate of 10°C / min, keeping warm for 6-8h, stopping heating, and cooling the tubular heating furnace to room temperature at a rate of 2°C / min to obtain a pre-treated powder; in step A3, the weight ratio of activated powder to water is 1:10, and the CO2 inlet flow rate is 10L / h.

[0020] Reaction principle:

[0021] C2F4+4LiHCO3+2O2→4LiF+H2O+3CO2

[0022] LiF+H2O→LiOH+HF

[0023] 2LiOH+CO2→Li2CO3+H2O

[0024] Further, in step S3, the reprocessing includes the following steps:

[0025] B1. The pre-treated powder is mixed with iron powder to obtain a mixed powder;

[0026] B2, regenerating the mixed powder to obtain a regenerated powder precursor;

[0027] B3. Magnetic separation is performed on the regenerated powder precursor to obtain the regenerated powder.

[0028] Furthermore, in step B1, the weight ratio of the pre-treated powder to the iron powder is 1:0.5; in step B2, the activation treatment includes: after the mixed powder is transferred to a tubular heating furnace, nitrogen is introduced for protection, the tubular heating furnace is raised to 1000±5°C at a rate of 10°C / min, and then a mixed gas is introduced and kept warm for 2-3 hours; after maintaining the temperature, the mixed gas is disconnected, oxygen is introduced, and after keeping warm for 1-2 hours, the tubular heating furnace is cooled to room temperature at a rate of 4°C / min to obtain a regenerated powder precursor, wherein the mixed gas is composed of carbon dioxide and nitrogen in a volume ratio of 1:2; in step B3, the regenerated powder is obtained after removing excess impurities using a magnetic separation method.

[0029] Reaction principle:

[0030] CO2+C→2CO

[0031] 4Fe+3O2→2Fe2O3

[0032] 3Fe+2O2→Fe3O4

[0033] The byproducts generated by the reaction are magnetic compared to iron oxide and can be easily removed using a magnet.

[0034] Furthermore, in step S4, a calcination treatment includes: after the mixed powder is transferred to a tubular heating furnace, nitrogen protection is introduced, the tubular heating furnace is heated to 800±5°C at a rate of 10°C / min, and then kept warm for 6-8h, and the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain calcined powder.

[0035] Reaction principle:

[0036] 2Fe2O3+3Li2CO3+6H3PO4→4LiFePO4+6CO2+3H2O

[0037] Further, in step S5, the carbon source binder is composed of epoxy resin, phenolic resin, benzene glycol, polypropylene glycol, diphenylamine and carbon black in a weight ratio of 5:1:0.3:0.5:0.2:3; the weight ratio of the calcined powder to the carbon source binder is 1:0.05-0.1; the post-processing operation includes: grinding the lithium iron phosphate agglomerate with a ball mill to obtain D50=10±0.5nm and a compaction density of 1.5±0.1g / cm 3 Regenerated lithium iron phosphate.

[0038] Further, in step S5, the secondary calcination treatment includes: after the mixed powder is transferred to a tubular heating furnace, nitrogen protection is introduced, the tubular heating furnace is heated to 400±5°C at a rate of 10°C / min, and the nitrogen flow rate is increased to 0.5m 3 Water vapor is introduced into the tubular heating furnace at a flow rate of 10°C / min to 900±10°C, and the temperature is kept at this temperature for 6-10h. The heating is stopped, and the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain large-particle lithium iron phosphate agglomerates.

[0039] Furthermore, in step S5, the selected conductive agent is carbon fiber, the adhesive is polytetrafluoroethylene, the weight ratio of lithium iron phosphate, carbon fiber and polytetrafluoroethylene is 7:2:1, and the matrix material is aluminum foil.

[0040] The present invention has the following beneficial effects:

[0041] 1. In the decarbonization and regeneration process of the positive electrode material of the lithium iron phosphate battery of the present invention, the metal compound lithium bicarbonate is used in the defluorination process, which can react with tetrafluoroethylene in the lithium iron phosphate battery to generate lithium fluoride. No impurity metal ions are introduced in the process, so that the final product is purer; the intermediate product lithium fluoride is reacted with water to generate lithium hydroxide, and then carbon dioxide is introduced to generate lithium carbonate. The product is consistent with the final selected lithium source, saving reagents and achieving higher benefits; in the decarbonization process, iron is used as a catalyst to catalyze the reaction of carbon dioxide and carbon powder to generate carbon monoxide. After the reaction is completed, oxygen can be directly introduced without cooling, so that the iron powder reacts with oxygen to generate iron oxide, saving energy, and the unreacted iron powder and the by-product ferroferric oxide can also be extracted by magnetic separation. The iron oxide retained in the system also overlaps with the final iron source, further saving reagents.

[0042] 2. In the decarbonization and regeneration process of the positive electrode material of lithium iron phosphate battery of the present invention, the chemical methods used in the defluorination, decarbonization and carbon coating processes are all calcination, and the instruments are consistent; the unified instruments can bring standardized operation procedures and data processing methods, which are beneficial to quality control and quality assurance. At the same time, operators can more easily become familiar with and master the unified operation procedures, thereby reducing the possibility of operating errors, and can also more easily realize the centralization of technical support and maintenance services; large-scale procurement of the same type of instruments may lead to a reduction in procurement costs and maintenance costs. At the same time, maintenance and training for the same type of instruments is also more convenient and economical.

[0043] 3. In the decarbonization and regeneration process of the positive electrode material of the lithium iron phosphate battery of the present invention, when the lithium iron phosphate powder with carbon powder removed and the carbon source binder are co-calcined to achieve the coating effect, epoxy resin is selected as the basic carbon source, phenolic resin is used as an additional binder, and hydroquinone is used as an antioxidant to play multiple roles such as cross-linking, anti-oxidation, stabilization and toughening, which is helpful to improve the performance and stability of the binder; polypropylene glycol is used as a flow regulator to improve the rheological properties of the carbon source binder, making it easier to flow and fill in the processing process, which is beneficial to improve the compactness of the product; diphenylamine is used as a curing agent, which mainly plays a role in catalysis, improving wear resistance and The effects of improving corrosion resistance and performance stability are helpful to improve the performance and reliability of the adhesive; carbon black, as a reinforcing agent and filler, mainly plays the role of reinforcing fillers, improving conductivity, improving wear resistance, improving thermal stability and improving color appearance, which helps to improve the performance and application range of the adhesive; the water vapor introduced during the calcination process can promote the repair of defects on the surface of the carbon coating at high temperature, and improve its structural integrity and stability; it can optimize the pore structure of the carbon coating, increase the specific surface area and pore distribution of the material, and enhance the electron transmission performance inside the carbon coating, thereby improving the conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0045] Figure 1 The present invention is a flowchart of the method for decarbonization and regeneration of positive electrode materials for lithium iron phosphate batteries. DETAILED DESCRIPTION

[0046] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] This embodiment provides a method for decarbonizing and regenerating a positive electrode material of a lithium iron phosphate battery, comprising the following steps:

[0049] S1. Preparation of lithium iron phosphate powder

[0050] The iron phosphate slag is added into a pulverizer and crushed, and passed through a 16-mesh sieve to obtain lithium iron phosphate powder.

[0051] S2. Preparation of pre-treated powder

[0052] The iron phosphate slag powder and the lithium bicarbonate powder are mixed in a weight ratio of 1:0.5 to obtain a mixed lithium iron phosphate powder;

[0053] After the mixed lithium iron phosphate powder is transferred to a tubular heating furnace, nitrogen is introduced for protection, the tubular heating furnace is heated to 400°C at a rate of 10°C / min, and the temperature is kept for 7 hours. The tubular heating furnace is cooled to room temperature at a rate of 2°C / min, and the material is discharged to obtain an activated powder;

[0054] The activated powder and water were added into a stirring tank at a weight ratio of 1:10 and stirred. The temperature of the stirring tank was raised to 50°C and reacted for 1.5 hours. The temperature was lowered to room temperature. CO2 was introduced from the bottom of the stirring tank at a flow rate of 10 L / h and reacted for 2 hours. The mixture was filtered and the filter cake was dried to obtain the pre-treated powder.

[0055] S3. Pre-treated powder is reprocessed to prepare recycled powder

[0056] The pre-treatment powder and the iron powder are mixed in a weight ratio of 1:0.5 to obtain a mixed pre-treatment powder;

[0057] The mixed powder was transferred to a nitrogen-protected tubular heating furnace, and nitrogen protection was introduced. The tubular heating furnace was raised to 995°C at a rate of 10°C / min, and the mixed gas was introduced into the tubular heating furnace, and the temperature was kept for 2 hours; oxygen was introduced into the tubular heating furnace, and the temperature was kept for 1 hour, and the tubular heating furnace was cooled to room temperature at a rate of 4°C / min to obtain a regenerated powder precursor, wherein the mixed gas was carbon dioxide and nitrogen in a volume ratio of 1:2;

[0058] The regenerated powder precursor is adsorbed by magnetic separation to remove the remaining iron powder and ferroferric oxide to obtain the regenerated powder.

[0059] S4, primary calcination

[0060] After measuring the molar ratio of lithium, iron and phosphorus in the regenerated powder using an X-ray fluorescence spectrometer, a calculated amount of lithium carbonate, iron oxide powder and phosphoric acid mixed powder was added so that the molar ratio of lithium, iron and phosphorus in the mixed regenerated powder was 7.1569:7.1568:7.1567;

[0061] The mixed powder was transferred to a tubular heating furnace and nitrogen was introduced for protection. The temperature of the tubular heating furnace was increased to 795°C at a rate of 10°C / min and kept warm for 6 hours. The tubular heating furnace was cooled to room temperature at a rate of 2°C / min and discharged to obtain calcined powder.

[0062] S5. Secondary calcination

[0063] The epoxy resin, the phenolic resin, the benzene glycol, the polypropylene glycol, the diphenylamine and the carbon black are mixed in a weight ratio of 5:1:0.3:0.5:0.2:3 to obtain a carbon source adhesive;

[0064] The calcined powder and the carbon source binder were mixed at a weight ratio of 1:0.05, and the mixed powder was transferred to a tubular heating furnace, and nitrogen was introduced for protection. The tubular heating furnace was heated to 395°C at a rate of 10°C / min, and then heated at 0.5m 3 Water vapor is introduced into the tubular heating furnace at a flow rate of 10°C / min to 890°C, and the temperature is kept at this temperature for 6 hours. The heating is stopped, and the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain large-particle lithium iron phosphate aggregates.

[0065] The lithium iron phosphate agglomerates were crushed by ball milling to obtain D50 = 9.6 nm and a compacted density of 1.52 g / cm 3 Regenerated lithium iron phosphate.

[0066] S6. Preparation of electrode materials

[0067] The regenerated lithium iron phosphate, the conductive agent carbon fiber and the adhesive polytetrafluoroethylene are mixed in a weight ratio of 7:2:1, and evenly applied to the base material to obtain a prefabricated electrode sheet, wherein the base material is aluminum foil;

[0068] After the prefabricated electrode sheet is placed in a vacuum oven for drying, the prefabricated electrode sheet is placed in a tubular heating furnace, nitrogen is introduced for protection, the temperature is raised to 250°C at a rate of 10°C / min, and after keeping the temperature for 2 hours, the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain an electrode material;

[0069] Example 2

[0070] This embodiment provides a method for decarbonizing and regenerating a positive electrode material of a lithium iron phosphate battery, comprising the following steps:

[0071] S1. Preparation of lithium iron phosphate powder

[0072] The iron phosphate slag is added into a pulverizer and crushed, and passed through a 16-mesh sieve to obtain lithium iron phosphate powder.

[0073] S2. Preparation of pre-treated powder

[0074] The iron phosphate slag powder and the lithium bicarbonate powder are mixed in a ratio of 1:0.5 to obtain a mixed lithium iron phosphate powder;

[0075] After the mixed lithium iron phosphate powder is transferred to a tubular heating furnace, nitrogen is introduced for protection, the tubular heating furnace is heated to 395°C at a rate of 10°C / min, and then kept warm for 6 hours. The tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain an activated powder;

[0076] The activated powder and water were added into a stirring kettle at a weight ratio of 1:10 and stirred. The temperature of the stirring kettle was raised to 40°C, reacted for 1 hour, then lowered to room temperature, CO2 was introduced into the bottom of the reactor at a flow rate of 10 L / h, reacted for 2 hours, filtered, and the filter cake was dried to obtain the pre-treated powder.

[0077] S3. Pre-treated powder is reprocessed to prepare recycled powder

[0078] The pre-treatment powder and the iron powder are mixed in a weight ratio of 1:0.5 to obtain a mixed pre-treatment powder;

[0079] The mixed powder was transferred to a tubular heating furnace protected by nitrogen, and nitrogen was introduced for protection. The temperature of the tubular heating furnace was raised to 1000°C at a rate of 10°C / min, and the mixed gas was introduced into the tubular heating furnace for insulation treatment for 2 hours; oxygen was introduced into the tubular heating furnace for insulation treatment for 1.5 hours, and the tubular heating furnace was cooled to room temperature at a rate of 4°C / min to obtain a regenerated powder precursor, wherein the mixed gas was composed of carbon dioxide and nitrogen in a volume ratio of 1:2;

[0080] The regenerated powder precursor is adsorbed by magnetic separation to remove the remaining iron powder and ferroferric oxide to obtain the regenerated powder.

[0081] S4, primary calcination

[0082] After measuring the molar ratio of lithium, iron and phosphorus in the regenerated powder using an X-ray fluorescence spectrometer, a calculated amount of lithium carbonate, iron oxide powder and phosphoric acid mixed powder was added so that the molar ratio of lithium and iron / phosphorus in the mixed regenerated powder was 6.1543:6.1542:6.1543;

[0083] The mixed powder was transferred to a tubular heating furnace and nitrogen was introduced for protection. The temperature of the tubular heating furnace was increased to 800°C at a rate of 10°C / min and kept warm for 7 hours. The tubular heating furnace was cooled to room temperature at a rate of 2°C / min and the material was discharged to obtain calcined powder.

[0084] S5. Secondary calcination

[0085] The epoxy resin, the phenolic resin, the benzene glycol, the polypropylene glycol, the diphenylamine and the carbon black are mixed in a weight ratio of 5:1:0.3:0.5:0.2:3 to obtain a carbon source adhesive;

[0086] The calcined powder was mixed with the carbon source binder at a weight ratio of 1:0.50, and the mixed powder was transferred to a tubular heating furnace. Nitrogen was introduced for protection. The tubular heating furnace was heated to 400°C at a rate of 10°C / min and then heated at 0.5m / min. 3Water vapor is introduced into the tubular heating furnace at a flow rate of 10°C / min to 900°C, and the temperature is kept at this temperature for 7 hours. The heating is stopped, and the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain large-particle lithium iron phosphate agglomerates.

[0087] The lithium iron phosphate aggregates were crushed by ball milling to obtain D50 = 10.1 nm and a compacted density of 1.51 g / cm 3 Regenerated lithium iron phosphate.

[0088] S6. Preparation of electrode materials

[0089] The regenerated lithium iron phosphate, the conductive agent carbon fiber and the adhesive polytetrafluoroethylene are mixed in a weight ratio of 7:2:1, and evenly applied to the base material to obtain a prefabricated electrode sheet, wherein the base material is aluminum foil;

[0090] After the prefabricated electrode sheet was placed in a vacuum oven for drying, it was placed in a tubular heating furnace, nitrogen was introduced for protection, the temperature was raised to 250°C at a rate of 10°C / min, and after keeping warm for 2h, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min to obtain the electrode material.

[0091] Example 3

[0092] This embodiment provides a method for decarbonizing and regenerating a positive electrode material of a lithium iron phosphate battery, comprising the following steps:

[0093] S1. Preparation of lithium iron phosphate powder

[0094] The iron phosphate slag is added into a pulverizer and crushed, and passed through a 16-mesh sieve to obtain lithium iron phosphate powder.

[0095] S2. Preparation of pre-treated powder

[0096] The iron phosphate slag powder and the lithium bicarbonate powder are mixed in a weight ratio of 1:0.5 to obtain a mixed lithium iron phosphate powder;

[0097] After the mixed lithium iron phosphate powder is transferred to a tubular heating furnace, nitrogen is introduced for protection, the tubular heating furnace is heated to 405°C at a rate of 10°C / min, and the temperature is kept for 8 hours. The tubular heating furnace is cooled to room temperature at a rate of 2°C / min, and the material is discharged to obtain an activated powder;

[0098] The activated powder and water were added into a stirring tank at a weight ratio of 1:10 and stirred. The temperature of the stirring tank was raised to 60°C, reacted for 2 hours, then lowered to room temperature, and CO2 was introduced from the bottom of the stirring tank at a flow rate of 10 L / h. The reaction was continued for 3 hours, and the filter cake was dried to obtain the pre-treated powder.

[0099] S3. Pre-treated powder is reprocessed to prepare recycled powder

[0100] The pre-treatment powder and the iron powder are mixed in a weight ratio of 1:0.5 to obtain a mixed pre-treatment powder;

[0101] The mixed powder was transferred to a nitrogen-protected tubular heating furnace, and nitrogen protection was introduced. The tubular heating furnace was raised to 1005°C at a rate of 10°C / min, and the mixed gas was introduced into the tubular heating furnace, and the temperature was kept for 2 hours; oxygen was introduced into the tubular heating furnace, and the temperature was kept for 1 hour, and the tubular heating furnace was cooled to room temperature at a rate of 4°C / min to obtain a regenerated powder precursor, wherein the mixed gas was carbon dioxide and nitrogen in a volume ratio of 1:2;

[0102] The regenerated powder precursor is adsorbed by magnetic separation to remove the remaining iron powder and ferroferric oxide to obtain the regenerated powder.

[0103] S4. Primary calcination

[0104] After measuring the molar ratio of lithium, iron and phosphorus in the regenerated powder using an X-ray fluorescence spectrometer, a calculated amount of lithium carbonate, iron oxide powder and phosphoric acid mixed powder was added so that the molar ratio of lithium and iron / phosphorus in the mixed regenerated powder was 7.5641:7.5642:7.5641;

[0105] The mixed powder was transferred to a tubular heating furnace and nitrogen was introduced for protection. The temperature of the tubular heating furnace was increased to 805°C at a rate of 10°C / min and kept warm for 6 hours. The tubular heating furnace was cooled to room temperature at a rate of 2°C / min and discharged to obtain calcined powder.

[0106] S5, secondary calcination: epoxy resin, phenolic resin, benzene glycol, polypropylene glycol, diphenylamine and carbon black are mixed in a weight ratio of 5:1:0.3:0.5:0.2:3 to obtain a carbon source adhesive;

[0107] The calcined powder and the carbon source binder were mixed at a weight ratio of 1:0.05, and the mixed powder was transferred to a tubular heating furnace, and nitrogen was introduced for protection. The tubular heating furnace was heated to 405°C at a rate of 10°C / min, and then heated at 0.5m 3 Water vapor is introduced into the tubular heating furnace at a flow rate of 10°C / min to 910°C, and the temperature is kept at this temperature for 6 hours. The heating is stopped, and the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain large-particle lithium iron phosphate aggregates.

[0108] The lithium iron phosphate aggregates were crushed by ball milling to obtain D50 = 9.9 nm and a compacted density of 1.48 g / cm 3 Regenerated lithium iron phosphate.

[0109] S6. Preparation of electrode materials

[0110] The regenerated lithium iron phosphate, the conductive agent carbon fiber and the adhesive polytetrafluoroethylene are mixed in a weight ratio of 7:2:1, and evenly applied to the base material to obtain a prefabricated electrode sheet, wherein the base material is aluminum foil;

[0111] After the prefabricated electrode sheet was placed in a vacuum oven for drying, it was placed in a tubular heating furnace, nitrogen was introduced for protection, the temperature was raised to 250°C at a rate of 10°C / min, and after keeping warm for 2h, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min to obtain the electrode material.

[0112] Comparative Example 1

[0113] Compared with Example 3, step S5 of this comparative example is: after mixing the calcined powder and glucose at a weight ratio of 1:0.05, the mixed powder is transferred to a tubular heating furnace, nitrogen is introduced for protection, the tubular heating furnace is heated to 405°C at a rate of 10°C / min, and then heated at 0.5m 3 Water vapor is introduced into the tubular heating furnace at a flow rate of 10°C / min to 910°C, and the temperature is kept at this temperature for 6 hours. The heating is stopped, and the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain large-particle lithium iron phosphate agglomerates.

[0114] Comparative Example 2

[0115] Compared with Example 3, step S5 in this comparative example is:

[0116] The epoxy resin, the phenolic resin, the benzene glycol, the polypropylene glycol, the diphenylamine and the carbon black are mixed in a weight ratio of 5:1:0.3:0.5:0.2:3 to obtain a carbon source adhesive;

[0117] The calcined powder and the carbon source binder were mixed in a weight ratio of 1:0.05, and the mixed powder was transferred to a tubular heating furnace. Nitrogen was introduced for protection, and the tubular heating furnace was heated to 910°C at a rate of 10°C / min and kept warm for 6 hours. The heating was stopped, and the tubular heating furnace was cooled to room temperature at a rate of 2°C / min to obtain large-particle lithium iron phosphate agglomerates.

[0118] Performance Test:

[0119] The carbon content, fluorine content and electrical properties of the samples prepared in Examples 1-3 and Comparative Examples 1-2 were tested, wherein the carbon content of the samples was detected with reference to the standard YS / T 1028.4-2015 "Chemical Analysis Method for Lithium Iron Phosphate Part 4: Determination of Carbon Content by High-Frequency Combustion Infrared Absorption Method"; the fluorine content was detected with reference to the standard GB / T 40563-2021 "Fluoride Red Phosphor", and the electrical properties were tested with reference to the standard GB / T42161-2022 "Test Method for First Discharge Specific Capacity and First Charge and Discharge Efficiency of Lithium Iron Phosphate Electrochemical Performance Test". The test data results are shown in Tables 1-2.

[0120] Table 1. Content test data of samples before and after decarburization and fluorine

[0121]

[0122] Table 2. Capacitance test data of regenerated electrode materials

[0123]

[0124]

[0125] Data Analysis:

[0126] Analyzing the data in Table 1 above, in the method for decarbonization and regeneration of lithium iron phosphate positive electrode material, after defluorination treatment, the fluorine content of the product is less than 0.005%, and the defluorination rate reaches 90.0%; after decarbonization treatment, the carbon content of the product is less than 1.5%, and the decarbonization rate reaches 94.0%, which can indicate that the lithium iron phosphate material after defluorination by using lithium bicarbonate and iron powder can meet the use standard as a positive electrode material for lithium iron phosphate batteries; by comparing the data of Example 3 and Comparative Example 1 in Table 2 above, it is found that the epoxy resin, phenolic resin, benzene glycol, polypropylene glycol, diphenylamine and carbon black are in a weight ratio of 5:1:0.3:0.5: Compared with the traditional carbon source glucose, the special carbon source adhesive mixed in a ratio of 0.2:3 can more fully coat the lithium iron phosphate powder with carbon, thereby improving the capacitance of the electrode material and further improving the performance of the lithium iron phosphate battery; by comparing the data of Example 3 and Comparative Example 2 in Table 2 above, it is found that during the calcination of lithium iron phosphate and the carbon source adhesive, the introduction of water vapor can promote the repair of defects on the surface of the carbon coating layer at high temperature, thereby improving its structural integrity and stability; the pore structure of the carbon coating layer can be optimized, the specific surface area and pore distribution of the material can be increased, and the electron transport performance inside the carbon coating layer can be improved, thereby improving the conductive properties of the material.

[0127] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0128] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0129] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for decarbonizing and regenerating positive electrode materials of lithium iron phosphate batteries, characterized in that: The following steps are involved: S1. crushing and sieving the discarded positive electrode material of lithium iron phosphate batteries to obtain lithium iron phosphate powder; S2, performing preliminary processing on the lithium iron phosphate powder to obtain pre-treated powder; S3, reprocessing the pre-treated powder to obtain recycled powder; S4, mixing the regenerated powder, lithium carbonate, iron oxide powder and phosphoric acid, and calcining them once to prepare a calcined powder; S5, mixing the calcined powder and the carbon source binder, performing secondary calcination, and post-processing to obtain regenerated lithium iron phosphate; S6. Mix the regenerated lithium iron phosphate, conductive agent and adhesive and apply them evenly to the base material to prepare the electrode material.

2. A method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 1, characterized in that: In step S2, the primary processing includes the following steps: A1, mixing iron phosphate slag powder and lithium bicarbonate powder to obtain mixed lithium iron phosphate powder; A2, activating the mixed lithium iron phosphate powder to obtain activated powder; A3. Add activated powder and water into a reactor and stir. Set the reactor temperature to 40-60°C. React for 1-2 hours. Lower the reactor temperature to room temperature. Pass CO2 into the reactor and react for 2-3 hours. Filter with suction and dry the filter cake to obtain the pre-treated powder.

3. A method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 2, characterized in that: In step A1, the weight ratio of iron phosphate slag powder to lithium bicarbonate is 1:0.5; in step A2, the activation treatment includes: after transferring the activated powder precursor to a tubular heating furnace, introducing nitrogen protection, raising the tubular heating furnace to 400±5°C at a rate of 10°C / min, keeping warm for 6-8h, stopping heating, and cooling the tubular heating furnace to room temperature at a rate of 2°C / min to obtain a pre-treated powder; in step A3, the weight ratio of activated powder to water is 1:10, and the CO2 inlet flow rate is 10L / h.

4. The method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 1, characterized in that: In step S3, the reprocessing includes the following steps: B1. The pre-treated powder is mixed with iron powder to obtain a mixed powder; B2, regenerating the mixed powder to obtain a regenerated powder precursor; B3. Magnetic separation is performed on the regenerated powder precursor to obtain the regenerated powder.

5. A method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 4, characterized in that: In step B1, the weight ratio of the pre-treated powder to the iron powder is 1:0.5; in step B2, the activation treatment includes: after the mixed powder is transferred to a tubular heating furnace, nitrogen is introduced for protection, the tubular heating furnace is raised to 1000±5°C at a rate of 10°C / min, and then a mixed gas is introduced for insulation for 2-3 hours; after maintaining the temperature, the mixed gas is disconnected, oxygen is introduced, and after insulation for 1-2 hours, the tubular heating furnace is cooled to room temperature at a rate of 4°C / min to obtain a regenerated powder precursor, wherein the mixed gas is composed of carbon dioxide and nitrogen in a volume ratio of 1:2; in step B3, the regenerated powder is obtained after removing excess impurities using a magnetic separation method.

6. The method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 1, characterized in that: In step S4, a calcination treatment includes: after the mixed powder is transferred to a tubular heating furnace, nitrogen protection is introduced, the tubular heating furnace is heated to 800±5°C at a rate of 10°C / min, and after keeping warm for 6-8 hours, the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain calcined powder.

7. The method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 1, characterized in that: In step S5, the carbon source binder is composed of epoxy resin, phenolic resin, benzene glycol, polypropylene glycol, diphenylamine and carbon black in a weight ratio of 5:1:0.3:0.5:0.2:3; the weight ratio of the calcined powder to the carbon source binder is 1:0.05-0.1; The post-processing operation includes: crushing the lithium iron phosphate agglomerates with a ball mill to obtain regenerated lithium iron phosphate, wherein the particle size of the regenerated lithium iron phosphate is D50=10±0.5nm and the compaction density is 1.5±0.1g / cm 3 .

8. The method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 1, characterized in that: In step S5, the secondary calcination treatment includes: after the mixed powder is transferred to the tubular heating furnace, nitrogen protection is introduced, the tubular heating furnace is heated to 400±5℃ at a rate of 10℃ / min, and the nitrogen flow rate is increased to 0.5m 3 Water vapor is introduced into the tubular heating furnace at a flow rate of 10°C / min to 900±10°C, and the temperature is kept at this temperature for 6-10h. After the heating is terminated, the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain large-particle lithium iron phosphate agglomerates.

9. The method for decarbonizing and regenerating anode materials of lithium iron phosphate batteries according to claim 1, characterized in that: In step S5, the selected conductive agent is carbon fiber, the adhesive is polytetrafluoroethylene and lithium iron phosphate, the weight ratio of carbon fiber to polytetrafluoroethylene is 7:2:1, and the matrix material is aluminum foil.