Method for preparing lignite-based phenolic carbon aerogel through cooperation of hot pressing and solvothermal and application of lignite-based phenolic carbon aerogel

Through the coordinated preparation method of hot pressing and solvent-heat, chlorine is used to prepare phenolic carbon aerogel with high photothermal conversion performance and adjustable pore structure, which solves the problem of large consumption of petroleum-based phenol in the preparation of carbon aerogel and improves solar power drive The water evaporation performance of the interface and realizes the efficient utilization of lignite resources.

CN118908181APending Publication Date: 2024-11-08ANHUI UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202411017873.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the preparation of carbon aerogel requires a large amount of petroleum-based phenol, and its pore structure is difficult to adjust, which affects its performance in water evaporation at the solar-driven interface, and lignite resources are not effectively utilized.

Method used

The method of hot pressing and solvothermal preparation is adopted to heat dissolute lignite, formic acid and organic solvents, and then add phenols, aldehydes and acids to perform solvothermal reactions. The lignite-based phenolic carbon aerogel is prepared by hot pressing melamine foam to achieve Adjustability of the pore structure.

Benefits of technology

Successfully replaced some petroleum-based phenol to prepare a phenolic carbon aerogel with high photothermal conversion performance and adjustable pore structure, which improved its performance in water evaporation at the solar-driven interface, reduced raw material costs, and increased lignite Utilization value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908181A_ABST
    Figure CN118908181A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing lignite-based phenolic carbon aerogel through cooperation of hot pressing and solvothermal and application of the lignite-based phenolic carbon aerogel, and belongs to the field of high-value utilization of low-rank coal. The preparation method comprises the following steps: thermally dissolving lignite to obtain a thermally-dissolved substance, and carrying out solvothermal reaction by taking melamine foam as a framework, the lignite thermally-dissolved substance and aldehydes as raw materials and acid as a catalyst to obtain phenolic aldehyde organic gel; and performing normal-pressure drying and carbonization to obtain the phenolic carbon aerogel. The lignite-based phenolic carbon aerogel with adjustable macroporous and microporous structures is respectively obtained by hot pressing of melamine foam and adjustment of solvothermal temperature, and the aerogel can be used for solar-driven interface water evaporation. According to the method, the phenolic carbon aerogel with the adjustable pore diameter is prepared by replacing phenols with the lignite hot melt, the cost of raw materials is reduced, the utilization value of lignite is improved, meanwhile, operation is easy, complex freeze drying and expensive templates are not needed, and the method has a good application prospect of solar-driven interface water evaporation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of high-value utilization of low-rank coal, and in particular to a method for preparing lignite-based phenolic carbon aerogel by synergistic hot pressing and solvent thermal reaction, and application of the aerogel in solar-driven interfacial water evaporation. Background Art

[0002] my country has abundant low-rank lignite resources, with a reserve of more than 130 billion tons. However, lignite has a low degree of metamorphism, high moisture content, low calorific value, and is easily weathered and self-ignited. The traditional energy utilization method based on combustion for heating is inefficient, highly polluting, and emits a large amount of CO2. Therefore, it is urgent to develop high-value and low-carbon utilization technologies for lignite.

[0003] At present, obtaining fresh water from seawater has become a focus of attention. At present, seawater desalination technology mainly includes multi-stage flash evaporation and reverse osmosis, but these methods have problems of high energy consumption, high investment or difficulty in scalability. In recent years, solar-driven interfacial water evaporation has attracted much attention due to its advantages such as high energy efficiency and zero carbon emissions. The key is to develop efficient photothermal materials. Carbon aerogels are widely used as photothermal materials for solar-driven interfacial water evaporation due to their advantages such as high porosity, good thermal insulation, and high light absorption. Among them, the preparation of phenolic carbon aerogels requires a large amount of phenol. The industrial production of phenol mainly adopts the isopropylbenzene method, and isopropylbenzene mainly comes from petrochemicals, resulting in a high price for phenol. Therefore, it is of great significance to find a substitute for petroleum-based phenol. In view of the structural characteristics of lignite rich in aromatic ring structure and phenolic hydroxyl groups, it is expected to partially replace petroleum-based phenol to prepare phenolic carbon aerogels. In addition, the pore structure has a great influence on the water management and thermal management of carbon aerogels, and the development of lignite-based phenolic carbon aerogels with adjustable pore structure is of great significance. Summary of the invention

[0004] The purpose of the present invention is to provide a method and application of hot pressing and solvent thermal synergistic preparation of lignite-based phenolic carbon aerogel, and to use cheap lignite to replace part of the petrochemical raw material phenol to prepare a method of phenolic carbon aerogel with high photothermal conversion performance and adjustable pore structure, so as to provide a new way for the high-value utilization of lignite and the pore size modulation of carbon aerogel. At the same time, the aerogel can be used in solar-driven interfacial water evaporation and achieve good results.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent heat synergistically comprises the following steps:

[0007] 1) adding lignite, formic acid and an organic solvent into an autoclave and performing thermal dissolution in a nitrogen atmosphere to obtain a lignite thermal dissolution;

[0008] 2) dissolving the lignite hot melt and phenols in an organic solvent to obtain a mixed solution;

[0009] 3) hot-pressing the melamine foam, and then placing it into the above solution, and then adding aldehydes and acids to carry out a solvent thermal reaction to obtain a lignite-based phenolic organic gel;

[0010] 4) washing the phenolic organic gel with ethanol, and then drying it under normal pressure to obtain a lignite-based phenolic organic aerogel;

[0011] 5) Carbonizing the phenolic organic aerogel to obtain lignite-based phenolic carbon aerogel.

[0012] Furthermore, the organic solvent in step (1) is one of methanol, ethanol, isopropanol, toluene or cyclohexane; and the ratio of lignite, formic acid and organic solvent is 0.5-5g:1-5mL:10-50mL.

[0013] Furthermore, the hot melt reaction temperature of step (1) is 250-350°C, and the reaction time is 1-8h.

[0014] Furthermore, the organic solvent in step (2) is one of methanol, ethanol, isopropanol, n-butanol and acetone; the phenol is one of phenol, o-cresol, m-cresol, p-cresol and resorcinol; and the mass ratio of the lignite hot melt to the phenol is 1:9-1:1.

[0015] Furthermore, in step (3), the aldehyde is one or two of formaldehyde, paraformaldehyde, and furfural; and the acid is one of hydrochloric acid, sulfuric acid, phosphoric acid, formic acid, and oxalic acid.

[0016] Furthermore, in step (3), the hot pressing temperature is 100-300°C, and the hot pressing time is 4-15 minutes.

[0017] Furthermore, in step (3), the solvent thermal reaction temperature is 80-160°C and the time is 6-36h.

[0018] Furthermore, the ratio of the phenols, aldehydes and acids in step (2) and step (3) is 0.80–1.44 g:1.5–5 mL:0.5–2 mL.

[0019] Furthermore, in step (5), the carbonization temperature is 400-900°C and the time is 1-8h.

[0020] It should be further explained that by hot pressing melamine foam and adjusting the thermal temperature of the solvent, lignite-based phenolic carbon aerogels with adjustable macropore and micropore structures can be obtained respectively, thereby achieving the effect of adjustable pore size.

[0021] Another object of the present invention is to provide an application of the lignite-based phenolic carbon aerogel obtained by the above preparation method in solar-driven interfacial water evaporation.

[0022] Beneficial effects of the present invention:

[0023] 1. The method of the present invention is simple and does not require complicated freeze-drying or expensive templates.

[0024] 2. The present invention utilizes lignite thermal solution rich in aromatic ring structure, phenolic hydroxyl group and alkyl side chain to replace phenols to prepare carbon aerogel, which not only has good photothermal performance but also has low density.

[0025] 3. The present invention uses hot-pressed melamine foam as a skeleton to prepare lignite-based phenolic carbon aerogel, which solves the problems of poor mechanical strength and insufficient water management ability of conventional phenolic carbon aerogel.

[0026] 4. The utilization mode mainly using lignite combustion for heating has low value and emits a large amount of CO2 and gaseous pollutants. The present invention uses lignite thermal melt to replace phenols to prepare phenolic carbon aerogel, which not only reduces the cost of raw materials, but also increases the utilization value of lignite. At the same time, it improves the solar-driven interfacial water evaporation performance of conventional phenolic carbon aerogel, and thus has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention will be further described below in conjunction with the accompanying drawings.

[0028] Figure 1 This is a real photo of the 50% carbon aerogel in Example 1 of the present invention.

[0029] Figure 2 Optical microscope photographs of 50% carbon aerogels in Examples 1-3 of the present invention: (ac) LPCA / 100-3, (df) LPCA / 120-3, (gi) LPCA / 140-3 and (jl) LPCA / 100-2.

[0030] Figure 3 1 is the stress-strain curve of the carbon aerogel in Example 1-2 of the present invention.

[0031] Figure 4 Graphs showing the saturated water content (a) and water transmission rate (b) of the carbon aerogels in Examples 1-5 of the present invention.

[0032] Figure 5 Graph showing the solar-driven water evaporation performance of the carbon aerogels in Examples 2, 3 and 5 of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Embodiment 1:

[0035] 2g of Zhaotong lignite, 3mL of formic acid and 30mL of ethanol were added to an autoclave, and the mixture was heated at 300℃ for 2h in a nitrogen atmosphere. The lignite hot melt was obtained after centrifugation and filtration. 0.8g of phenol and 0.8g of lignite hot melt (phenol substitution rate was 50%) were weighed and dissolved in 30mL of ethanol to obtain a mixed solution; melamine foam was placed in the above solution, and 5mL of formaldehyde and 1.5mL of hydrochloric acid were added, and the solvent thermal reaction was carried out at 120℃ for 12h to obtain a lignite-based phenolic organic gel; the phenolic organic gel was washed with ethanol until the washing liquid was colorless, and then dried at normal pressure to obtain a lignite-based phenolic organic aerogel (50% aerogel); the phenolic organic aerogel was carbonized at 500℃ for 2h to obtain a lignite-based phenolic carbon aerogel (LPCA / 120-3, Figure 1 and 2 ). Density is 0.042g / cm 3 , the pore structure is mainly composed of mesopores and macropores ( Figure 2 ). When the strain is 80%, the compressive strength is 0.43MPa ( Figure 3 ). Saturated water content is 19g·g -1 , water transmission rate is 0.091g·min -1 ( Figure 4 ). Under 1 times the sunlight, the water evaporation rate is 1.86 kg·m -2 h -1 , which is 4.0 times that of pure water.

[0036] Embodiment 2:

[0037] 2g of Zhaotong lignite, 3mL of formic acid and 30mL of ethanol were added to an autoclave, and the mixture was heated at 300℃ for 4h in a nitrogen atmosphere. The lignite hot melt was obtained after centrifugation and filtration. 0.8g of phenol and 0.8g of lignite hot melt (phenol substitution rate was 50%) were weighed and dissolved in 30mL of ethanol to obtain a mixed solution; melamine foam after hot pressing at 230℃ for 6min was placed in the above solution, and then 5mL of formaldehyde and 1.5mL of hydrochloric acid were added, and the solvent thermal reaction was carried out at 100℃ for 12h to obtain a lignite-based phenolic organic gel; the phenolic organic gel was washed with ethanol until the washing liquid was colorless, and then dried at normal pressure to obtain a lignite-based phenolic organic aerogel (50% aerogel); the phenolic organic aerogel was carbonized at 600℃ for 2h to obtain a lignite-based phenolic carbon aerogel (LPCA / 100-2). The density is 0.053g / cm 3 The macropore size is smaller than that of LPCA / 120-3, and the pore size of the phenolic resin accumulation is larger ( Figure 2 ). When the strain is 80%, the compressive strength is 2.20MPa ( Figure 3 ). The saturated water content is 17.6 g·g -1 , water transmission rate is 0.086g·min -1 ( Figure 4 ). Under 1 times the sunlight, the water evaporation rate is as high as 2.10 kg·m -2 h -1 ( Figure 5 ).

[0038] Embodiment 3:

[0039] 3g of Zhaotong lignite, 3mL of formic acid and 30mL of methanol were added to an autoclave, and heat-dissolved at 320℃ in a nitrogen atmosphere for 8h. The lignite heat solution was obtained after centrifugation and filtration. 0.8g of phenol and 0.8g of lignite heat solution (phenol substitution rate was 50%) were weighed and dissolved in 30mL of ethanol to obtain a mixed solution; melamine foam was placed in the above solution, and then 5mL of formaldehyde and 1.5mL of hydrochloric acid were added, and the solvent thermal reaction was carried out at 140℃ for 12h to obtain a lignite-based phenolic organic gel; the phenolic organic gel was washed with ethanol until the washing liquid was colorless, and then dried at normal pressure to obtain a lignite-based phenolic organic aerogel (50% aerogel); the phenolic organic aerogel was carbonized at 600℃ for 2h to obtain a lignite-based phenolic carbon aerogel (LPCA / 140-3). The density is 0.044g / cm 3 The macropore size is consistent with that of LPCA / 120-3, and the pore size of the phenolic resin accumulation is reduced ( Figure 2 ). The saturated water content is 18.6 g·g -1 , water transmission rate is 0.092g·min -1 ( Figure 4 ). Under 1 times the sunlight, the water evaporation rate is 1.84 kg·m- 2 h -1 ( Figure 5 ).

[0040] Embodiment 4:

[0041] 2g of Zhaotong lignite, 3mL of formic acid and 30mL of isopropanol were added to an autoclave, and the mixture was heated at 300℃ for 2h in a nitrogen atmosphere. The lignite hot melt was obtained after centrifugation and filtration. 0.8g of phenol and 0.8g of lignite hot melt (phenol substitution rate was 50%) were weighed and dissolved in 30mL of acetone to obtain a mixed solution; melamine foam after hot pressing at 230℃ for 8min was placed in the above solution, and then 5mL of formaldehyde and 1.5mL of hydrochloric acid were added, and the solvent thermal reaction was carried out at 120℃ for 16h to obtain a lignite-based phenolic organic gel; the above phenolic organic gel was washed with ethanol until the washing liquid was colorless, and then dried at normal pressure to obtain a lignite-based phenolic organic aerogel (50% aerogel); the above phenolic organic aerogel was carbonized at 500℃ for 2h to obtain a lignite-based phenolic carbon aerogel (LPCA / 120-1). The density is 0.063g / cm 3 The macropore size is smaller than that of LPCA / 120-3, and the pore size of the phenolic resin stacking pores does not change much. The saturated water content is 15.6g·g -1 , water transmission rate is 0.060g·min -1 ( Figure 4 ). Under 1 times the sunlight, the water evaporation rate is 2.00 kg·m -2 h -1 .

[0042] Embodiment 5:

[0043] 2g of Zhaotong lignite, 3mL of formic acid and 30mL of ethanol were added to an autoclave, and heat-dissolved at 280℃ for 2h in a nitrogen atmosphere. The lignite heat solution was obtained after centrifugation and filtration. Weigh 0.8g of phenol and 0.8g of lignite heat solution (phenol substitution rate is 50%), dissolve in 30mL of n-butanol to obtain a mixed solution; put the melamine foam after hot pressing at 230℃ for 6min into the above solution, and then add 5mL of formaldehyde and 1.5mL of hydrochloric acid, and perform solvent thermal reaction at 120℃ for 8h to obtain lignite-based phenolic organic gel; wash the above phenolic organic gel with ethanol until the washing liquid is colorless, and then dry it at normal pressure to obtain lignite-based phenolic organic aerogel (50% aerogel); carbonize the above phenolic organic aerogel at 500℃ for 2h to obtain lignite-based phenolic carbon aerogel (LPCA / 120-2). The density is 0.055g / cm 3 The macropore size is smaller than that of LPCA / 120-3, and the pore size of the phenolic resin stacking pores does not change much. The saturated water content is 17.6g·g -1 , water transmission rate is 0.083 g·min-1 ( Figure 4 ). Under 1 times the sunlight, the water evaporation rate is as high as 2.02kg·m -2 h -1 ( Figure 5 ).

[0044] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.

Claims

1. A method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergy, characterized in that: The following steps are involved: 1) adding lignite, formic acid and an organic solvent into an autoclave and performing thermal dissolution in a nitrogen atmosphere to obtain a lignite thermal dissolution; 2) dissolving the lignite hot melt and phenols in an organic solvent to obtain a mixed solution; 3) hot-pressing the melamine foam, and then placing it into the above solution, and then adding aldehydes and acids to carry out a solvent thermal reaction to obtain a lignite-based phenolic organic gel; 4) washing the phenolic organic gel with ethanol, and then drying it under normal pressure to obtain a lignite-based phenolic organic aerogel; 5) Carbonizing the phenolic organic aerogel to obtain lignite-based phenolic carbon aerogel.

2. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: The organic solvent in step (1) is one of methanol, ethanol, isopropanol, toluene or cyclohexane; the ratio of lignite, formic acid and organic solvent is 0.5-5g:1-5mL:10-50mL.

3. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: The hot melt reaction temperature of step (1) is 250-350°C and the reaction time is 1-8h.

4. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: The organic solvent in step (2) is one of methanol, ethanol, isopropanol, n-butanol and acetone; the phenol is one of phenol, o-cresol, m-cresol, p-cresol and resorcinol; and the mass ratio of the lignite hot melt to the phenol is 1:9-1:

1.

5. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: In step (3), the aldehyde is one or two of formaldehyde, paraformaldehyde and furfural; and the acid is one of hydrochloric acid, sulfuric acid, phosphoric acid, formic acid and oxalic acid.

6. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: In step (3), the hot pressing temperature is 100-300°C and the hot pressing time is 4-15 minutes.

7. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: In step (3), the solvent thermal reaction temperature is 80-160°C and the time is 6-36h.

8. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: The ratio of phenols, aldehydes and acids in step (2) and step (3) is 0.80–1.44 g:1.5–5 mL:0.5–2 mL.

9. The method for preparing lignite-based phenolic carbon aerogel by hot pressing and solvent thermal synergistically according to claim 1, characterized in that: The carbonization temperature of step (5) is 400-900°C and the time is 1-8h.

10. Use of lignite-based phenolic carbon aerogel prepared according to the method according to any one of claims 1 to 9 in solar-driven interfacial water evaporation.

Citation Information

Patent Citations

  • Lignite-based toughened phenolic foam and preparation method thereof

    CN112194875A

  • Brown coal residue-based porous carbon material as well as preparation method and application thereof

    CN115020121A

  • Preparation and application of coal tar-based phenolic carbon aerogel

    CN115259133A

  • Preparation method and application of ultrathin aerogel composite light thermal insulation material

    CN115725154A

  • Carbon foam / carbon aerogel / phase change material ternary complex and preparation method thereof

    CN117534466A

Cited By

  • Preparation method and application of phenolic oil-based phase separation phenolic aerogel

    CN119661794A