Method for preparing high-purity magnesium oxide by taking light calcined magnesium oxide as raw material

By lightly calcining magnesium oxide and amino acid hydrating agent assisted in hydration and acid leaching treatment, the problems of low purity and high cost of preparing high-purity magnesium oxide in low-grade magnesium ore are solved, and efficient and environmentally friendly resource utilization is achieved.

CN118908248APending Publication Date: 2024-11-08DALIAN MARITIME UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065217.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, when using low-grade magnesium ore to prepare high-purity magnesium oxide, the hydration method has low purity and high cost. The acid leaching method poses a risk of environmental pollution, making it difficult to effectively utilize low-grade magnesium resources.

Method used

Use light flammable magnesium oxide and amino acid hydrating agent to assist in hydration to form a suspension. High-purity magnesium hydroxide is obtained through calcium removal and silicon removal treatment, and magnesium sulfate is recovered through acid leaching and dissolution steps, and finally calcination is used to obtain high-purity magnesium oxide. .

Benefits of technology

It improves the hydration rate and purity of magnesium oxide, reduces production costs, reduces the risk of environmental pollution, and provides an efficient way to utilize low-grade magnesium resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908248A_ABST
    Figure CN118908248A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of magnesium oxide preparation and purification, in particular to a method for preparing high-purity magnesium oxide by taking light calcined magnesium oxide as a raw material. The method comprises the following steps: reacting light calcined magnesia serving as a raw material with water under the assistance of an amino acid hydrating agent to generate a suspension, standing, separating slurry and precipitate, performing calcium removal and silicon removal treatment on the slurry to obtain high-purity magnesium hydroxide, and further calcining to obtain high-purity magnesium oxide, magnesium sulfate is recovered from the precipitate through the steps of acid leaching, solventing-out and the like, and magnesium sulfate is calcined to obtain high-purity magnesium oxide. According to the method, purification of the light calcined magnesia is realized through combination of hydration and acid leaching, the utilization rate of magnesium ions is not reduced, meanwhile, the operation cost is reduced, the pollutant discharge amount is small, a new way is provided for comprehensive utilization and development of the light calcined magnesia, and the method is green and high in yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnesium oxide preparation and purification, and in particular to a method for preparing high-purity magnesium oxide by using light-burned magnesium oxide as a raw material. Background Art

[0002] Magnesium oxide is a commonly used inorganic chemical material with the advantages of large specific surface area, strong adsorption and high reaction activity. It is widely used in the treatment of industrial organic waste gases such as nitrogen oxides, sulfur oxides and carbon dioxide, industrial wastewater such as dyes, pesticides and heavy metal ions, and heavy metal pollution in soil. High-purity magnesium oxide has excellent alkali resistance, electrical insulation and light transmittance, small thermal expansion coefficient and low thermal conductivity. It is an indispensable refractory material in metallurgy, chemical industry and non-metallic industry, and can be used to prepare high-end functional materials required in aerospace, aviation, military, metallurgy and other fields.

[0003] my country is one of the countries with the richest magnesium resources in the world. At present, the proven reserves of magnesite are about 3 billion tons. The irrational development of mines in the early stage has caused serious waste of resources. The amount of high-quality magnesium resources has been decreasing, and low-grade magnesium resources cannot be directly used to produce high-value-added magnesium products. In particular, some tailings and crushed ores cannot be used and are idle or abandoned, resulting in a huge waste of resources. Therefore, considering the long-term interests, in order to make better use of resources, it is urgent to solve the problems of low utilization rate of magnesite resources and shortage of high-grade magnesite by efficiently developing and utilizing low-grade and low-grade mineral resources.

[0004] Lightly burned magnesium oxide is a magnesium oxide product obtained by calcining magnesite at 700-1000°C, and its magnesium oxide content is about 85%. At present, the methods for preparing high-purity magnesium oxide using lightly burned magnesium oxide mainly include: hydration method and acid leaching method. The hydration method uses lightly burned magnesium oxide to react with hydration to generate magnesium hydroxide, and calcines magnesium hydroxide to obtain magnesium oxide. This method has simple steps and low cost, but because the hydration method is greatly affected by the raw materials, and the magnesium hydroxide generated by hydration covers the surface of magnesium oxide, preventing further hydration, resulting in low hydration rate and low purity of the product, it is difficult to use in practice. CN103204641A discloses a hydration purification method for low-grade magnesite, which uses low-grade magnesite calcined, hydrated and then calcined to obtain magnesium oxide, with simple steps, but the purity of the magnesium oxide product is low. The acid leaching method uses acid to react with magnesium ore to generate a magnesium salt solution, and generates hydroxide by changing the solubility of the magnesium salt or adding alkaline substances, recovering magnesium ions in the magnesium salt solution, and obtaining high-purity magnesium oxide by calcination. The acid leaching method has a thorough reaction, high utilization rate of magnesium ions, and a short production process, but due to the acid treatment, its operating cost is high and the equipment requirements are high. CN108502906A discloses a method for preparing high-purity magnesium hydroxide by acid-dissolving light-burned powder. After acid dissolution, ammonia is used to precipitate magnesium, which has high production costs and great harm to the environment.

[0005] In summary, my country is facing the problem of the depletion of high-grade magnesium sources, the surge in industrial demand for high-grade magnesium sources and the increasing quality requirements. In contrast, low-grade magnesium sources are piled up in large quantities and cannot be effectively utilized. There are some problems with the method of using low-grade magnesium sources to produce high-grade magnesium sources. The hydration method has a simple process and low cost, but the hydration rate and purity of the product are low; the acid leaching method can obtain high-purity products, but the cost is high, the process is complicated, and there is a problem that chemical reagents may cause environmental pollution. Therefore, it is necessary to find a method that can not only improve the hydration rate and purity of the product, but also reduce costs and reduce the risk of environmental pollution. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a method for preparing high-purity magnesium oxide using light-burned magnesium oxide as a raw material. The light-burned magnesium oxide is hydrated with the aid of an amino acid hydrating agent to generate a suspension, and then the slurry and the precipitate are separated after standing, and the slurry is treated by decalcification and desiliconization to obtain high-purity magnesium hydroxide, which is further calcined to obtain high-purity magnesium oxide; the precipitate is recovered by acid leaching, dissolution and other steps to obtain magnesium sulfate, and the magnesium sulfate is calcined to obtain high-purity magnesium oxide.

[0007] In order to achieve the above object, the technical solution of the present invention is as follows:

[0008] The present invention provides a method for preparing high-purity magnesium oxide using light-burned magnesium oxide as a raw material, comprising the following steps:

[0009] (1) Hydration and stratification: The light-burned magnesium oxide powder and water react with each other with the aid of an amino acid hydrating agent. After the reaction is completed, the mixture is allowed to stand for separation to obtain a slurry and a precipitate. The slurry is filtered to obtain a filter cake 1 and a filtrate 1. The filtrate 1 is reused in the hydration and stratification stage.

[0010] (2) decalcification: the filter cake 1 obtained in step (1) is washed, magnesium chloride and water are added thereto to prepare a suspension 1, the suspension 1 is reacted under stirring conditions, and then filtered to obtain a filter cake 2 and a filtrate 2, and the filtrate 2 is reused in the decalcification stage;

[0011] (3) silicon removal: washing the filter cake 2 obtained in step (2), adding sodium hydroxide and water to prepare a suspension 2, reacting the suspension 2 under stirring, and then filtering to obtain a filter cake 3 and a filtrate 3, washing and drying the filter cake 3 to obtain high-purity magnesium hydroxide, and calcining the high-purity magnesium hydroxide to obtain high-purity magnesium oxide;

[0012] (4) Acid leaching to extract magnesium: adding the precipitate obtained in step (1) to a sulfuric acid solution, performing an acid leaching reaction under stirring conditions, and filtering to obtain a magnesium salt solution;

[0013] (5) dissolution crystallization: adding an organic solvent to the magnesium salt solution obtained in step (4), performing solid-liquid separation after crystallization is completed to obtain a crystallization mother liquor and magnesium sulfate crystals, distilling the crystallization mother liquor to recover the organic solvent, washing the magnesium sulfate crystals and calcining to obtain high-purity magnesium oxide and sulfur dioxide, and absorbing the sulfur dioxide with hydrogen peroxide and then recycling it to acid leaching magnesium.

[0014] In the above technical solution, further, in step (1), the liquid-to-solid ratio of water to light-burned magnesium oxide powder is 3:1-30:1; the standing time is 0.5-1h; the temperature of the hydration reaction is 50-90°C, and the hydration time is 2-6h.

[0015] In the above technical scheme, further, in step (1), the amino acid hydrating agent is one or more of glycine, alanine, glutamic acid, valine, threonine, leucine, isoleucine, serine, aspartic acid, lysine, and arginine; and the amount of the amino acid hydrating agent added is 0.1%-15% of the mass of the light-burned magnesium oxide.

[0016] In the above technical solution, further, in step (2), the amount of magnesium chloride added is 5%-10% of the mass of the filter cake 1; the solid content of the suspension 1 is 10%-20%; the reaction temperature is 25-50°C, the stirring speed is 100-200rpm, and the reaction time is 1-2h.

[0017] In the above technical solution, further, in step (3), the amount of sodium hydroxide added is 2%-15% of the mass of the filter cake 2; the solid content of the suspension 2 is 10%-20%; the reaction temperature is 25-50°C, the stirring speed is 100-200rpm, and the reaction time is 1-2h.

[0018] In the above technical solution, further, in step (3), the drying temperature is 90-100°C, and the drying time is 10-12h; the calcination temperature is 500-700°C, and the calcination time is 2-6h.

[0019] In the above technical scheme, further, in step (4), the liquid-solid ratio of the precipitate to the sulfuric acid solution is 10:1-20:1; the concentration of the sulfuric acid solution is 1-2 mol / L; the temperature of the acid leaching reaction is 50-90°C, the stirring speed is 100-400rpm, and the reaction time is 0.5-2h.

[0020] In the above technical solution, further, in step (5), the amount of organic solvent added is 10%-40% of the volume of the magnesium salt solution; the calcination temperature is 1200-1500° C., and the calcination time is 2-6 hours.

[0021] In the above technical solution, further, in step (5), the organic solvent is a mixture of one or more of methanol, ethanol, glycerol, and isopropanol.

[0022] The beneficial effects of the present invention are:

[0023] 1. The present invention uses light-burned magnesium oxide to produce high-purity magnesium oxide. The light-burned magnesium oxide used has many impurities and low purity and is widely available. The light-burned magnesium oxide is purified by hydration combined with acid leaching, which finds a new utilization method for preparing high-grade magnesium sources from domestic low-grade magnesium sources.

[0024] 2. The present invention utilizes amino acids as hydrating agents to assist in the hydration of magnesium oxide, thereby solving the problems of low hydration rate, high impurities, and great influence of the original powder in the traditional hydration method, and obtaining extremely high hydration rate and purity. At the same time, the complexing ability of carboxylate groups on magnesium and the alkalinity provided by amine groups are utilized to promote the dissolution of magnesium oxide and the heterogeneous generation of magnesium hydroxide, and the magnesium hydroxide is separated, thereby achieving the purpose of "clear and turbid diversion" treatment, reducing the amount of reagents and sulfuric acid leaching in the subsequent impurity removal process, and reducing the utilization rate of magnesium ions while reducing the operating costs.

[0025] 3. The present invention recycles the generated filtrate, waste gas and organic solvent to reduce pollutant emissions. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is a process flow chart of the method of the present invention. DETAILED DESCRIPTION

[0027] The following examples may enable those skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0028] Unless otherwise specified, the materials used in the embodiments of the present invention can be obtained through commercial channels or prepared according to conventional methods well known to those skilled in the art.

[0029] Example 1

[0030] (1) Hydration and stratification: 500 g of light-burned magnesium oxide powder (magnesite calcined at 800° C. for 3 h, sieved through a 200-mesh sieve, with a magnesium oxide content of 90%) was prepared into a suspension with water at a liquid-to-solid ratio of 3:1, and leucine was added as a hydrating agent in an amount of 1% of the mass of the light-burned magnesium oxide powder. The suspension was then hydrated at 50° C. and 300 rpm for 2.5 h. After the hydration was completed, the suspension was allowed to stand for 0.5 h, and a slurry and a precipitate were separated. The slurry was filtered to obtain a filter cake 1 and a filtrate 1, wherein the filtrate 1 was reused in the hydration and stratification stage;

[0031] (2) decalcification: the filter cake 1 obtained in step (1) is washed with water to remove the adsorbed residual hydrating agent, 5% by weight of magnesium chloride is added to the filter cake 1, and water is added to prepare a suspension 1 with a solid content of 10%, the suspension 1 is reacted at 35° C. and 150 rpm under stirring conditions for 1.5 h, and then filtered to obtain a filter cake 2 and a filtrate 2, wherein the filtrate 2 is reused in the decalcification stage;

[0032] (3) Silicon removal: The filter cake 2 obtained in step (2) is washed with water to remove the adsorbed residual magnesium chloride and calcium chloride, and sodium hydroxide (5% by weight of the filter cake 2) is added, and water is added to prepare a suspension 2 with a solid content of 15%. The suspension 2 is reacted at 35° C. and 200 rpm under stirring conditions for 1.5 hours, and then filtered to obtain a filter cake 3 and a filtrate 3, wherein the filtrate 3 is reused in the silicon removal stage, the filter cake 3 is washed with clean water three times to remove the adsorbed residual sodium hydroxide, and then dried at 80° C. for 10 hours to obtain high-purity magnesium hydroxide, and the high-purity magnesium hydroxide is calcined at 650° C. for 2 hours to obtain high-purity magnesium oxide, and the purity of the magnesium oxide is 99.5% after testing;

[0033] (4) Acid leaching of magnesium: The precipitate obtained by hydration and stratification in step (1) was washed and filtered, and then mixed with 1.5 mol / L sulfuric acid at a liquid-to-solid ratio of 18:1, and reacted at 60° C. and 150 rpm for 1.5 h. After filtering the insoluble matter, a magnesium salt solution was obtained;

[0034] (5) Dissolution crystallization: methanol solution was added in an amount of 10% of the volume of the magnesium salt solution, and the reaction was carried out at 35°C and 160 rpm under stirring conditions for 1.5 hours. After the crystallization was completed, the solid-liquid separation was carried out to obtain a crystallization mother liquor and magnesium sulfate crystals. The distillation temperature was controlled at 65°C and the distillation alcohol-water ratio was 0.25:1. 0.78 L of methanol solution was recovered. The magnesium sulfate crystals were washed twice with water to remove impurities remaining on the surface of the crystals, and then calcined at 1300°C for 4 hours to obtain high-purity magnesium oxide. The purity of the magnesium oxide was tested to be 99.34%. SO2 in the exhaust gas was absorbed by H2O2 and then reused in the acid leaching stage of magnesium.

[0035] Example 2

[0036] (1) Hydration and stratification: 500 g of light-burned magnesium oxide powder (magnesite calcined at 800° C. for 3 h, sieved through a 200-mesh sieve, with a magnesium oxide content of 90%) was prepared into a suspension with water at a liquid-to-solid ratio of 10:1, and threonine was added as a hydrating agent in an amount of 2.5% of the mass of the light-burned magnesium oxide powder. The suspension was then hydrated at 70° C. and 400 rpm for 3 h. After the hydration was completed, the suspension was allowed to stand for 0.75 h to separate the sizing liquid and the precipitate. The sizing liquid was filtered to obtain filter cake 1 and filtrate 1, wherein the filtrate 1 was reused to the hydration and stratification stage;

[0037] (2) decalcification: the filter cake 1 obtained in step (1) is washed with water to remove the adsorbed residual hydrating agent, magnesium chloride is added in an amount of 10% by weight of the filter cake 1, and water is added to prepare a suspension 1 with a solid content of 20%, the suspension 1 is reacted at 25° C. and stirred at 100 rpm for 1 hour, and then filtered to obtain a filter cake 2 and a filtrate 2, wherein the filtrate 2 is reused in the decalcification stage;

[0038] (3) Silicon removal: The filter cake 2 obtained in step (2) is washed with water to remove the adsorbed residual magnesium chloride and calcium chloride, and sodium hydroxide (7.5% by weight of the filter cake 2) is added, and water is added to prepare a suspension 2 with a solid content of 15%. The suspension 2 is reacted at 25° C. and 200 rpm under stirring conditions for 1.5 hours, and then filtered to obtain a filter cake 3 and a filtrate 3, wherein the filtrate 3 is reused in the silicon removal stage, the filter cake 3 is washed with clean water to remove the adsorbed residual sodium hydroxide, and then dried at 80° C. for 12 hours to obtain high-purity magnesium hydroxide, and the high-purity magnesium hydroxide is calcined at 650° C. for 2 hours to obtain high-purity magnesium oxide. The purity of the magnesium oxide is 99.2% after testing;

[0039] (4) Acid leaching of magnesium: The precipitate obtained by hydration and stratification in step (1) was washed and filtered, and then mixed with 1.6 mol / L sulfuric acid at a liquid-to-solid ratio of 15:1, and reacted at 60° C. and 150 rpm for 2 h. After filtering the insoluble matter, a magnesium salt solution was obtained;

[0040] (5) Dissolution crystallization: add ethanol solution in an amount of 15% of the volume of the magnesium salt solution, react at 35°C and 250rpm stirring conditions for 1.5h. After the crystallization is completed, the solid-liquid separation is carried out to obtain a crystallization mother liquor and magnesium sulfate crystals. The distillation temperature is controlled at 70°C and the distillation alcohol-water ratio is 0.3:1. 0.94L of ethanol solution is recovered. The magnesium sulfate crystals are washed twice with water to remove impurities remaining on the surface of the crystals, and then calcined at 1200°C for 5h to obtain high-purity magnesium oxide. The purity of the magnesium oxide is detected to be 99.21%. SO2 in the exhaust gas is absorbed by H2O2 and then reused in the acid leaching stage of magnesium.

[0041] Example 3

[0042] (1) Hydration and stratification: 500 g of light-burned magnesium oxide powder (magnesite calcined at 800° C. for 3 h, sieved through a 200-mesh sieve, with a magnesium oxide content of 90%) was prepared into a suspension with water at a liquid-to-solid ratio of 20:1, and lysine was added as a hydrating agent in an amount of 10% of the mass of the light-burned magnesium oxide powder. The suspension was then hydrated at 90° C. and 400 rpm for 2.5 h. After the hydration was completed, the suspension was allowed to stand for 0.5 h, and a slurry and a precipitate were separated. The slurry was filtered to obtain a filter cake 1 and a filtrate 1, wherein the filtrate 1 was reused in the hydration and stratification stage;

[0043] (2) decalcification: the filter cake 1 obtained in step (1) is washed with water to remove the adsorbed residual hydrating agent, 6% by weight of magnesium chloride is added to the filter cake 1, and water is added to prepare a suspension 1 with a solid content of 15%, the suspension 1 is reacted at 45° C. and 150 rpm under stirring conditions for 1.5 h, and then filtered to obtain a filter cake 2 and a filtrate 2, wherein the filtrate 2 is reused in the decalcification stage;

[0044] (3) Silicon removal: The filter cake 2 obtained in step (2) is washed with water to remove the adsorbed residual magnesium chloride and calcium chloride, and sodium hydroxide (7.5% by weight of the filter cake 2) is added, and water is added to prepare a suspension 2 with a solid content of 20%. The suspension 2 is reacted at 45° C. and 200 rpm under stirring conditions for 1.5 h, and then filtered to obtain a filter cake 3 and a filtrate 3, wherein the filtrate 3 is reused in the silicon removal stage, the filter cake 3 is washed with clean water to remove the adsorbed residual sodium hydroxide, and then dried at 80° C. for 10 h to obtain high-purity magnesium hydroxide, and the high-purity magnesium hydroxide is calcined at 650° C. for 2 h to obtain high-purity magnesium oxide. The purity of the magnesium oxide is 99.12% after testing;

[0045] (4) Acid leaching of magnesium: The precipitate obtained by hydration and stratification in step (1) was washed and filtered, and then mixed with 1.5 mol / L sulfuric acid at a liquid-to-solid ratio of 12:1, and reacted at 60° C. and 150 rpm for 1.5 h. After filtering the insoluble matter, a magnesium salt solution was obtained;

[0046] (5) Dissolution crystallization: methanol solution was added in an amount accounting for 25% of the volume of the magnesium salt solution, and the reaction was carried out at 35°C and 200 rpm under stirring conditions for 1.5 hours. After the crystallization was completed, the solid-liquid separation was performed to obtain a crystallization mother liquor and magnesium sulfate crystals. The distillation temperature was controlled at 65°C and the distillation alcohol-water ratio was 0.4:1. 1.25L of methanol solution was recovered. The magnesium sulfate crystals were washed twice with water to remove impurities remaining on the surface of the crystals, and then calcined at 1400°C for 4 hours to obtain high-purity magnesium oxide. The purity of the magnesium oxide was tested to be 99.11%. SO2 in the exhaust gas was absorbed by H2O2 and then reused in the acid leaching stage of magnesium.

[0047] Example 4

[0048] (1) Hydration and stratification: 500 g of light-burned magnesium oxide powder (magnesite calcined at 800° C. for 3 h, sieved through a 200-mesh sieve, with a magnesium oxide content of 90%) was prepared into a suspension with water at a liquid-to-solid ratio of 15:1, and valine was added as a hydrating agent in an amount of 6% of the mass of the light-burned magnesium oxide powder. The suspension was then hydrated at 80° C. and 350 rpm for 2 h. After the hydration was completed, the suspension was allowed to stand for 1 h to separate the sizing liquid and the precipitate. The sizing liquid was filtered to obtain filter cake 1 and filtrate 1, wherein the filtrate 1 was reused to the hydration and stratification stage;

[0049] 2) decalcification: the filter cake 1 obtained in step (1) is washed with water to remove the adsorbed residual hydrating agent, 8% of the mass of the filter cake 1 is added with magnesium chloride, and water is added to prepare a suspension 1 with a solid content of 15%, the suspension 1 is reacted at 50° C. and 150 rpm under stirring conditions for 2 h, and then filtered to obtain a filter cake 2 and a filtrate 2, wherein the filtrate 2 is reused in the decalcification stage;

[0050] (3) Silicon removal: The filter cake 2 obtained in step (2) is washed with water to remove the adsorbed residual magnesium chloride and calcium chloride, 5% by weight of sodium hydroxide is added to the filter cake 2, and water is added to prepare a suspension 2 with a solid content of 15%, the suspension 2 is reacted at 50° C. and 150 rpm for 2 h, and then filtered to obtain a filter cake 3 and a filtrate 3, wherein the filtrate 3 is reused in the silicon removal stage, the filter cake 3 is washed with clean water to remove the adsorbed residual sodium hydroxide, and then dried at 80° C. for 12 h to obtain high-purity magnesium hydroxide, and the high-purity magnesium hydroxide is calcined at 650° C. for 2 h to obtain high-purity magnesium oxide, and the purity of the magnesium oxide is 99.31% after testing;

[0051] (4) Acid leaching of magnesium: The precipitate obtained by hydration and stratification in step (1) was washed and filtered, and then mixed with 2 mol / L sulfuric acid at a liquid-to-solid ratio of 12:1, and reacted at 80° C. and 150 rpm for 1 h. After filtering the insoluble matter, a magnesium salt solution was obtained;

[0052] (5) Dissolution crystallization: add ethanol solution in an amount of 25% of the volume of the magnesium salt solution, react at 40°C and 200rpm stirring conditions for 1.5h, after the completion of crystallization, separate the solid and liquid to obtain crystallization mother liquor and magnesium sulfate crystals, control the distillation temperature at 80°C and the distillation alcohol-water ratio at 0.4:1, recover 1.25L of ethanol solution, wash the magnesium sulfate crystals with water three times to remove impurities remaining on the crystal surface, and calcine at 1200°C for 5h to obtain high-purity magnesium oxide. The purity of magnesium oxide is 99.21% after testing, and SO2 in the waste gas is absorbed by H2O2 and then reused in the acid leaching stage of magnesium.

[0053] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined in the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.

Claims

1. A method for preparing high-purity magnesium oxide using light-burned magnesium oxide as a raw material, characterized in that: The steps include: (1) Hydration and stratification: The light-burned magnesium oxide powder and water react with each other with the aid of an amino acid hydrating agent. After the reaction is completed, the mixture is allowed to stand for separation to obtain a slurry and a precipitate. The slurry is filtered to obtain a filter cake 1 and a filtrate 1. The filtrate 1 is reused in the hydration and stratification stage. (2) decalcification: the filter cake 1 obtained in step (1) is washed, magnesium chloride and water are added thereto to prepare a suspension 1, the suspension 1 is reacted under stirring conditions, and then filtered to obtain a filter cake 2 and a filtrate 2, and the filtrate 2 is reused in the decalcification stage; (3) silicon removal: washing the filter cake 2 obtained in step (2), adding sodium hydroxide and water to prepare a suspension 2, reacting the suspension 2 under stirring, and then filtering to obtain a filter cake 3 and a filtrate 3, washing and drying the filter cake 3 to obtain high-purity magnesium hydroxide, and calcining the high-purity magnesium hydroxide to obtain high-purity magnesium oxide; (4) Acid leaching to extract magnesium: adding the precipitate obtained in step (1) to a sulfuric acid solution, performing an acid leaching reaction under stirring conditions, and filtering to obtain a magnesium salt solution; (5) dissolution crystallization: adding an organic solvent to the magnesium salt solution obtained in step (4), performing solid-liquid separation after crystallization is completed to obtain a crystallization mother liquor and magnesium sulfate crystals, distilling the crystallization mother liquor to recover the organic solvent, washing the magnesium sulfate crystals and calcining them to obtain high-purity magnesium oxide and sulfur dioxide, and absorbing the sulfur dioxide with hydrogen peroxide and then recycling it to the stage of acid leaching magnesium.

2. The method for preparing high-purity magnesium oxide using light-burned magnesium oxide as raw material according to claim 1, characterized in that: In step (1), the liquid-to-solid ratio of water to light-burned magnesium oxide powder is 3:1-30:1; The standing time is 0.5-1h; The hydration reaction temperature is 50-90°C, and the hydration time is 2-6h.

3. The method for preparing high-purity magnesium oxide using light-burned magnesium oxide as raw material according to claim 1, characterized in that: In step (1), the amino acid hydrating agent is one or more of glycine, alanine, glutamic acid, valine, threonine, leucine, isoleucine, serine, aspartic acid, lysine, and arginine; The amount of the amino acid hydrating agent added is 0.1%-15% of the mass of the light-burned magnesium oxide.

4. The method for preparing high-purity magnesium oxide using light-burned magnesium oxide as raw material according to claim 1, characterized in that: In step (2), the amount of magnesium chloride added is 5%-10% of the mass of the filter cake 1; The solid content of the suspension 1 is 10%-20%; The reaction temperature is 25-50° C., the stirring speed is 100-200 rpm, and the reaction time is 1-2 h.

5. The method for preparing high-purity magnesium oxide using light-burned magnesium oxide as raw material according to claim 1, characterized in that: In step (3), the amount of sodium hydroxide added is 2%-15% of the mass of filter cake 2; The solid content of the suspension 2 is 10%-20%; The reaction temperature is 25-50° C., the stirring speed is 100-200 rpm, and the reaction time is 1-2 h.

6. The method for preparing high-purity magnesium oxide using light-burned magnesium oxide as raw material according to claim 1, characterized in that: In step (3), the drying temperature is 90-100° C. and the drying time is 10-12 h; The calcination temperature is 500-700° C., and the calcination time is 2-6 hours.

7. The method for preparing high-purity magnesium oxide using light-burned magnesium oxide as raw material according to claim 1, characterized in that: In step (4), the liquid-to-solid ratio of the precipitate to the sulfuric acid solution is 10:1-20:1; The concentration of the sulfuric acid solution is 1-2 mol / L; The temperature of the acid leaching reaction is 50-90° C., the stirring speed is 100-400 rpm, and the reaction time is 0.5-2 h.

8. The method for preparing high-purity magnesium oxide using light-burned magnesium oxide as raw material according to claim 1, characterized in that: In step (5), the amount of the organic solvent added is 10%-40% of the volume of the magnesium salt solution; The calcination temperature is 1200-1500° C., and the calcination time is 2-6 hours.