Method for preparing sodium aluminate clinker by dechlorination and denitrification of aluminum ash through dry sintering

Through the dry sintering of aluminum ash, dechlorination and nitrogen removal method, the reaction of iron sulfate with NaCl and AlN in aluminum ash is efficiently removed from chlorine and nitrogen in sodium aluminate clinker, and the aluminium ash wet treatment of ammonia air pollution and fire The method of dealing with the problem of low dechlorination has achieved efficient and environmentally friendly preparation of sodium aluminate clinker and reduced production costs.

CN118908256APending Publication Date: 2024-11-08HUOLINGUOLE JINLIAN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310512365.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The aluminum ash wet treatment has severe environmental pollution of ammonia, low dechlorination by fire treatment, low conversion of aluminum nitride, and high chlorine and nitrogen content of the product.

Method used

The aluminum ash dry sintering method is used to form sodium aluminate by grinding the aluminum ash, sodium carbonate and iron sulfate in a rotary furnace, and then preheating, primary calcining and dechlorination reactions. The secondary calcining is used to produce sodium aluminate Clinker uses the high-temperature decomposition characteristics of iron sulfate to react with NaCl and AlN in aluminum ash to achieve efficient removal of chlorine and nitrogen.

Benefits of technology

The generated sodium aluminate product has high purity and low chlorine and nitrogen content, which solves the environmental pollution problem, realizes the resource utilization of aluminum ash, and avoids ammonia pollution during the washing process. The process flow is short, the operation is simple, and the production cost is Low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908256A_ABST
    Figure CN118908256A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing sodium aluminate clinker by dechlorination and denitrification through aluminum ash dry sintering, belongs to the technical field of chemical production, and aims to solve the problems of serious environmental pollution caused by aluminum ash wet treatment of ammonia gas, low dechlorination and low aluminum nitride conversion rate in pyrogenic treatment and high chlorine and nitrogen content of a product in the prior art. The method comprises the following steps: grinding and uniformly mixing aluminum ash, sodium carbonate and ferric sulfate to obtain mixed powder; preheating the mixed powder; the preheated mixed powder is subjected to primary roasting, ferric sulfate is decomposed into Fe2O3, SO2 and O2, SO2 reacts with NaCl in the aluminum ash to remove chlorine, and Fe2O3 and O2 react with AlN in the aluminum ash to remove nitrogen; carrying out secondary roasting on the mixed powder subjected to primary roasting, and carrying out sintering reaction on Al2O3 and Na2CO3 in the aluminum ash to generate a sodium aluminate clinker; and the mixed powder obtained after secondary roasting is cooled. The method can be used for preparing the sodium aluminate clinker through aluminum ash dry sintering dechlorination and denitrification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical production, and in particular relates to a method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash. Background Art

[0002] Aluminum ash is the product of cooling the slag produced in the production process of electrolytic aluminum or cast aluminum. The main component of aluminum ash is aluminum oxide, and it also contains a small amount of metallic aluminum and some aluminum nitride, sodium fluoride, cryolite, etc. The metallic aluminum contained in aluminum ash is easy to catch fire when exposed to open flames, and the aluminum nitride contained in it will produce irritating ammonia when it comes into contact with water, causing great harm to the natural environment. Aluminum ash is highly flammable, irritating, leachable and harmful.

[0003] At present, there are two main methods for harmless disposal and resource utilization of aluminum ash in industry: pyrometallurgy and hydrometallurgy. The pyrometallurgy mainly uses aluminum ash as raw material to produce calcium aluminate slag for steelmaking by sintering or electric melting. The production is to mix aluminum ash and limestone (CaCO3) in a certain proportion and heat them in a rotary kiln or electric furnace at a heating temperature of 1200-1500℃. The alumina in the aluminum ash reacts with lime to form calcium aluminate slag; the reaction formula is: 7Al2O3+12CaCO3=12CaO·7Al2O3+12CO2(g). The production of calcium aluminate slag by pyrometallurgy from aluminum ash can avoid the escape of ammonia in the production process and solve the pollution problem of ammonia. However, due to the high content of nitrogen, fluorine and other elements in aluminum ash, the nitrogen and fluorine content of the produced calcium aluminate slag exceeds the standard, resulting in limited product utilization. Wet production uses aluminum ash as raw material, dechlorinates and denitrifies the aluminum ash in an acidic or alkaline environment, and further produces products such as aluminum sulfate and aluminum chloride. Although wet production can make comprehensive use of the aluminum in the aluminum ash, aluminum nitride will react with water during the production process to generate ammonia, which is easy to spread and pollute the environment. The reaction formula is: 2AlN+3H2O=Al2O3+2NH3(g). Since the generation of ammonia is difficult to avoid in the wet utilization of aluminum ash, and ammonia pollution is difficult to control, the environmental protection requirements for wet processing of aluminum ash are becoming more and more stringent.

[0004] The soda-lime sintering method is one of the main methods for producing alumina from high-silicon bauxite. The principle is to mix bauxite, sodium carbonate and lime in a certain proportion, sinter them in a rotary kiln to form a clinker composed of sodium aluminate (Na2O·Al2O3), sodium ferrite (Na2O·Fe2O3, calcium orthosilicate (2CaO·SiO2) and sodium titanate (CaO·TiO2), and then use a dilute alkaline solution to dissolve the sodium aluminate in the clinker. However, this method has low dechlorination, low aluminum nitride conversion rate, and high chlorine and nitrogen content in the product. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a method for preparing sodium aluminate clinker by dry sintering dechlorination and denitrogenation of aluminum ash, so as to solve the problems in the prior art of serious ammonia environmental pollution caused by wet treatment of aluminum ash, low dechlorination by pyrolysis, low aluminum nitride conversion rate and high chlorine and nitrogen content in the product.

[0006] The purpose of the present invention is mainly achieved through the following technical solutions.

[0007] The present invention provides a method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification, comprising the following steps:

[0008] Step 1: Grind aluminum ash, sodium carbonate and ferrous sulfate to obtain a mixed powder, and directly load the mixed powder into a rotary hearth furnace;

[0009] Step 2: Preheat the mixed powder;

[0010] Step 3: The preheated mixed powder is subjected to a roasting and dechlorination and denitrification reaction, wherein the ferric sulfate is decomposed into Fe2O3, SO2 and O2, SO2 reacts with NaCl in the aluminum ash to remove chlorine, and Fe2O3 and O2 react with AlN in the aluminum ash to remove nitrogen;

[0011] Step 4: The mixed powder of the primary roasting and dechlorination and denitrification is subjected to secondary roasting, and Al2O3 in the aluminum ash reacts with Na2CO3 to form sodium aluminate clinker;

[0012] Step 5: Cool the mixed powder after secondary roasting to complete the production of sodium aluminate clinker.

[0013] Furthermore, in step 1, the weight of sodium carbonate is 80% to 110% of the weight of the aluminum ash, and the weight of ferric sulfate is 5% to 10% of the weight of the aluminum ash.

[0014] Furthermore, in step 1, the grinding particle size is below 100 mesh.

[0015] Furthermore, in step 2, the mixed powder is heated to 350-450° C. after preheating.

[0016] Furthermore, in step 3, the reaction temperature is 500-1000° C., and the reaction time is 20-120 min.

[0017] Furthermore, in step 3, the generated chlorine-containing flue gas is discharged for dechlorination treatment.

[0018] Furthermore, in step 4, the reaction temperature is 1000-1350° C., and the reaction time is 10-60 min.

[0019] Furthermore, in step 4, the volatile matter containing dust generated by the secondary roasting is discharged for dust removal.

[0020] Furthermore, in step 5, the chlorine content in the sodium aluminate clinker is less than 0.5%, and the nitrogen content in the sodium aluminate clinker is less than 0.2%.

[0021] Furthermore, the method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification adopts a rotary hearth furnace, which includes a batching unit, a furnace body, a first distribution plate and a second distribution plate. The inner cavity of the furnace body is divided into a heating chamber and a roasting chamber which are independently arranged in the vertical direction. The roasting chamber is divided into a preheating zone, a first roasting zone, a second roasting zone and a cooling zone in sequence along the running direction of the mixed powder. A powder feeding port is provided in the preheating zone, and the batching unit is connected to the powder feeding port. A first smoke exhaust port is provided in the first roasting zone, and a second smoke exhaust port is provided in the second roasting zone. The first distribution plate is located at the feed end of the preheating zone, and the second distribution plate is located between the first roasting zone and the second roasting zone.

[0022] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects.

[0023] A) Aiming at the problem that the chlorine and nitrogen content in aluminum ash is high and the traditional wet dechlorination and nitrogen environmental pollution is serious, the method for preparing sodium aluminate clinker by dry sintering dechlorination and denitrification of aluminum ash provided by the present invention is to add ferric sulfate as a dechlorination and denitrification promoter, and roast in a rotary hearth furnace to obtain low-chlorine and low-nitrogen sodium aluminate clinker. The sodium aluminate product generated by the method has high purity, the aluminum ash does not need to be dechlorinated and denitrified by wet method, the aluminum ash has high conversion rate of aluminum nitride, and the removal rate of chlorine is high, which can solve the problem of environmental pollution, and the sodium aluminate clinker for extracting aluminum oxide is prepared, which can realize the resource efficient utilization of aluminum ash.

[0024] B) The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash provided by the present invention does not need to wash the aluminum ash for dechlorination and denitrification first, thus avoiding the problem of AlN reacting with water during the washing process to release NH3 to pollute the environment and the problem of sewage treatment, thereby achieving clean production and resource utilization of aluminum ash.

[0025] C) The method for preparing sodium aluminate clinker by dry sintering dechlorination and denitrification of aluminum ash provided by the present invention adopts ferric sulfate as a dechlorination and denitrification promoter, and utilizes the high temperature (500-1000°C) decomposition property of ferric sulfate. The generated SO2 can react with NaCl to dechlorinate (2NaCl+SO2+O2=Na2SO4+Cl2), and the solid Fe2O3 can react with AlN to denitrify (Fe2O3+2AlN=2Fe+Al2O3+N2), thereby realizing efficient removal of chlorine and nitrogen during dry sintering and preparing sodium aluminate clinker with low chlorine and nitrogen content.

[0026] D) The method for preparing sodium aluminate clinker by dry sintering, dechlorination and denitrification of aluminum ash provided by the present invention does not require briquetting. During the roasting process, the metal aluminum and aluminum nitride in the aluminum ash can be used for oxidation and heat release, thereby reducing roasting fuel consumption. The process flow is short, the operation is simple, the production cost is low, and it has good economic benefits.

[0027] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the embodiments of the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0029] Figure 1 A flow chart of the method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification provided by the present invention;

[0030] Figure 2 A schematic diagram of the structure of a rotary hearth furnace in the method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification provided by the present invention;

[0031] Figure 3 A schematic diagram of the connection between the first distribution plate and the furnace body in the method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification provided by the present invention;

[0032] Figure 4 A schematic diagram of the connection between the second distribution plate and the furnace body in the method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification provided by the present invention;

[0033] Figure 5 A schematic diagram of the connection of the height adjustment blocks in the method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification provided by the present invention;

[0034] Figure 6 for Figure 5 AA section view.

[0035] Reference numerals:

[0036] 1-preheating zone; 2-first roasting zone; 3-second roasting zone; 4-cooling zone; 5-powder feeding port; 6-first distribution plate; 7-second distribution plate; 8-spiral discharge port; 9-first smoke exhaust port; 10-second smoke exhaust port; 11-furnace bottom; 12-side wall; 13-top wall; 14-distribution plate guide rail; 15-height adjustment member; 151-height adjustment block; 152-first adjustment slot; 153-second adjustment slot; 154-third adjustment slot; 16-connecting protrusion; 17-first limit plate; 18-second limit plate. DETAILED DESCRIPTION

[0037] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0038] The present invention provides a method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification. Figure 1 , including the following steps:

[0039] Step 1: Raw material preparation: Grind aluminum ash, sodium carbonate and ferric sulfate and mix them to obtain a mixed powder, and directly charge the mixed powder into a rotary hearth furnace, wherein the weight of sodium carbonate is 80% to 110% of the weight of aluminum ash, the weight of ferric sulfate is 5% to 10% of the weight of aluminum ash, and the grinding particle size is less than 100 mesh;

[0040] Step 2: preheat the mixed powder, and heat the mixed powder to 350-450°C after preheating;

[0041] Step 3: The preheated mixed powder is subjected to a roasting and dechlorination and denitrification reaction: the mixed powder is heated to 500-1000°C in a rotary hearth furnace, the heating time is 10-60 minutes, the reaction time is 20-120 minutes, the ferric sulfate is decomposed into Fe2O3, SO2 and O2, SO2 reacts with NaCl in the aluminum ash to remove chlorine, the chlorine in the aluminum ash is converted into chlorine gas and discharged from the mixed powder in gaseous form, Fe2O3 and O2 react with AlN in the aluminum ash to remove nitrogen, Fe2O3 is a solid oxidant, which can react with AlN for a long time to achieve efficient removal of nitrogen and chlorine in the aluminum ash, the specific reaction formula is as follows:

[0042] The dechlorination reaction is: 2NaCl+SO2+O2=Na2SO4+Cl2

[0043] The denitrification reaction is: Fe2O3+2AlN=2Fe+Al2O3+N2

[0044] The generated chlorine-containing flue gas is discharged for treatment;

[0045] Step 4: Secondary roasting of the mixed powder after primary roasting and dechlorination and denitrification: The mixed powder after primary roasting and dechlorination and denitrification is secondary roasted, and Al2O3 in the aluminum ash reacts with Na2CO3 to generate sodium aluminate clinker. The reaction temperature is 1000-1350°C, and the reaction time is 10-60 minutes. The specific reaction formula is as follows:

[0046] Al2O3+Na2CO3=2NaAlO2+CO2

[0047] The volatiles (containing dust and CO2) produced by the secondary roasting are discharged for dust removal;

[0048] Step 5: Cool the mixed powder after secondary roasting to complete the production of sodium aluminate clinker. The chlorine content in the sodium aluminate clinker is <0.5%, and the nitrogen content in the clinker is <0.2%. It should be noted that the sodium aluminate clinker is used to leaching and extracting alumina to achieve the recycling of hazardous waste aluminum ash.

[0049] Compared with the prior art, the present invention aims at the problem that the chlorine and nitrogen content in aluminum ash is high, and the traditional wet dechlorination and nitrogen environmental pollution is serious. A method for preparing sodium aluminate clinker by dry sintering dechlorination and denitrification of aluminum ash is provided. By adding ferric sulfate as a dechlorination and denitrification promoter, low-chlorine and low-nitrogen sodium aluminate clinker is obtained by roasting in a rotary hearth furnace. The sodium aluminate product generated by the method has high purity, the aluminum ash does not need to be subjected to wet dechlorination and denitrification, the aluminum ash has a high conversion rate of aluminum nitride, and the removal rate of chlorine is high, which can solve the problem of environmental pollution, and the sodium aluminate clinker for extracting aluminum oxide is prepared, which can realize the resource utilization and efficient utilization of aluminum ash.

[0050] Specifically, on the one hand, the above-mentioned method of dry sintering dechlorination and denitrification of aluminum ash to prepare sodium aluminate clinker does not need to wash the aluminum ash for dechlorination and denitrification first, thus avoiding the release of NH3 from the reaction of AlN with water during the washing process to pollute the environment and the problem of sewage treatment, thereby realizing the clean production and resource utilization of aluminum ash.

[0051] On the other hand, the above-mentioned method for preparing sodium aluminate clinker by dry sintering dechlorination and denitrification of aluminum ash adopts ferric sulfate as a dechlorination and denitrification promoter, and utilizes the high temperature (500-1000°C) decomposition characteristics of ferric sulfate. The generated SO2 can react with NaCl to dechlorinate (2NaCl+SO2+O2=Na2SO4+Cl2), and the solid Fe2O3 can react with AlN to denitrify (Fe2O3+2AlN=2Fe+Al2O3+N2), thereby realizing the efficient removal of chlorine and nitrogen during the dry sintering process and preparing sodium aluminate clinker with low chlorine and nitrogen content.

[0052] On the other hand, the above-mentioned method for preparing sodium aluminate clinker by dry sintering dechlorination and denitrogenation of aluminum ash does not require briquetting. During the roasting process, the metallic aluminum and aluminum nitride in the aluminum ash can be used for oxidation and heat release, thereby reducing roasting fuel consumption. The process flow is short, the operation is simple, the production cost is low, and it has good economic benefits.

[0053] For example, the above-mentioned method for preparing sodium aluminate clinker by dry sintering of aluminum ash for dechlorination and denitrification adopts a rotary hearth furnace, see Figures 2 to 4 The rotary hearth furnace includes a batching unit, a furnace body, a first distribution plate 6 and a second distribution plate 7. The inner cavity of the furnace body is divided into a heating chamber and a roasting chamber which are independently arranged in the vertical direction. An electric heater or a heating burner is arranged in the heating chamber. The roasting chamber is divided into a preheating zone 1, a first roasting zone 2, a second roasting zone 3 and a cooling zone 4 in sequence along the running direction of the mixed powder. The temperature of the preheating zone 1 is below 500°C, the control temperature of the first roasting zone 2 is 500-1000°C, the control temperature of the second roasting zone 3 is 1000-1350°C, and the preheating zone 1 (for example, the feeding end of the preheating zone 1) is opened. The material feeding port 5 is connected to the batching unit, the first roasting zone 2 (for example, the discharge end of the first roasting zone 2) is provided with a first smoke exhaust port 9, the second roasting zone 3 (for example, the discharge end of the second roasting zone 3) is provided with a second smoke exhaust port 10, the first distribution plate 6 is located at the feeding end of the preheating zone 1, and the mixed powder of aluminum ash, sodium carbonate and ferric sulfate entering from the powder feeding port 5 passes through the first distribution plate 6 and enters the preheating zone 1, the second distribution plate 7 is located between the first roasting zone 2 and the second roasting zone 3, and the mixed powder of aluminum ash, sodium carbonate and ferric sulfate passes through the second plate and enters the second roasting zone 3.

[0054] It should be noted that the raw materials used in traditional rotary hearth furnace technology usually require the raw materials to be pressed or pelletized to produce pellets. However, for aluminum ash, water needs to be added during pressing or pelletizing. Adding water to aluminum ash for pressing or pelletizing will produce serious ammonia pollution. Therefore, it is usually not considered to use a rotary hearth furnace for aluminum ash roasting.

[0055] Compared with the prior art, the rotary hearth furnace for producing sodium aluminate by roasting aluminum ash provided by the present invention is suitable for direct high-temperature roasting of powder materials. Mixed powder materials containing aluminum ash are directly fed into the furnace. Sodium chlorate can be produced by roasting aluminum ash in a rotary hearth furnace without generating ammonia pollution. The sintering temperature is uniform and high, and the roasting quality of the product can be greatly improved.

[0056] Specifically, the rotary hearth furnace for producing sodium aluminate by roasting aluminum ash provided by the present invention adopts an external heating method, and the heating chamber and the roasting chamber are independently arranged. The heating medium (for example, fuel gas) does not directly contact the mixed powder in the roasting chamber, so that the rotary hearth furnace can be used to roast aluminum ash to produce sodium aluminate. In addition, the heating chamber and the roasting chamber are independently arranged. Since the smoke generated by roasting is not mixed with the smoke generated in the roasting chamber, it is beneficial to achieve harmless treatment of the smoke generated in the roasting chamber.

[0057] At the same time, in the above-mentioned rotary hearth furnace used for roasting aluminum ash to produce sodium aluminate, the roasting chamber of the rotary hearth furnace is divided into a preheating zone 1, a first roasting zone 2, a second roasting zone 3 and a cooling zone 4, and a first smoke exhaust port 9 and a second smoke exhaust port 10 are respectively provided in the first roasting zone 2 and the second roasting zone 3. The chlorine-containing flue gas generated by roasting the mixed powder in the first roasting zone 2 is discharged through the first smoke exhaust port 9. The chlorine concentration in the chlorine-containing flue gas is high, which is conducive to the low-cost treatment of the chlorine-containing flue gas. By respectively providing two roasting zones and two smoke exhaust ports, the flue gas generated by different roasting temperatures can be graded.

[0058] In addition, through the first distribution plate 6, uniform distribution from the powder feed port to the preheating zone 1 can be achieved, and through the second distribution plate 7, uniform distribution from the first roasting zone 2 to the second roasting zone 3 can be achieved, thereby greatly improving the heating uniformity and heating efficiency of the mixed powder, facilitating the discharge and treatment of volatiles in aluminum ash, and improving the roasting quality of the product.

[0059] As for the structure of the batching unit, specifically, it includes an aluminum ash storage chamber, a sodium carbonate storage chamber, a ferrous sulfate storage chamber and a mixing chamber. The discharge ports of the aluminum ash storage chamber, the sodium carbonate storage chamber and the ferrous sulfate storage chamber are respectively connected to the feed port of the mixing chamber, and the discharge port of the mixing chamber is connected to the powder feed port. The raw materials (i.e., aluminum ash, sodium carbonate and aluminum sulfate) are supplied into the mixing chamber for mixing to obtain mixed powder, and are supplied into the preheating chamber through the powder feed port.

[0060] It can be understood that in order to form the inner cavity of the rotary hearth furnace, the above-mentioned furnace body includes a furnace bottom 11, side walls 12 and a top wall 13. The furnace bottom 11 serves as the bottom surface of the furnace body, the side walls 12 serve as the sides of the furnace body, and the top wall 13 serves as the top surface of the furnace body. One of the side walls 12 is defined as a first side wall 12, and the other side wall 12 is defined as a second side wall 12. One side of the furnace bottom 11 is connected to the bottom of the first side wall 12, and the other side of the furnace bottom 11 is connected to the bottom of the second side wall 12. One side of the top wall 13 is connected to the bottom of the first side wall 12, and the other side of the top wall 13 is connected to the bottom of the second side wall 12, thereby forming a furnace body.

[0061] As for the structures of the first distribution plate 6 and the second distribution plate 7, the structures of the two are basically the same. Specifically, they include a plate body and a serrated portion arranged at one end of the plate body facing the mixed powder (i.e., the lower end). The serrated portion is inserted into the mixed powder. The distribution plate with a serrated end can increase the surface area of ​​the mixed powder, thereby obtaining a larger heating area and improving the heating efficiency.

[0062] In order to realize automatic material turning, the saw teeth of the second distribution plate 7 are staggered with the saw teeth of the first distribution plate 6, and the tooth tips of the second distribution plate 7 correspond to the tooth roots of the first distribution plate 6. In this way, when the mixed powder passes through the first distribution plate 6, a sawtooth or wavy surface will be formed. When passing through the second distribution plate 7, the tooth tips of the second distribution plate 7 will correspond to the protrusions on the surface of the mixed powder and insert into the protrusions, thereby realizing automatic material turning, further improving the heating uniformity of the mixed powder, achieving uniform heating from top to bottom, and improving the quality of the roasted products.

[0063] In order to improve the stability of the sawtooth shape of the mixed powder and ensure that the sawtooth shape of the mixed powder does not collapse during the roasting process, illustratively, the tooth tip angle of the sawtooth of the first distribution plate 6 and the second distribution plate 7 is 60 to 90 degrees.

[0064] In order to prevent the mixed powder from piling up when passing through the second distribution plate 7, the distance between the tooth tip of the second distribution plate 7 and the furnace bottom 11 of the furnace body is greater than the distance between the tooth tip of the first distribution plate 6 and the furnace bottom 11 of the furnace body.

[0065] In order to ensure uniform distribution, the distance between the tooth tip of the first distribution plate 6 and the furnace bottom 11 of the furnace body is 1 to 2 cm, and the sawtooth height of the first distribution plate 6 is 10 to 15 cm.

[0066] Similarly, the distance between the tooth tip of the second distribution plate 7 and the furnace bottom 11 of the furnace body is 3-4 cm, and the sawtooth height of the second distribution plate 7 is 10-15 cm.

[0067] Considering that different aluminum ash may require adjusting the distance between the first distribution plate 6, the second distribution plate 7 and the furnace bottom 11 of the furnace body, that is, the distribution thickness of the mixed powder, the first distribution plate 6 and the second distribution plate 7 further include a connecting protrusion 16 and a height adjustment member 15, see Figures 5 and 6 The height adjustment member 15 includes an adjustment rod and a height adjustment block 151. The height adjustment block 151 is provided with a plurality of height adjustment grooves which penetrate the height adjustment block 151 transversely. The depths of the plurality of height adjustment grooves are different. The connecting protrusion 16 is fixedly connected to the plate body. The adjustment rod is rotatably connected to the connecting protrusion 16. The height adjustment block 151 is fixedly connected to the side wall 12 of the furnace body. The adjustment rod is inserted into any of the height adjustment grooves, so as to adjust the cloth thickness according to the heating performance of the mixed powder, and then adjust the roasting time to improve the heating uniformity of the mixed powder.

[0068] For example, there are three height adjustment slots, and the three height adjustment slots all have intersections at the center of the height adjustment block 151. The three height adjustment slots are the first adjustment slot 152, the second adjustment slot 153, and the third adjustment slot 154. The first adjustment slot 152 has a slot depth of 1 cm, the second adjustment slot 153 has a slot depth of 3 cm, the third adjustment slot 154 has a slot depth of 5 cm, and the height of the adjustment rod is 6 cm. In this way, when the adjustment rod is placed in the first adjustment slot 152, the height of the adjustment rod is 5 cm higher than the first adjustment slot 152; when the adjustment rod is rotated to place it in the second adjustment slot 153, the height of the adjustment rod is 3 cm higher than the second adjustment slot 153; when the adjustment rod is rotated to place it in the third adjustment slot 154, the height of the adjustment rod is 1 cm higher than the third adjustment slot 154, so that the spacing between the first distribution plate 6, the second distribution plate 7 and the furnace bottom 11 of the furnace body can be adjusted, and the adjustable distance range is 1 to 5 cm.

[0069] Taking into account that during the distribution process, the mixed powder will have a certain force on the first distribution plate 6 and the second distribution plate 7, in order to reduce the deformation and shaking of the first distribution plate 6 and the second distribution plate 7, the above-mentioned first distribution plate 6 and the second distribution plate 7 also include distribution plate guide rails 14, one of which is arranged on one side wall 12 of the furnace body in the vertical direction, and the other distribution plate guide rail 14 is arranged on the other side wall 12 of the furnace body in the vertical direction. The plate body is inserted into the distribution plate guide rail 14, and the distribution plate guide rail 14 can limit the horizontal movement of the plate body, thereby reducing the deformation and shaking of the first distribution plate 6 and the second distribution plate 7.

[0070] In order to ensure the dechlorination and denitrification effects and the reaction effects of the calcination reaction at the same time, the arc angles of the first calcination zone 2 and the second calcination zone 3 are equal, and the corresponding mixed powders are heated for the same time in the first calcination zone 2 and the second calcination zone 3. This is because, considering the limited volume of the calcination chamber, it is divided into four areas (preheating zone 1, first calcination zone 2, second calcination zone 3 and cooling zone 4), and the size of each area needs to be comprehensively considered to ensure the respective heating and reaction effects.

[0071] Exemplarily, the arc angle of the preheating zone 1 is 85-95° (e.g., 90°), the arc angle of the first roasting zone 2 is 100-110° (e.g., 105°), the arc angle of the second roasting zone 3 is 100-110° (e.g., 105°), and the arc angle of the cooling zone 4 is 55-65° (e.g., 60°).

[0072] That is to say, the preheating zone 1 is from the powder feeding port 5 to the position where the rotary hearth furnace is rotated 85 to 95 degrees, the first roasting zone 2 is from the end of the preheating zone 1 to the position where the rotary hearth furnace is rotated 100 to 110 degrees, the second roasting zone 3 is from the end of the first roasting zone 2 to the position where the rotary hearth furnace is rotated 100 to 110 degrees, and the cooling zone 4 is from the end of the second roasting zone 3 to the position where the rotary hearth furnace is rotated 55 to 65 degrees (i.e., the position of the discharge port).

[0073] From the perspective of the temperature at the feed end of the first roasting zone 2, the first distribution plate 6 is made of stainless steel or heat-resistant alloy steel, the thickness of the first distribution plate 6 is 1 to 3 cm, and the width difference between the furnace bottom 11 of the furnace body and the width of the first distribution plate 6 is 10 to 20 cm. In this way, by appropriately shortening the width of the first distribution plate 6, it can be ensured that the mixed powder is basically evenly distributed on the furnace bottom 11 without leaking out from the gaps on both sides of the furnace bottom 11.

[0074] In order to further prevent the mixed powder from leaking out of the gaps on both sides of the furnace bottom 11, the above-mentioned first distribution plate 6 also includes a first limiting plate 17. There are two first limiting plates 17, which are arranged perpendicular to the running direction of the mixed powder. One of the first limiting plates 17 is arranged on one side of the first distribution plate 6, and the other first limiting plate 17 is arranged on the other side of the first distribution plate 6. The shape of the first limiting plate 17 is an inverted L-shape, and the gap between the bottom end of the first limiting plate 17 and the furnace bottom 11 is 0.5 to 0.8 cm.

[0075] Similarly, from the perspective of the temperature between the first calcination zone 2 and the second calcination zone 3, the second distribution plate 7 is made of silicon carbide, and the thickness of the second distribution plate 7 is 2 to 4 cm (for example, 3 cm). This is because the temperature between the first calcination zone 2 and the second calcination zone 3 is relatively high, and the use of silicon carbide as the material of the second distribution plate 7 has high heat resistance and wear resistance, which can effectively extend the service life of the second distribution plate 7.

[0076] In order to further prevent the mixed powder from leaking out of the gaps on both sides of the furnace bottom 11, the above-mentioned second distribution plate 7 also includes a second limiting plate 18. There are two second limiting plates 18, which are arranged perpendicular to the running direction of the mixed powder. One second limiting plate 18 is arranged on one side of the second distribution plate 7, and the other second limiting plate 18 is arranged on the other side of the second distribution plate 7. The shape of the second limiting plate 18 is an inverted L-shape, and the gap between the bottom end of the second limiting plate 18 and the furnace bottom 11 is 0.5 to 0.8 cm.

[0077] It can be understood that in order to achieve uniform discharge of sodium aluminate, a spiral discharge port 8 is provided at the discharge end of the cooling zone 4, and spiral and uniform discharge of sodium aluminate is achieved through the spiral discharge port 8.

[0078] Embodiment 1

[0079] A mixed powder of aluminum ash, sodium carbonate and ferrous sulfate is added to the powder feeding port through a belt. The feed end of the preheating zone is equipped with a first distribution plate made of stainless steel. The first distribution plate is serrated, with a thickness of 2 cm and an included angle of 60°. The distance between the tip of the sawtooth of the first distribution plate and the root of the sawtooth of the first distribution plate is 10 cm, and the length of the first distribution plate is 10 cm smaller than the width of the furnace bottom.

[0080] The guide rails of the first distribution board are installed on the side wall. A height adjustment member is installed on both sides of the top wall 13. The height adjustment member is adjusted so that the distance between the tooth tip of the first distribution board and the furnace bottom is 1 cm.

[0081] The mixed powder in the powder feeding port rotates with the rotary hearth furnace, and is evenly distributed through the first distribution plate, and passes through the preheating zone and enters the first roasting zone. The heating temperature in the first roasting zone is 500°C. The mixed powder reacts to produce chlorine-containing flue gas, which is discharged from the first exhaust port. The rotary hearth furnace uses natural gas for external heating, and the generated flue gas is not mixed with the roasting flue gas.

[0082] A second distribution plate made of silicon carbide is installed between the first roasting zone and the second roasting zone. The thickness is 3cm, the angle of the saw teeth is 60°, and the distance between the tip of the second distribution plate and the furnace bottom is 3cm. The mixed powder is turned over when passing through the second distribution plate, and then enters the second roasting zone. The heating temperature of the second roasting zone is 1000℃, and the volatiles generated by roasting are discharged through the second exhaust port. The mixed powder is sintered into sodium aluminate in the second roasting zone, and then cooled in the cooling zone and discharged through the spiral discharge port.

[0083] The raw materials of this embodiment include aluminum ash (Al content 45%, Cl content 2%, N content 5%), industrial sodium carbonate and industrial ferric sulfate.

[0084] Process steps: 100kg of aluminum ash, 93kg of industrial sodium carbonate and 5kg of industrial ferric sulfate are ground to less than 100 meshes on a ball mill, and then the mixed powder is added into a rotary hearth furnace. The rotary hearth furnace adopts electric heating to control the short temperature of dechlorination and denitrification to 500°C, the insulation time is 60min, and the calcination reaction temperature of sodium aluminate is controlled to 1000°C, the insulation time is 60min. After the reaction is completed, the mixed powder is discharged from the rotary hearth furnace and cooled to obtain sodium aluminate clinker, and the Cl content in the clinker is 0.2% and the nitrogen content is 0.1%.

[0085] Example 2

[0086] The structure and parameters of the rotary hearth furnace used in this embodiment are basically the same as those in Embodiment 1, and will not be described in detail here.

[0087] The raw materials of this embodiment include aluminum ash (Al content 51%, Cl content 5%, N content 3%), industrial sodium carbonate and industrial ferric sulfate.

[0088] Process steps: 100kg of aluminum ash, 110kg of industrial sodium carbonate and 8kg of industrial ferric sulfate are ground to less than 100 meshes on a ball mill, and then the mixed powder is added into a rotary hearth furnace. The rotary hearth furnace adopts electric heating to control the short temperature of dechlorination and denitrification to 800°C, the insulation time is 30min, the calcination reaction temperature of sodium aluminate is controlled to 1200°C, the insulation time is 40min, and after the reaction is completed, the mixed powder is discharged from the rotary hearth furnace and cooled to obtain sodium aluminate clinker, the Cl content in the clinker is 0.5%, and the nitrogen content is 0.2%.

[0089] Example 3

[0090] The structure and parameters of the rotary hearth furnace used in this embodiment are basically the same as those in Embodiment 1, and will not be described in detail here.

[0091] The raw materials of this embodiment include aluminum ash (Al content 40%, Cl content 8%, N content 4%), industrial sodium carbonate and industrial ferric sulfate.

[0092] Process steps: 100kg of aluminum ash, 80kg of industrial sodium carbonate and 10kg of industrial ferric sulfate are ground to less than 100 meshes on a ball mill, and then the mixed powder is added into a rotary hearth furnace. The rotary hearth furnace adopts electric heating to control the short temperature of dechlorination and denitrification to 1000°C, the insulation time is 30min, and the reaction temperature of sodium aluminate is controlled to 1350°C, the insulation time is 10min. After the reaction is completed, the mixed powder is discharged from the rotary hearth furnace and cooled to obtain sodium aluminate clinker, and the Cl content in the clinker is 0.4% and the nitrogen content is 0.1%.

[0093] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash, characterized in that: The steps include: Step 1: Grind aluminum ash, sodium carbonate and ferrous sulfate to obtain a mixed powder, and directly load the mixed powder into a rotary hearth furnace; Step 2: Preheat the mixed powder; Step 3: The preheated mixed powder is subjected to a roasting and dechlorination and denitrification reaction, wherein the ferric sulfate is decomposed into Fe2O3, SO2 and O2, SO2 reacts with NaCl in the aluminum ash to remove chlorine, and Fe2O3 and O2 react with AlN in the aluminum ash to remove nitrogen; Step 4: The mixed powder of the primary roasting and dechlorination and denitrification is subjected to secondary roasting, and Al2O3 in the aluminum ash reacts with Na2CO3 to form sodium aluminate clinker; Step 5: Cool the mixed powder after secondary roasting to complete the production of sodium aluminate clinker.

2. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In step 1, the weight of sodium carbonate is 80% to 110% of the weight of the aluminum ash, and the weight of ferric sulfate is 5% to 10% of the weight of the aluminum ash.

3. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In the step 1, the grinding particle size is below 100 mesh.

4. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In the step 2, the mixed powder is heated to 350-450° C. after being preheated.

5. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In step 3, the reaction temperature is 500-1000° C., and the reaction time is 20-120 min.

6. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In step 3, the generated chlorine-containing flue gas is discharged for dechlorination treatment.

7. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In step 4, the reaction temperature is 1000-1350° C., and the reaction time is 10-60 min.

8. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In step 4, the volatile matter containing dust generated by the secondary roasting is discharged for dust removal.

9. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to claim 1, characterized in that: In step 5, the chlorine content in the sodium aluminate clinker is less than 0.5%, and the nitrogen content in the sodium aluminate clinker is less than 0.2%.

10. The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash according to any one of claims 1 to 9, characterized in that: The method for preparing sodium aluminate clinker by dry sintering and dechlorination and denitrification of aluminum ash adopts a rotary hearth furnace.

Citation Information

Cited By

  • Secondary aluminum ash denitrification pretreatment method

    CN121315014A