Preparation method and application of basalt coupled carbon fiber composite biological electrode
Through the preparation of basalt fiber and carbon fiber composite materials, combined with SiCnw/Ti60 composite materials, basalt coupled carbon fiber composite bioelectrode is formed, which solves the problems of insufficient degradation efficiency and voltage output of bioelectrode materials in the prior art, and achieves efficient wastewater treatment effect .
Patent Information
- Application Number
- CN202410972573.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing bioelectrode materials have insufficient degradation efficiency and voltage output in microbial fuel cells, and cannot effectively treat difficult-to-degradable organic pollutants in industrial wastewater, limiting the biological purification effect and industrial applications.
Basalt fiber and carbon fiber composite materials are used to increase the fiber surface area through Soxhlet extraction and etching treatment, and combined with SiCnw/Ti60 composite materials, a basalt coupled carbon fiber composite bioelectrode is formed to enhance its bioaffinity and mechanical properties, and to electrolyze it in microbial biologic Applied in the pool.
It significantly improves the biodegradation performance and conductivity of bioelectrodes, improves the sewage treatment efficiency of microbial electrolytic cells, and provides a low-cost and efficient industrial wastewater treatment solution.
Smart Images

Figure CN118908398A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bioelectrodes, and in particular relates to a preparation method and application of a basalt-coupled carbon fiber composite bioelectrode. Background Art
[0002] In the process of biotechnology treatment of wastewater in the chemical industry, the activity of microorganisms and the efficiency of electron transfer are the key factors affecting the biological purification effect. Among them, microbial electrochemical system (BES) is a new technology currently widely used in environmental bioremediation. The main principle is to use microorganisms to degrade organic pollutants and convert the chemical energy in pollutants into electrical energy in situ. It is a new type of biotechnology and energy recovery technology. Representative technologies include microbial fuel cells (MFC) and microbial electrolysis cells (MEC).
[0003] Among them, the material and selection of the electrode directly affect the degradation efficiency and voltage output of BES for pollutants. At present, the most widely used bioelectrode materials are mostly carbon-based materials (graphite electrodes, carbon cloth, etc.), metal materials (nickel foam, titanium wire mesh, etc.), conductive polymer materials (glassy carbon) and composite electrodes (polyaniline coating, carbon nanotube composites). Among them, carbon-based materials have been widely used in microbial fuel cells due to their good electrochemical stability, biocompatibility and structural plasticity. Compared with other electrode materials, carbon-based materials are cheap and easy to obtain, but compared with fillers in conventional biological systems, they are still relatively expensive and cannot be used in large-scale mass production, thus limiting the industrial application of BES in wastewater treatment. However, most of the ordinary biological fillers do not have good electrical conductivity, and cannot construct BES to improve the effect of biodegradation. They can only play the role of enriching microorganisms to form biofilms. Therefore, the demand for developing new bioelectrode materials for industrial applications is more urgent.
[0004] Industrial wastewater contains a variety of difficult-to-degrade organic substances, which pose a threat to the environment and human health. Wastewater generated in the production process of the chemical industry often contains a large amount of difficult-to-degrade organic pollutants with complex composition, high concentration and poor biodegradability, so biotechnology cannot achieve the expected results.
[0005] Therefore, how to improve the preparation method and materials of the composite bioelectrode to further improve its bioaffinity and mechanical properties, so as to improve its biodegradability for sewage has become a technical problem to be solved in this field. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a basalt-coupled carbon fiber composite bioelectrode, which is used to solve the technical problem of how to further improve its biological affinity and mechanical properties by improving the preparation method and materials of the composite bioelectrode, so as to improve its biodegradability of sewage.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing a basalt-coupled carbon fiber composite bioelectrode comprises the following steps:
[0009] (1) Using the Soxhlet extraction method, the basalt fiber is placed in a solvent, and the original impregnation agent on the surface of the basalt fiber is dissolved by heating and refluxing. After the Soxhlet extraction is completed, the fiber is taken out, washed with water and dried to obtain clean basalt fiber;
[0010] (2) Etching treatment of basalt fiber: prepare an etching solution using sodium hydroxide, hydrochloric acid and nitric acid, immerse the clean basalt fiber in the etching solution, etch to increase the fiber specific surface area, surface roughness and adhesion, take out after the reaction, wash with water and dry to obtain basalt fiber filler;
[0011] (3) After cutting the carbon fiber, soak it in hydrochloric acid and sulfuric acid for more than 2 hours, store it in acetone overnight, and then take it out and dry it;
[0012] (4) connecting the basalt fiber filler and the carbon fiber by weaving them in a 2:1 ratio, and connecting the carbon fiber to the end of the basalt fiber to obtain a basalt carbon fiber composite material;
[0013] (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill, and then place them in a planetary ball mill for ball milling to obtain a mixed powder;
[0014] (6) placing the mixed powder into a graphite mold with a diameter of 1 mm and sintering it in a spark plasma activated sintering furnace to complete the coupling of SiCnw and Ti60, and finally obtaining a SiCnw / Ti60 composite material;
[0015] (7) The woven basalt carbon fiber composite material is clamped by two SiCnw / Ti60 composite materials, and the two titanium wires are continuously twisted to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material to obtain a basalt-coupled carbon fiber composite bioelectrode material.
[0016] Furthermore, in the preparation method of the basalt-coupled carbon fiber composite bioelectrode, in step (1), the solvent used is one of acetone, isopropanol, cyclohexane, and petroleum ether, the heating reflux temperature is 40 to 100° C., and the heating reflux time is 12 to 72 hours.
[0017] Furthermore, in the preparation method of the basalt-coupled carbon fiber composite bioelectrode, in step (2), the concentration of sodium hydroxide is 0.5-2 mol / L; the concentration of hydrochloric acid is 0.5-2 mol / L; the concentration of nitric acid is 0.01-0.1 mol / L; the etching time is 10-120 min, and the temperature of the etching solution is 20-100°C.
[0018] Preferably, the concentration of sodium hydroxide is 1 mol / L; the concentration of hydrochloric acid is 1 mol / L; the concentration of nitric acid is 0.03 mol / L; the etching time is 60 min, and the temperature of the etching solution is 40°C.
[0019] Furthermore, in the preparation method of the basalt-coupled carbon fiber composite bioelectrode, in step (5), the ball mill and the grinding balls are both made of stainless steel, and the ball-to-material ratio is 3 to 5:1; the ball mill speed is 300 to 500 r / min, and the ball milling time is 4 to 6 hours.
[0020] Furthermore, in the preparation method of the basalt-coupled carbon fiber composite bioelectrode, in step (6), the sintering temperature is 1000-1200° C., the pressure is 40-60 MPa, and the insulation time is 5-20 min.
[0021] The present invention also provides an application method of a basalt-coupled carbon fiber composite bioelectrode, which is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor comprises the following steps:
[0022] (1) Assembling basalt coupled carbon fiber composite bioelectrode materials to obtain the anode and cathode of the microbial electrolytic cell;
[0023] (2) Inoculating the bacterial community: inoculating the electroactive bacterial community in the sludge into the anode of the reactor;
[0024] (3) Cultivation of biofilm: After inoculation, a stable electroactive biofilm was formed after 7 days of cultivation;
[0025] (4) Wastewater addition: After the stable electroactive biofilm is formed, it is immersed in artificially prepared synthetic wastewater to control the pH of the wastewater to 6-8;
[0026] (5) Operation: applying a voltage between the anode and cathode of the microbial electrolysis cell, the voltage range is 0.02-0.4 V;
[0027] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0028] Preferably, the sludge inoculated in step (2) is taken from Yanjing Beer Guilin Liquan Co., Ltd., and the fresh sludge is anaerobically cultured in the laboratory for one week, then diluted with tap water at a mud-water volume ratio of 1:2, and then 2L of the diluted sludge is passed into the anode of the device; step (4) controls the pH of the wastewater to 7.
[0029] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0030] 1. The preparation method of the basalt-coupled carbon fiber composite bioelectrode of the present invention, on the basis of the existing technology, connects the basalt fiber filler and the carbon fiber by weaving and connecting them in strands, and the basalt carbon fiber composite material is tightly connected with the SiCnw / Ti60 composite material; since the basalt fiber has a large specific surface area and excellent biocompatibility, the carbon fiber has excellent conductivity, and the SiCnw / Ti60 composite material has good bioaffinity and stable electrochemical properties and excellent mechanical properties, the electrode biological bearing capacity, conductivity and mechanical properties are greatly improved. When applied to a microbial electrolytic cell, the microorganisms can quickly attach to the electrode material and form a biofilm, and when placed in a conventional biofilter and a biological system, the biodegradability can be significantly improved.
[0031] 2. The preparation method of basalt-coupled carbon fiber composite bioelectrode is simple to operate, low-cost, and has mild process conditions. The addition of SiCnw / Ti60 composite materials and electroactive bacteria can improve the efficiency of organic matter removal, providing an efficient solution for industrial wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 Schematic diagram of the preparation of the basalt-coupled carbon fiber composite bioelectrode of the present invention;
[0034] Figure 2 Electron microscope images of materials before and after microbial biofilm formation in the microbial electrolysis cell of the present invention;
[0035] Figure 3 Implementation diagram of the microbial electrolysis cell of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0039] (1) Using the Soxhlet extraction method, the basalt fiber is placed in acetone, and the original impregnation agent on the surface of the basalt fiber is dissolved by heating and reflux, wherein the heating and reflux temperature is 40° C. and the heating and reflux time is 12 h. After the Soxhlet extraction is completed, the fiber is taken out, washed with water and dried to obtain clean basalt fiber;
[0040] (2) Etching treatment of basalt fiber: prepare an etching solution with 0.5 mol / L sodium hydroxide, 0.5 mol / L hydrochloric acid, and 0.01 mol / L nitric acid, immerse the clean basalt fiber in the etching solution, wherein the etching time is 10 min, and the etching solution temperature is 20°C. After the reaction is completed, take out, wash with water, and dry to obtain basalt fiber filler;
[0041] (3) After the carbon fiber is cut, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours, placed in acetone overnight, and then taken out and dried. Carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods;
[0042] (4) The basalt fiber filler and the carbon fiber are connected by weaving in a 2:1 ratio, and the carbon fiber is connected to the end of the basalt fiber to obtain a basalt carbon fiber composite material. The porosity of the basalt fiber provides an attachment point for biological molecules, while the conductivity of the carbon fiber provides an electron transfer channel for electrochemical degradation;
[0043] (5) Ti60 alloy powder and SiCnw were weighed, loaded into a ball mill, and then placed in a planetary ball mill for ball milling, wherein the ball-to-material ratio was 3:1, the ball mill speed was 300 r / min, and the ball milling time was 4 h to obtain a mixed powder. The titanium alloy has the characteristics of high specific strength, excellent corrosion resistance and high conductivity. The one-dimensional nanomaterial silicon carbide nanowire (SiCnw) not only inherits the excellent properties of high strength and low thermal expansion coefficient of SiC, but also has better mechanical properties, such as higher strength and better toughness due to its unique nanoscale effect;
[0044] (6) placing the mixed powder into a graphite mold with a diameter of 1 mm and sintering it in a spark plasma activated sintering furnace, wherein the sintering temperature is 1000° C., the pressure is 40 MPa, and the holding time is 5 min to complete the coupling of SiCnw and Ti60 to obtain a SiCnw / Ti60 composite material;
[0045] (7) The woven basalt carbon fiber composite material was clamped by two SiCnw / Ti60 composite materials, and the two SiCnw / Ti60 composite materials were continuously twisted to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally a basalt-coupled carbon fiber composite bioelectrode material was obtained. The prepared basalt-coupled carbon fiber composite bioelectrode material was named MBFNW1.
[0046] The MBFNW1 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor comprises the following steps:
[0047] (1) Assembling basalt coupled carbon fiber composite bioelectrode materials to obtain the anode and cathode of the microbial electrolytic cell;
[0048] (2) Inoculation of bacteria: The electroactive bacteria in the sludge were inoculated into the anode of the reactor. The inoculated sludge was taken from Yanjing Beer Guilin Liquan Co., Ltd. After one week of anaerobic culture, tap water was added to dilute the sludge at a sludge-water volume ratio of 1:2, and 2 L of the diluted sludge was introduced into the anode of the device.
[0049] (3) Cultivation of biofilm: After inoculation with sludge, a stable electroactive biofilm was formed after 7 days of cultivation;
[0050] (4) Wastewater addition: After the stable electroactive biofilm is formed, it is immersed in artificially prepared synthetic wastewater to control the pH of the wastewater to 6;
[0051] (5) Operation: Apply a voltage of 0.02 V between the anode and cathode of the microbial electrolysis cell;
[0052] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0053] Example 2
[0054] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0055] (1) Using the Soxhlet extraction method, the basalt fiber is placed in acetone, and the original impregnation agent on the surface of the basalt fiber is dissolved by heating and reflux, wherein the heating and reflux temperature is 50° C. and the heating and reflux time is 24 h. After the Soxhlet extraction is completed, the fiber is taken out, washed with water and dried to obtain clean basalt fiber;
[0056] (2) Etching treatment of basalt fiber: prepare an etching solution with 1 mol / L sodium hydroxide, 1 mol / L hydrochloric acid, and 0.02 mol / L nitric acid, immerse the clean basalt fiber in the etching solution, wherein the etching time is 30 min, and the etching solution temperature is 30°C. After the reaction is completed, take out, wash with water, and dry to obtain basalt fiber filler;
[0057] (3) After the carbon fiber is cut, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours, placed in acetone overnight, and then taken out and dried. Carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods;
[0058] (4) The basalt fiber filler and the carbon fiber are connected by weaving in a 2:1 ratio, and the carbon fiber is connected to the end of the basalt fiber to obtain a basalt carbon fiber composite material. The porosity of the basalt fiber provides an attachment point for biological molecules, while the conductivity of the carbon fiber provides an electron transfer channel for electrochemical degradation;
[0059] (5) Ti60 alloy powder and SiCnw were weighed, loaded into a ball mill, and then placed in a planetary ball mill for ball milling, wherein the ball-to-material ratio was 3:1, the ball mill speed was 300 r / min, and the ball milling time was 4 h to obtain a mixed powder. The titanium alloy has the characteristics of high specific strength, excellent corrosion resistance and high conductivity. The one-dimensional nanomaterial silicon carbide nanowire (SiCnw) not only inherits the excellent properties of high strength and low thermal expansion coefficient of SiC, but also has better mechanical properties, such as higher strength and better toughness due to its unique nanoscale effect;
[0060] (6) placing the mixed powder into a graphite mold with a diameter of 1 mm, and sintering it in a spark plasma activated sintering furnace, wherein the sintering temperature is 1100° C., the pressure is 45 MPa, and the holding time is 10 min to complete the coupling of SiCnw and Ti60 to obtain a SiCnw / Ti60 composite material;
[0061] (7) The woven basalt carbon fiber composite material was clamped by two SiCnw / Ti60 composite materials, and the two SiCnw / Ti60 composite materials were continuously twisted to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally a basalt-coupled carbon fiber composite bioelectrode material was obtained. The prepared basalt-coupled carbon fiber composite bioelectrode material was named MBFNW2.
[0062] The MBFNW2 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor comprises the following steps:
[0063] (1) Assembling basalt coupled carbon fiber composite bioelectrode materials to obtain the anode and cathode of the microbial electrolytic cell;
[0064] (2) Inoculation of bacteria: The electroactive bacteria in the sludge were inoculated into the anode of the reactor. The inoculated sludge was taken from Yanjing Beer Guilin Liquan Co., Ltd. After one week of anaerobic culture, tap water was added to dilute the sludge at a sludge-water volume ratio of 1:2, and 2 L of the diluted sludge was introduced into the anode of the device.
[0065] (3) Cultivation of biofilm: After inoculation with sludge, a stable electroactive biofilm was formed after 7 days of cultivation;
[0066] (4) Wastewater addition: After the stable electroactive biofilm is formed, it is immersed in artificially prepared synthetic wastewater to control the pH of the wastewater to 7;
[0067] (5) Operation: Apply a voltage of 0.05 V between the anode and cathode of the microbial electrolysis cell;
[0068] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0069] Example 3
[0070] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0071] (1) Using the Soxhlet extraction method, the basalt fiber is placed in isopropanol, and the original impregnation agent on the surface of the basalt fiber is dissolved by heating and reflux, wherein the heating and reflux temperature is 60° C. and the heating and reflux time is 24 h. After the Soxhlet extraction is completed, the fiber is taken out, washed with water and dried to obtain clean basalt fiber;
[0072] (2) Etching treatment of basalt fiber: prepare an etching solution with 1 mol / L sodium hydroxide, 1 mol / L hydrochloric acid, and 0.03 mol / L nitric acid, immerse the clean basalt fiber in the etching solution, wherein the etching time is 60 min, and the etching solution temperature is 40°C. After the reaction is completed, take out, wash with water, and dry to obtain basalt fiber filler;
[0073] (3) After the carbon fiber is cut, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours, placed in acetone overnight, and then taken out and dried. Carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods;
[0074] (4) The basalt fiber filler and the carbon fiber are connected by weaving in a 2:1 ratio, and the carbon fiber is connected to the end of the basalt fiber to obtain a basalt carbon fiber composite material. The porosity of the basalt fiber provides an attachment point for biological molecules, while the conductivity of the carbon fiber provides an electron transfer channel for electrochemical degradation;
[0075] (5) Ti60 alloy powder and SiCnw are weighed, loaded into a ball mill, and then placed in a planetary ball mill for ball milling, wherein the ball-to-material ratio is 3:1, the ball mill speed is 300r / min, and the ball milling time is 5h to obtain a mixed powder. The titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. The one-dimensional nanomaterial silicon carbide nanowire (SiCnw) not only inherits the excellent properties of SiC's high strength and low thermal expansion coefficient, but also has better mechanical properties due to its unique nanoscale effect, such as higher strength and better toughness;
[0076] (6) placing the mixed powder into a graphite mold with a diameter of 1 mm, and sintering it in a spark plasma activated sintering furnace, wherein the sintering temperature is 1000° C., the pressure is 45 MPa, and the holding time is 5 min to complete the coupling of SiCnw and Ti60 to obtain a SiCnw / Ti60 composite material;
[0077] (7) The woven basalt carbon fiber composite material was clamped by two SiCnw / Ti60 composite materials, and the two SiCnw / Ti60 composite materials were continuously twisted to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally a basalt-coupled carbon fiber composite bioelectrode material was obtained. The prepared basalt-coupled carbon fiber composite bioelectrode material was named MBFNW3.
[0078] The MBFNW3 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor comprises the following steps:
[0079] (1) Assembling basalt coupled carbon fiber composite bioelectrode materials to obtain the anode and cathode of the microbial electrolytic cell;
[0080] (2) Inoculation of bacteria: The electroactive bacteria in the sludge were inoculated into the anode of the reactor. The inoculated sludge was taken from Yanjing Beer Guilin Liquan Co., Ltd. After one week of anaerobic culture, tap water was added to dilute the sludge at a sludge-water volume ratio of 1:2, and 2 L of the diluted sludge was introduced into the anode of the device.
[0081] (3) Cultivation of biofilm: After inoculation with sludge, a stable electroactive biofilm was formed after 7 days of cultivation;
[0082] (4) Wastewater addition: After the stable electroactive biofilm is formed, it is immersed in artificially prepared synthetic wastewater to control the pH of the wastewater to 7;
[0083] (5) Operation: Apply a voltage of 0.1 V between the anode and cathode of the microbial electrolysis cell;
[0084] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0085] Example 4
[0086] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0087] (1) Using the Soxhlet extraction method, the basalt fiber is placed in cyclohexane, and the original impregnation agent on the surface of the basalt fiber is dissolved by heating and reflux, wherein the heating and reflux temperature is 80°C and the heating and reflux time is 72 hours. After the Soxhlet extraction is completed, the fiber is taken out, washed with water and dried to obtain clean basalt fiber;
[0088] (2) Etching treatment of basalt fiber: prepare an etching solution with 1.5 mol / L sodium hydroxide, 1.5 mol / L hydrochloric acid, and 0.05 mol / L nitric acid, immerse the clean basalt fiber in the etching solution, wherein the etching time is 120 min, and the etching solution temperature is 80°C. After the reaction is completed, take out, wash with water, and dry to obtain basalt fiber filler;
[0089] (3) After the carbon fiber is cut, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours, placed in acetone overnight, and then taken out and dried. Carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods;
[0090] (4) The basalt fiber filler and the carbon fiber are connected by weaving in a 2:1 ratio, and the carbon fiber is connected to the end of the basalt fiber to obtain a basalt carbon fiber composite material. The porosity of the basalt fiber provides an attachment point for biological molecules, while the conductivity of the carbon fiber provides an electron transfer channel for electrochemical degradation;
[0091] (5) Ti60 alloy powder and SiCnw are weighed, loaded into a ball mill, and then placed in a planetary ball mill for ball milling, wherein the ball-to-material ratio is 4:1, the ball mill speed is 400r / min, and the ball milling time is 5h to obtain a mixed powder. The titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. The one-dimensional nanomaterial silicon carbide nanowire (SiCnw) not only inherits the excellent properties of SiC's high strength and low thermal expansion coefficient, but also has better mechanical properties due to its unique nanoscale effect, such as higher strength and better toughness;
[0092] (6) placing the mixed powder into a graphite mold with a diameter of 1 mm, and sintering it in a spark plasma activated sintering furnace, wherein the sintering temperature is 1200° C., the pressure is 50 MPa, and the holding time is 15 min to complete the coupling of SiCnw and Ti60 to obtain a SiCnw / Ti60 composite material;
[0093] (7) The woven basalt carbon fiber composite material was clamped by two SiCnw / Ti60 composite materials, and the two SiCnw / Ti60 composite materials were continuously twisted to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally a basalt-coupled carbon fiber composite bioelectrode material was obtained. The prepared basalt-coupled carbon fiber composite bioelectrode material was named MBFNW4.
[0094] The MBFNW4 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor comprises the following steps:
[0095] (1) Assembling basalt coupled carbon fiber composite bioelectrode materials to obtain the anode and cathode of the microbial electrolytic cell;
[0096] (2) Inoculation of bacteria: The electroactive bacteria in the sludge were inoculated into the anode of the reactor. The inoculated sludge was taken from Yanjing Beer Guilin Liquan Co., Ltd. After one week of anaerobic culture, the fresh sludge was diluted with tap water at a sludge-to-water volume ratio of 1:2, and 2 L of the diluted sludge was introduced into the anode of the device.
[0097] (3) Cultivation of biofilm: After inoculation with sludge, a stable electroactive biofilm was formed after 7 days of cultivation;
[0098] (4) Wastewater addition: After the stable electroactive biofilm is formed, it is immersed in artificially prepared synthetic wastewater to control the pH of the wastewater to 8;
[0099] (5) Operation: Apply a voltage of 0.2 V between the anode and cathode of the microbial electrolysis cell;
[0100] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0101] Example 5
[0102] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0103] (1) Using the Soxhlet extraction method, the basalt fiber is placed in petroleum ether, and the original impregnation agent on the surface of the basalt fiber is dissolved by heating and reflux, wherein the heating and reflux temperature is 100° C. and the heating and reflux time is 72 hours. After the Soxhlet extraction is completed, the fiber is taken out, washed with water and dried to obtain clean basalt fiber;
[0104] (2) Etching treatment of basalt fiber: prepare an etching solution with 2 mol / L sodium hydroxide, 2 mol / L hydrochloric acid, and 0.1 mol / L nitric acid, immerse the clean basalt fiber in the etching solution, wherein the etching time is 120 min, and the etching solution temperature is 100°C. After the reaction is completed, take out, wash with water, and dry to obtain basalt fiber filler;
[0105] (3) After the carbon fiber is cut, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours, placed in acetone overnight, and then taken out and dried. Carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods;
[0106] (4) The basalt fiber filler and the carbon fiber are connected by weaving in a 2:1 ratio, and the carbon fiber is connected to the end of the basalt fiber to obtain a basalt carbon fiber composite material. The porosity of the basalt fiber provides an attachment point for biological molecules, while the conductivity of the carbon fiber provides an electron transfer channel for electrochemical degradation;
[0107] (5) Ti60 alloy powder and SiCnw are weighed, loaded into a ball mill, and then placed in a planetary ball mill for ball milling, wherein the ball-to-material ratio is 5:1, the ball mill speed is 500r / min, and the ball milling time is 6h to obtain a mixed powder. The titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. The one-dimensional nanomaterial silicon carbide nanowire (SiCnw) not only inherits the excellent properties of SiC's high strength and low thermal expansion coefficient, but also has better mechanical properties due to its unique nanoscale effect, such as higher strength and better toughness;
[0108] (6) placing the mixed powder into a graphite mold with a diameter of 1 mm, and sintering it in a spark plasma activated sintering furnace, wherein the sintering temperature is 1200° C., the pressure is 60 MPa, and the holding time is 20 min to complete the coupling of SiCnw and Ti60 to obtain a SiCnw / Ti60 composite material;
[0109] (7) The woven basalt carbon fiber composite material was clamped by two SiCnw / Ti60 composite materials, and the two SiCnw / Ti60 composite materials were continuously twisted to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally a basalt-coupled carbon fiber composite bioelectrode material was obtained. The prepared basalt-coupled carbon fiber composite bioelectrode material was named MBFNW5.
[0110] The MBFNW5 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor comprises the following steps:
[0111] (1) Assembling basalt coupled carbon fiber composite bioelectrode materials to obtain the anode and cathode of the microbial electrolytic cell;
[0112] (2) Inoculation of bacteria: The electroactive bacteria in the sludge were inoculated into the anode of the reactor. The inoculated sludge was taken from Yanjing Beer Guilin Liquan Co., Ltd. After one week of anaerobic culture, tap water was added to dilute the sludge at a sludge-water volume ratio of 1:2, and 2 L of the diluted sludge was introduced into the anode of the device.
[0113] (3) Cultivation of biofilm: After inoculation with sludge, a stable electroactive biofilm was formed after 7 days of cultivation;
[0114] (4) Wastewater addition: After the stable electroactive biofilm is formed, it is immersed in artificially prepared synthetic wastewater to control the pH of the wastewater to 8;
[0115] (5) Operation: Apply a voltage of 0.4 V between the anode and cathode of the microbial electrolysis cell;
[0116] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0117] Comparative Example 1
[0118] Comparative Example 1 Compared with Example 3, when preparing the basalt-coupled carbon fiber composite bioelectrode in Comparative Example 1, titanium alloy was directly used for connection without adding SiCnw for improvement, and other conditions remained unchanged.
[0119] Comparative Example 2
[0120] Comparative Example 2 Compared with Example 3, when preparing the microbial electrolysis cell, the electrode is directly placed in the wastewater without inoculating sludge colonies, and other conditions remain unchanged.
[0121] Comparative Example 3
[0122] Comparative Example 3 Compared with Example 3, when preparing basalt fiber, Comparative Example 3 directly uses basalt fiber without etching treatment, and other conditions remain unchanged.
[0123] Comparative Example 4
[0124] Compared with Example 3, in Comparative Example 4, when preparing carbon fiber, carbon fiber is directly used without soaking in hydrochloric acid and sulfuric acid in sequence, and other conditions remain unchanged.
[0125] Experimental example
[0126] The performance of the basalt-coupled carbon fiber composite bioelectrodes prepared in Examples 1-5 and Comparative Examples 1-4 were monitored.
[0127] 1. COD effluent concentration
[0128] With industrial sewage configured with COD 500mg / L and COD:N:P ratio of 100:5:1 as influent, the COD effluent concentration was measured by the online automatic monitoring instrument from the fifth day after the microbial electrolysis cell reactor was connected. The monitored values were counted every five days, three groups of data were counted each time, and a total of six times. The average COD effluent concentration is shown in Table 1:
[0129] Table 1
[0130]
[0131]
[0132] It can be seen from the results of the measurement in Table 1 that the microbial electrolysis cell of the basalt-coupled carbon fiber composite bioelectrode material prepared in Examples 1-5 of the present invention has an excellent COD removal rate. By comparing Comparative Example 1 with Examples 1-5, it can be seen that adding SiCnw to improve Ti60 can improve the COD removal rate of the microbial electrolysis cell of the basalt-coupled carbon fiber composite bioelectrode material; by comparing Comparative Example 2 with Examples 1-5, it can be seen that inoculating sludge bacteria can improve the COD removal rate of the microbial electrolysis cell of the basalt-coupled carbon fiber composite bioelectrode material; by comparing Comparative Example 3 with Examples 1-5, it can be seen that etching the basalt fiber can improve the COD removal rate of the microbial electrolysis cell of the basalt-coupled carbon fiber composite bioelectrode material; by comparing Comparative Example 4 with Examples 1-5, it can be seen that soaking the carbon fiber in hydrochloric acid and sulfuric acid in sequence can improve the COD removal rate of the microbial electrolysis cell of the basalt-coupled carbon fiber composite bioelectrode material.
[0133] 2. Total nitrogen effluent concentration
[0134] With industrial wastewater configured with COD 500mg / L and COD:N:P ratio of 100:5:1 as the influent, the total nitrogen effluent concentration was measured by the online automatic monitoring instrument from the 5th day after the microbial electrolysis cell reactor was connected. The monitored values were counted every 5 days, three groups of data were counted each time, and a total of 6 times. The average value of the total nitrogen effluent concentration is shown in Table 2:
[0135] Table 2
[0136]
[0137]
[0138] It can be seen from the results of Table 2 that the microbial electrolysis pool of basalt-coupled carbon fiber composite bioelectrode materials prepared in Examples 1-5 of the present invention has an excellent total nitrogen removal rate. By comparing Comparative Example 1 with Examples 1-5, it can be seen that adding SiCnw to improve Ti60 can improve the total nitrogen removal rate of the microbial electrolysis pool of basalt-coupled carbon fiber composite bioelectrode materials; by comparing Comparative Example 2 with Examples 1-5, it can be seen that inoculating sludge bacteria can improve the total nitrogen removal rate of the microbial electrolysis pool of basalt-coupled carbon fiber composite bioelectrode materials; by comparing Comparative Example 3 with Examples 1-5, it can be seen that etching basalt fibers can improve the total nitrogen removal rate of the microbial electrolysis pool of basalt-coupled carbon fiber composite bioelectrode materials; by comparing Comparative Example 4 with Examples 1-5, it can be seen that soaking carbon fibers in hydrochloric acid and sulfuric acid in sequence can improve the total nitrogen removal rate of the microbial electrolysis pool of basalt-coupled carbon fiber composite bioelectrode materials.
[0139] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0140] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a basalt-coupled carbon fiber composite bioelectrode, characterized in that: The steps include: (1) Using the Soxhlet extraction method, the basalt fiber is placed in a solvent, and the original impregnation agent on the surface of the basalt fiber is dissolved by heating and refluxing. After the Soxhlet extraction is completed, the fiber is taken out, washed with water and dried to obtain clean basalt fiber; (2) Etching treatment of basalt fiber: prepare an etching solution with sodium hydroxide, hydrochloric acid and nitric acid, immerse the clean basalt fiber in the etching solution, etch to increase the fiber specific surface area, surface roughness and adhesion, take out after the reaction, wash with water and dry to obtain basalt fiber filler; (3) After cutting the carbon fiber, soak it in hydrochloric acid and sulfuric acid for more than 2 hours, store it in acetone overnight, and then take it out and dry it; (4) connecting the basalt fiber filler and the carbon fiber by weaving them in a 2:1 ratio, and connecting the carbon fiber to the end of the basalt fiber to obtain a basalt carbon fiber composite material; (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill, and then place them in a planetary ball mill for ball milling to obtain a mixed powder; (6) placing the mixed powder into a graphite mold with a diameter of 1 mm and sintering it in a spark plasma activated sintering furnace to complete the coupling of SiCnw and Ti60, and finally obtaining a SiCnw / Ti60 composite material; (7) The woven basalt carbon fiber composite material is clamped by two SiCnw / Ti60 composite materials, and the two SiCnw / Ti60 composite materials are continuously twisted to tightly connect the basalt carbon fiber composite material with the SiCnw / Ti60 composite material to obtain a basalt-coupled carbon fiber composite bioelectrode material.
2. The method for preparing the basalt-coupled carbon fiber composite bioelectrode according to claim 1, characterized in that: In step (1), the solvent used is one of acetone, isopropanol, cyclohexane and petroleum ether; the heating reflux temperature is 40 to 100° C., and the heating reflux time is 12 to 72 hours.
3. The method for preparing the basalt-coupled carbon fiber composite bioelectrode according to claim 1, characterized in that: In step (2), the concentration of sodium hydroxide is 0.5-2 mol / L, the concentration of hydrochloric acid is 0.5-2 mol / L, the concentration of nitric acid is 0.01-0.1 mol / L, the etching time is 10-120 min, and the temperature of the etching solution is 20-100° C.
4. The method for preparing the basalt-coupled carbon fiber composite bioelectrode according to claim 1, characterized in that: In step (5), the ball-to-material ratio is 3-5:1; the ball mill speed is 300-500 r / min, and the ball milling time is 4-6 h.
5. The method for preparing the basalt-coupled carbon fiber composite bioelectrode according to claim 1, characterized in that: In step (6), the sintering temperature is 1000-1200° C., the pressure is 40-60 MPa, and the holding time is 5-20 min.
6. An application method of a basalt-coupled carbon fiber composite bioelectrode, characterized in that: The microorganism electrolysis cell is applied thereto. The assembly method of the microorganism electrolysis cell reactor comprises the following steps: (1) Assembling basalt coupled carbon fiber composite bioelectrode materials to obtain the anode and cathode of the microbial electrolytic cell; (2) Inoculating the bacterial community: inoculating the electroactive bacterial community in the sludge into the anode of the reactor; (3) Cultivation of biofilm: After inoculation, a stable electroactive biofilm was formed after 7 days of cultivation; (4) Wastewater addition: After the stable electroactive biofilm is formed, it is immersed in artificially prepared synthetic wastewater; (5) Operation: applying a voltage between the anode and cathode of the microbial electrolysis cell; (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
7. The application method of the basalt-coupled carbon fiber composite bioelectrode according to claim 6, characterized in that: The sludge inoculated in step (2) was taken from Yanjing Beer Guilin Liquan Co., Ltd. After the fresh sludge was anaerobically cultured in the laboratory for one week, tap water was added to dilute it at a sludge-to-water volume ratio of 1:2, and then 2L of the diluted sludge was passed into the anode of the device.
8. The application method of the basalt-coupled carbon fiber composite bioelectrode according to claim 6, characterized in that: In step (4), the pH of the wastewater is controlled to be 6-8.
9. The application method of the basalt-coupled carbon fiber composite bioelectrode according to claim 6, characterized in that: The voltage range in step (5) is 0.02 to 0.4 V.
Citation Information
Patent Citations
Preparation method of water treatment filler capable of loading microorganisms and filler system
CN114149072A
Anaerobic MBR (Membrane Bioreactor) deep carbon reduction device and method driven by electroactive biological membrane
CN115286101A
Preparation method of nano-cellulose modified basalt fiber biological filler
CN115745143A
Preparation method of diamond-based high-activity three-dimensional particle electrode material, three-dimensional electrode reactor and application
CN116332293A
Electric strengthening device and method for strengthening biological denitrification of swine wastewater
CN116768416A