Temperature-stable capacitor ceramic powder with core-shell structure and preparation method and application thereof
By using the combination of BaTiO3-based ceramic powder with modifier and glass powder in MLCC, the problem of unstable capacity temperature change rate and increased loss in small size and large capacity applications is solved, and stability is achieved The capacity temperature change rate and small dielectric loss are suitable for MLCC of thin dielectric layers.
Patent Information
- Application Number
- CN202410929334.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The X7R-based barium titanate-based ceramic material with medium and low temperature sintered in Pb-Ag internal electrode MLCC is difficult to accurately control the core-shell structure in process, resulting in unstable capacity temperature change rate in applications such as small size and large capacity of MLCC. The problem of increased loss.
Temperature-stable capacitor porcelain powder with core-shell structure is adopted, the main component is BaTiO3, doping modifiers include TiO2, NaCO3 and Nb2O5, and glass powder includes Li-B-Si and Bi-B glass compounds, and the particles are strictly controlled. The diameter and abrasive process stabilizes the particle size and activity of the main crystal phase and doped modified substances, and compensates for the core-shell structure concentration gradient when the dielectric layer becomes thin.
It realizes stable capacity temperature change rate and small dielectric loss in MLCC small size and large capacity applications, maintains high withstand voltage, and increases the dielectric constant at the temperature end of 25℃~125℃ by about 8%~15 with the increase in temperature. %.
Smart Images

Figure CN118908723A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic materials and their manufacturing, and in particular to a temperature-stable capacitor ceramic powder with a core-shell structure, a preparation method and application thereof. Background Art
[0002] Multilayer ceramic capacitors (MLCC) with temperature stability and large capacity are suitable for circuits such as switching power supplies, power amplifiers, and transmitters. They play the role of bypass, low-frequency coupling, power supply filtering, and DC blocking. They are widely used in aerospace, shipbuilding, automotive, communications, satellites, weapons, military equipment, and other fields. With the iterative upgrade of electronic technology and the increasing demand year by year, MLCC is developing towards large capacity, high stability, high reliability, and low cost, and the thickness of single-layer ceramic film dielectrics is tending to be thinner.
[0003] At present, barium titanate-based ceramic materials with X7R characteristics are the main materials for preparing such capacitors. They have been widely studied and are mostly used in MLCC capacitors. Most of these ceramic materials are rare earth oxides, alkaline earth metal oxides or carbonates, transition metal oxides, etc. doped with barium titanate to form a core-shell microstructure to achieve capacity temperature stability. The degree of temperature stability is determined by the core-shell structure concentration gradient of the grains of the main crystal phase of barium titanate. The core-shell structure concentration gradient is formed by doping. Affected by the type and quantity of dopants, the size of the main crystal phase particles, and the sintering process, the same doping amount can form different core-shell microstructure concentration gradients under different preparation and sintering processes, thereby obtaining different capacity temperature change rates. In the preparation process of MLCC, the grinding process, the thickness of the ceramic film, the internal electrode components, and the sintering curve will weaken the core-shell microstructure concentration gradient to varying degrees, which will affect the proportion of the material forming a "core-shell" structure, resulting in a deterioration of the capacity temperature change rate and an increase in loss. This phenomenon is more prominent when preparing small-sized and large-capacity MLCCs due to the thinning of the dielectric layer. This problem restricts the development of MLCCs to small sizes and large capacities.
[0004] In the prior art, patent ZL201611170717.6 proposed a dielectric material for medium and high voltage X7R multilayer ceramic capacitors, patent ZL201010530760.5 proposed a multilayer ceramic capacitor dielectric ceramic material with anti-reduction properties, and patent ZL201710922478.3 proposed a ceramic dielectric material for high withstand voltage MLCC and its preparation, but none of them has been applied to thin dielectric layer MLCC. The dielectric material invented by patent CN 114999817 A "A dielectric material for thin dielectric X7R MLCC and its preparation method" is suitable for making MLCC products with dielectrics of 4μm or more and working voltages of 25V and above, using base metal nickel or nickel alloy as the inner electrode, sintering in a nitrogen-hydrogen reducing atmosphere, and the sintering temperature is 1220-1260℃.
[0005] At present, the research and application of barium titanate-based ceramic materials with X7R characteristics sintered at medium and low temperatures for Pb-Ag internal electrode MLCCs are mainly focused on the formulation system, doping modification, etc. Although the content of the doping modifier is precisely controlled, the process is not precisely controlled. In the application of small-size and large-capacity MLCCs, there are problems such as unstable capacity temperature change rate and increased loss. Summary of the invention
[0006] The technical problem to be solved by the present invention is that it is difficult to accurately control the core-shell structure of the current barium titanate-based ceramic material with X7R characteristics sintered at medium and low temperatures for Pb-Ag internal electrode MLCC in terms of process, and there are problems such as unstable capacity temperature change rate and increased loss in small-size and large-capacity MLCC applications. The purpose is to provide a temperature-stable capacitor porcelain powder with a core-shell structure, a preparation method and application thereof, which solves the problem that it is difficult to accurately control the core-shell structure of the current barium titanate-based ceramic material with X7R characteristics sintered at medium and low temperatures for Pb-Ag internal electrode MLCC in terms of process, and there are problems such as unstable capacity temperature change rate and increased loss in small-size and large-capacity MLCC applications.
[0007] The present invention is achieved through the following technical solutions:
[0008] In the first aspect, the present application provides a temperature-stable capacitor porcelain powder with a core-shell structure, the main component of which is BaTiO3, and the BaTiO3 is doped with a modifier and glass powder; the components of the modifier include TiO2, NaCO3 and Nb2O5; the glass powder includes Li-B-Si glass compound and Bi-B glass compound.
[0009] In the preparation process of multilayer ceramic capacitors (MLCC), in order to fully mix the ceramic powder with the organic solvent, the ceramic powder and the organic solvent mixture need to be ground. This process causes the ceramic powder particle size to further decrease, which will weaken the core-shell structure concentration gradient of the ceramic after sintering, resulting in unstable capacity temperature change rate. At the same time, the internal electrode slurry will partially diffuse into the ceramic body when co-fired with the ceramic body, playing a role in fluxing and reducing the sintering temperature. When designing small-sized and large-capacity multilayer ceramic capacitors (MLCC), the thickness of the dielectric layer tends to be thinner, which aggravates the role of the internal electrode in assisting sintering, resulting in a weakening of the core-shell structure concentration gradient of the ceramic body. The above two reasons make the capacity temperature change rate of small-sized and large-capacity multilayer ceramic capacitors (MLCC) worse and the dielectric loss increase.
[0010] The temperature-stable capacitor porcelain powder with a core-shell structure of the present invention adds an appropriate amount of dopant during the formulation design, so that when the dielectric is thicker, the residual doping modified substance is attached to the surface of the shell layer. When the dielectric layer becomes thinner, the weakened core-shell structure concentration gradient is compensated, and a stable capacity temperature change rate and a small dielectric loss are maintained. The problem of unstable capacity temperature change rate and increased loss in the X7R characteristic barium titanate-based ceramic material sintered at medium and low temperatures for Pb-Ag inner electrode MLCC in small-size and large-capacity MLCC applications is solved, so that the capacity temperature change rate remains stable, and the dielectric loss and high withstand voltage are maintained.
[0011] The temperature-stable capacitor porcelain powder with a core-shell structure in the present invention has an obvious core-shell structure. After sintering, residual doping and modification substances are attached to the surface of the shell layer, which have not yet been completely dissolved with the shell layer of the main crystal phase. At the positive temperature end of 25°C to 125°C, the dielectric constant increases with increasing temperature, and the increase is in the range of 8% to 15%.
[0012] Furthermore, the amount of TiO2 in the modifier is 2-10wt% of the amount of the main component BaTiO3, the amount of NaCO3 is 0.5-2wt% of the amount of the main component BaTiO3; the amount of Nb2O5 is 1-2wt% of the amount of the main component BaTiO3.
[0013] Furthermore, the components of the modifier also include any one or more of Nd2O3, ZnO, Bi2O3, SrCO3, Al2O3, MnCO3, and Co2O3.
[0014] Furthermore, the amount of Nd2O3 is 0-0.8wt% of the main component BaTiO3; the amount of ZnO is 0-1.2wt% of the main component BaTiO3; the amount of Bi2O3 is 0-2wt% of the main component BaTiO3; the amount of SrCO3 is 0-2wt% of the main component BaTiO3; the amount of Al2O3 is 0.2-1wt% of the main component BaTiO3; the amount of MnCO3 is 0-0.5wt% of the main component BaTiO3; the amount of Co2O3 is 0-0.3wt% of the main component BaTiO3.
[0015] Furthermore, the glass powder is a cooling agent, the amount of the Li-B-Si glass compound is 0.05 to 0.3 wt% of the main component BaTiO3; the amount of the Bi-B glass compound is 0.05 to 0.3 wt% of the main component BaTiO3; the mass ratio of Li:B:Si in the Li-B-Si glass compound is 31:46:23.
[0016] Furthermore, the preparation method of the Li-B-Si glass compound is:
[0017] 1) Weigh LiCO3 powder, B2O3 powder and SiO2 powder according to the proportion, add them into a ball mill, and mix them evenly by wet ball milling;
[0018] 2) Drying the anhydrous ethanol on the uniformly mixed powder, sending the powder into a heating furnace for calcination, and then subjecting the glass material to wet ball milling and drying in sequence to obtain Li-B-Si glass powder.
[0019] Furthermore, the preparation method of the Bi-B glass compound is:
[0020] 1) Weigh Bi2O3 powder and B2O3 powder according to the proportion, add them into a ball mill, and mix them evenly by wet ball milling;
[0021] 2) Drying the anhydrous ethanol on the uniformly mixed powder, sending the powder into a heating furnace for calcination, and then subjecting the glass material to wet ball milling and drying in sequence to obtain Bi-B glass powder.
[0022] Furthermore, the mass ratio of Bi:B in the Bi-B glass compound is 89:11.
[0023] In a second aspect, the present application provides a method for preparing a temperature-stable capacitor porcelain powder having a core-shell structure, comprising the following steps:
[0024] Step 1: Weigh the main crystal phase BaTiO3 powder according to the dosage ratio and grind it by wet vibration ball milling until the particle size D 50 Reach 700-800 μm to obtain slurry A;
[0025] Step 2: Weigh the modifier according to the dosage ratio and grind it by wet vibration ball milling until the particle size is D 50 Reach 200-300 μm to obtain slurry B;
[0026] Step 3: Weigh the glass powder according to the proportion and grind it by wet vibration ball milling until the particle size is D 50 Reach 200-300 μm to obtain slurry C;
[0027] Step 4: Mix slurry B and slurry C, add slurry A after vibration ball milling, continue vibration ball milling to obtain ceramic slurry, and then dry and screen the ceramic slurry in sequence to obtain a temperature-stable capacitor ceramic powder with a core-shell structure.
[0028] The preparation method of the present invention strictly controls the particle sizes of the main components, doping modifiers and glass compounds, and stably controls the particle sizes and activities of the main crystalline phase materials and doping modifiers through abrasive processes and mixing processes, thereby reducing the instability of the core-shell microstructure concentration gradient caused by the abrasive process, solving the problem of the difficulty in accurately controlling the core-shell structure of the barium titanate-based ceramic material with X7R characteristics sintered at medium and low temperatures for Pb-Ag inner electrode MLCC, and improving the consistency of the capacity temperature change rate.
[0029] In a third aspect, the present application provides a capacitor, which is prepared using the temperature-stable capacitor porcelain powder with a core-shell structure or the temperature-stable capacitor porcelain powder with a core-shell structure prepared by the preparation method.
[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0031] (1) The temperature-stable capacitor porcelain powder with a core-shell structure of the present invention is designed with an appropriate amount of dopant, so that when the dielectric is thick, the residual doping modification material is attached to the surface of the shell layer. When the dielectric layer becomes thinner, the weakened core-shell structure concentration gradient is compensated, maintaining a stable capacity temperature change rate and a small dielectric loss. The problem of unstable capacity temperature change rate and increased loss of the X7R characteristic barium titanate-based ceramic material sintered at medium and low temperatures for Pb-Ag internal electrode MLCC in small-size and large-capacity MLCC applications is solved, so that the capacity temperature change rate remains stable, and the dielectric loss and high withstand voltage are maintained;
[0032] (2) The temperature-stable capacitor porcelain powder with a core-shell structure in the present invention has a distinct core-shell structure. After sintering, residual doping and modifying substances are attached to the surface of the shell layer, which have not yet been completely dissolved in the shell layer of the main crystal phase. At the positive temperature end of 25°C to 125°C, the dielectric constant increases with increasing temperature, increasing by about 8% to 15%;
[0033] (3) The preparation method of the present invention strictly controls the particle size of the main component, doping modifier and glass compound, and stably controls the particle size and activity of the main crystalline phase material and the doping modifier through abrasive process and mixing process, thereby reducing the instability of the core-shell microstructure concentration gradient caused by the abrasive process, solving the problem of the difficulty in accurately controlling the core-shell structure of the barium titanate-based ceramic material with X7R characteristics sintered at medium and low temperatures for Pb-Ag internal electrode MLCC, and improving the consistency of the capacity temperature change rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:
[0035] Figure 1 This is a SEM image of a wafer sample prepared by the method of Example 1 of the present invention;
[0036] Figure 2 This is a SEM image of an MLCC sample prepared by the method of Example 1 of the present invention;
[0037] Figure 3 This is a SEM image of a wafer sample prepared by the method of Example 3 of the present invention;
[0038] Figure 4 This is a SEM image of an MLCC sample prepared by the method of Example 3 of the present invention;
[0039] Figure 5 This is a SEM image of a wafer sample prepared by the method of Example 6 of the present invention;
[0040] Figure 6 This is a SEM image of an MLCC sample prepared by the method of Example 6 of the present invention;
[0041] Figure 7 is a SEM image of a wafer sample prepared by the method of Example 8 of the present invention;
[0042] Figure 8 This is a SEM image of an MLCC sample prepared by the method of Example 8 of the present invention;
[0043] Fig. 9 is a SEM image of a wafer sample prepared by the method of Example 9 of the present invention;
[0044] Fig.10 This is a SEM image of an MLCC sample prepared by the method of Example 9 of the present invention. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0046] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Example 1
[0048] This embodiment provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure, the formula and dosage of which are: 100g BaTiO3, 4g TiO2, 1.2g NaCO3, 1g Nb2O5, 0.8g Nd2O3, 0.32g ZnO, 0.2g Al2O3, 0.3g Li-B-Si glass compound, and 0.1g Bi-B glass compound.
[0049] Wherein, the preparation method of Li-B-Si glass compound is:
[0050] 1) Weigh 31g LiCO3 powder, 46g B2O3 powder, and 23g SiO2 powder, add them into a ball mill, and mix them evenly by wet ball milling; wherein the total mass of LiCO3 powder, B2O3 powder, and SiO2 powder: ball milling medium: anhydrous ethanol = 1:5:1;
[0051] 2) Drying the anhydrous ethanol on the uniformly mixed powder, sending the powder into a heating furnace and calcining it at 800° C. for 2.5 hours, and then wet ball milling and drying the glass material to obtain Li-B-Si glass powder.
[0052] Wherein, the preparation method of Bi-B glass compound is:
[0053] 1) Weigh 89g Bi2O3 powder and 11g B2O3 powder, add them into a ball mill, and mix them evenly by wet ball milling; wherein the total weight of Bi2O3 powder and B2O3 powder: ball milling medium: anhydrous ethanol = 1:5:1;
[0054] 2) Drying the anhydrous ethanol on the uniformly mixed powder, sending the powder into a heating furnace and calcining it at 600° C. for 2.5 hours, and then wet ball milling and drying the glass material to obtain Bi-B glass powder.
[0055] The preparation method of the temperature-stable capacitor porcelain powder with a core-shell structure is as follows:
[0056] S1: Weigh 100g of the main crystalline phase BaTiO3 powder and perform wet vibration ball milling according to the weight ratio of BaTiO3 powder: ball milling medium: deionized water = 1:5:1.4. During the ball milling process, the particle size is detected until the particle size D 50 Reach 750 μm to obtain slurry A;
[0057] S2: Weigh 4 g TiO2, 1.2 g NaCO3, 1 g Nb2O5, 0.8 g Nd2O3, 0.32 g ZnO, and 0.2 g Al2O3, and perform wet vibration ball milling according to the weight ratio of total mass of TiO2, NaCO3, Nb2O5, Nd2O3, ZnO, and Al2O3: ball milling medium: deionized water = 1:5:1.4. During the ball milling process, the particle size is detected until the particle size D 50 Reach 250 μm to obtain slurry B;
[0058] S3: Weigh 0.3 g of Li-B-Si glass compound and 0.1 g of Bi-B glass compound, and perform wet vibration ball milling according to the weight ratio of total mass of Li-B-Si glass compound and Bi-B glass compound: ball milling medium: deionized water = 1:5:1. During the ball milling process, the particle size is detected until the particle size D 50 Reach 250 μm to obtain slurry C;
[0059] S4: Slurry B and slurry C are mixed, and slurry A is added after vibration ball milling, and vibration ball milling is continued for 0.5 hours to obtain ceramic slurry, and then the ceramic slurry is dried and sieved in sequence to obtain a temperature-stable capacitor ceramic powder with a core-shell structure.
[0060] Among them, the ball milling media used in S1 to S4 are all zirconium balls.
[0061] Example 2
[0062] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that the formula and dosage used in this example are: 100g BaTiO3, 4g TiO2, 1.2g NaCO3, 2g Nb2O5, 0.6g Nd2O3, 0.32g ZnO, 0.2g Al2O3, 0.02g MnCO3, 0.3g Li-B-Si glass compound, and 0.1g Bi-B glass compound. Other technical features are exactly the same as those in Example 1.
[0063] Example 3
[0064] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that the formula and dosage used in this example are: 100g BaTiO3, 4g TiO2, 1.2g NaCO3, 2g Nb2O5, 0.6g Nd2O3, 0.32g ZnO, 0.2g Al2O3, 0.02g MnCO3, 0.1g Co2O3, 0.3g Li-B-Si glass compound, and 0.1g Bi-B glass compound. Other technical features are exactly the same as those in Example 1.
[0065] Example 4
[0066] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that the formula and dosage used in this example are: 100g BaTiO3, 7g TiO2, 2g NaCO3, 1.5g Nb2O5, 1.2g ZnO, 2g Bi2O3, 2g SrCO3, 1g Al2O3, 0.3g Co2O3, 0.1g Li-B-Si glass compound, and 0.05g Bi-B glass compound. Other technical features are exactly the same as those in Example 1.
[0067] Example 5
[0068] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that the formula and dosage used in this example are: 100g BaTiO3, 7g TiO2, 2g NaCO3, 2g Nb2O5, 0.2g Nd2O3, 1.2g ZnO, 2g Bi2O3, 2g SrCO3, 1g Al2O3, 0.02g MnCO3, 0.3g Co2O3, 0.1g Li-B-Si glass compound, 0.05g Bi-B glass compound. Other technical features are exactly the same as those in Example 1.
[0069] Example 6
[0070] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that the formula and dosage used in this example are: 100g BaTiO3, 6g TiO2, 1.4g NaCO3, 1.5g Nb2O5, 0.4g Nd2O3, 1g ZnO, 1g Bi2O3, 1g SrCO3, 0.5g Al2O3, 0.02g MnCO3, 0.2g Co2O3, 0.15g Li-B-Si glass compound, 0.05g Bi-B glass compound. Other technical features are exactly the same as those in Example 1.
[0071] Example 7
[0072] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that the formula and dosage used in this example are: 100g BaTiO3, 2g TiO2, 0.5g NaCO3, 1.5g Nb2O5, 0.5g Nd2O3, 0.5g Bi2O3, 1g Al2O3, 0.5g MnCO3, 0.1g Co2O3, 0.05g Li-B-Si glass compound, and 0.3g Bi-B glass compound. Other technical features are exactly the same as those in Example 1.
[0073] Example 8
[0074] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that when this example prepares a temperature-stable capacitor porcelain powder with a core-shell structure, the particle size D of the slurry A is 50 The other technical features are exactly the same as those in Example 1.
[0075] Example 9
[0076] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that when this example prepares a temperature-stable capacitor porcelain powder with a core-shell structure, the particle size D of the slurry A is 50 The other technical features are exactly the same as those in Example 1.
[0077] Example 10
[0078] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that when this example prepares a temperature-stable capacitor porcelain powder with a core-shell structure, the particle size D of the slurry B is 50The other technical features are exactly the same as those in Example 1.
[0079] Embodiment 11
[0080] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that when this example prepares a temperature-stable capacitor porcelain powder with a core-shell structure, the particle size D of the slurry B is 50 The other technical features are exactly the same as those in Example 1.
[0081] Example 12
[0082] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that when this example prepares a temperature-stable capacitor porcelain powder with a core-shell structure, the particle size D of the slurry C is 50 The other technical features are exactly the same as those in Example 1.
[0083] Embodiment 13
[0084] Based on Example 1, this example provides a method for preparing a temperature-stable capacitor porcelain powder with a core-shell structure. The difference from Example 1 is that when this example prepares a temperature-stable capacitor porcelain powder with a core-shell structure, the particle size D of the slurry C is 50 The other technical features are exactly the same as those in Example 1.
[0085] The temperature-stable capacitor ceramic powder with a core-shell structure prepared by the methods of Examples 1 to 13 was prepared into test samples for performance testing.
[0086] (1) Preparation of disc samples: 8 wt% paraffin wax was added to the prepared ceramic powder to make granules, which were pressed into discs using a hydraulic press. The temperature was then raised to 450°C at a rate of 2°C / min to expel the binder, and then raised to 1160°C at a rate of 3°C / min. After sintering for 3 hours, the discs were cooled in the furnace to obtain disc test samples.
[0087] (2) Preparation of MLCC samples: The prepared ceramic powder is ball-milled with zirconium oxide balls, toluene, ethanol, etc. in a ratio of 1:5:1.5. After 2 hours, 8 wt% of a binder is added. After 28 hours of ball-milling, a ceramic slurry is prepared. The ceramic slurry is cast on a spray-type casting machine to form a film strip. The film strip is printed with an internal electrode slurry and dried on a printing machine. The film strip printed with the internal electrode and the blank film strip are stacked in a design with an outer size of (2.3±0.20) mm×(1.6±0.20) mm, the number of internal electrodes connected in series is 1, and the number of internal electrode layers is not less than 20 to prepare a green bar block. The bar block is further pressurized and compacted by a warm isostatic press, and the green bar block is cut on a cutting machine to form a capacitor green body. The temperature is then raised to 550°C at a rate of 1°C / min to discharge the binder, and then raised to 1140°C at a rate of 1.5°C / min. After sintering for 3 hours, it is cooled in the furnace to prepare an MLCC test sample. The test results are shown in the following table.
[0088] Table 1 Performance list of ceramic powder disc samples
[0089]
[0090] Table 2 MLCC capacitor sample performance list
[0091]
[0092]
[0093] As shown in Table 1, Examples 1 to 13 of the present invention achieve a temperature-stable capacitor porcelain powder formula with X7R characteristics by doping BaTiO3 with modifiers and glass powder. The main modifiers TiO2, NaCO3 and Nb2O5 are the basis for the core-shell structure of the ceramic grains, and the composite doping of Nd2O3, ZnO, Bi2O 、 SrCO3 and Al2O3 promote the chemical reaction of shell structure materials, increase the shell structure concentration, further optimize and stabilize the capacity-temperature characteristics, trace doping of MnCO3 and Co2O3 optimizes dielectric loss and insulation properties, adding Li-B-Si glass compounds and Bi-B glass compounds to form a glass liquid phase, accelerate chemical reactions, promote sintering, and reduce the sintering temperature into porcelain.
[0094] In the abrasive process of Examples 1 to 13 of the present invention, the particle sizes of the main component, the doping modifier and the glass compound are strictly controlled. In Examples 1, 8 and 9, under the premise that other technical conditions remain unchanged, the particle size D of the main component of slurry A is 50 The particle size of the modified agent in slurry B is controlled to be 750μm, 700μm, and 800μm. In Example 1, Example 10, and Example 11, under the premise that other technical conditions remain unchanged, the particle size D of the modified agent in slurry B is 50The particle size of the glass compound in slurry C is controlled to be 250μm, 200μm, and 300μm. In Example 1, Example 12, and Example 13, under the premise that other technical conditions remain unchanged, the particle size D of the glass compound in slurry C is 50 The particle sizes of the main component of slurry A and the doped modifier of slurry B are controlled to be 250μm, 200μm, and 300μm. It can be seen from Table 1 that the particle sizes of the main component of slurry A and the doped modifier of slurry B are 50 The influence on the capacity temperature change rate is greater. The particle size of the main component of slurry A is D 50 Increase or dope the particle size D of the slurry B with the modifier 50 The capacity temperature change gradually increases. The glass compound in slurry C promotes sintering, and the particle size D 50 Reduced, insulation resistance and insulation strength improved.
[0095] It can be seen from Table 2 that after the temperature-stable capacitor porcelain powder with a core-shell structure of Examples 1 to 13 of the present invention is prepared into MLCC samples, compared with the electrical properties of the wafer samples, the sintering temperature is reduced, the insulation resistance is reduced, the dielectric loss is increased, and the capacity temperature change rate fluctuates greatly. In particular, the capacitance change rate of the MLCC sample with a dielectric thickness of 10 μm is reduced by about 10% after the temperature is increased from 25°C to 125°C compared with the wafer sample. These changes in electrical properties are due to the fact that in the preparation process of MLCC, in order to fully mix the porcelain powder and the organic solvent, the porcelain powder and the organic solvent mixture need to be ground. This process causes the porcelain powder particle size to further decrease, which will weaken the core-shell structure concentration gradient of the ceramic grains after sintering into porcelain, thereby causing changes in electrical properties, especially the capacity-temperature change rate. At the same time, the inner electrode metal slurry will partially diffuse into the porcelain body when co-fired with the porcelain body, which plays a role in fluxing and lowering the sintering temperature. The thinner the thickness of the single-layer porcelain film medium, the more aggravated the diffusion and fluxing effect of the inner electrode metal electrode, and the weaker the core-shell structure concentration gradient of the ceramic grains, the greater the change in the electrical properties of the MLCC.
[0096] In view of the development trend of thin-layer MLCC ceramic film dielectrics, the present invention fully considers the characteristics of increased dielectric loss after being prepared into MLCC and a significant decrease in the temperature change rate of capacity when the temperature rises from 25°C to 125°C when designing the ceramic powder formula, and invents a temperature-stable capacitor ceramic powder with a core-shell structure. Through the design of the ceramic powder formula components, the ceramic body grains present a core-shell structure after sintering, and residual doping and modifying substances are attached to the surface of the shell layer, which have not yet completely dissolved with the shell layer of the main crystal phase. At the positive temperature end of 25°C to 125°C, the dielectric constant increases with increasing temperature, and the increase is controlled to be within the range of 8% to 15%. At the same time, it also has a small dielectric loss. The electrical properties obtained by the ceramic powder formula component design can still maintain a capacity temperature change rate within ±15% at the positive temperature end of 25°C to 125°C after being prepared into MLCC with a thin dielectric layer. At the same time, the dielectric loss is small and the withstand voltage is high.
[0097] The present invention, based on the precise control of the ceramic powder formula components, strictly controls the particle sizes of the main components, doping modifiers and glass compounds through certain abrasive processes and mixing processes, reduces the concentration gradient fluctuation of the core-shell structure caused by the abrasive process, and improves the capacity temperature change rate stability of the Pb-Ag inner electrode MLCC prepared from barium titanate-based ceramic materials with X7R characteristics.
[0098] The wafer samples and MLCC samples made of temperature-stable capacitor porcelain powder with a core-shell structure prepared by the methods of Examples 1, 3, 6, 8 and 9 were microscopically inspected using an electron microscope. The electron microscope images are shown in FIG. Figures 1 to 10 shown.
[0099] Depend on Figures 1 to 5 It can be seen that the disc samples made of temperature-stable capacitor porcelain powder with a core-shell structure prepared by the methods of Example 1, Example 3, Example 6, Example 8, and Example 9 have more residual doping and modifying substances attached to the surface of the grain shell layer, among which the residual doping and modifying substances on the surface of the grain shell layer of Example 6 is the largest, and its capacity change rate with temperature is the largest when the temperature rises from 25°C to 125°C, which is +14.33%. On the contrary, the residual doping and modifying substances on the surface of the grain shell layer of Example 8 are less, and its capacity change rate with temperature is relatively small when the temperature rises from 25°C to 125°C.
[0100] After the temperature-stable capacitor ceramic powder with a core-shell structure prepared by the methods of Examples 1, 3, 6, 8, and 9 is prepared into MLCC, the ceramic powder is further ground during the preparation of the MLCC, so that the particle size of the ceramic powder is further reduced, the specific surface area of the ceramic powder particles is increased, and the doped modified substance is more likely to react during the sintering process and diffuse into the lattice of the main crystal phase grains. Figures 6 to 10 It can be seen that the residual doping modification substances on the surface of the grain shell are greatly reduced compared with the wafer sample, which weakens the concentration gradient of the core-shell structure. Therefore, the rate of change of capacity with temperature is significantly reduced relative to the wafer sample when the temperature rises from 25°C to 125°C.
[0101] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A temperature-stable capacitor ceramic powder with a core-shell structure, It is characterized in that The main component is BaTiO 3 , the BaTiO 3 The modifier and glass powder are doped in the present invention; the modifier comprises TiO 2 、NaCO 3 and Nb 2 O 5 ; The glass powder includes Li-B-Si glass compound and Bi-B glass compound.
2. The temperature-stable capacitor porcelain powder with a core-shell structure according to claim 1, It is characterized in that The modifier contains TiO 2 The dosage is the main component BaTiO 3 The dosage is 2~10wt%, NaCO 3 The dosage is the main component BaTiO 3 0.5~2wt% of dosage; Nb 2 O 5 The dosage is the main component BaTiO 3 The dosage is 1-2 wt%.
3. The temperature-stable capacitor porcelain powder with a core-shell structure according to claim 1, It is characterized in that The modifier also includes Nd 2 O 3 、ZnO、Bi 2 O 3 、SrCO 3 、Al 2 O 3 、MnCO 3 、Co 2 O 3 Any one or more of .
4. The temperature-stable capacitor porcelain powder with a core-shell structure according to claim 3, It is characterized in that Nd 2 O 3 The dosage is the main component BaTiO 3 The dosage is 0~0.8wt%; the dosage of ZnO is the main component BaTiO 3 Dosage 0~1.2wt%; Bi 2 O 3 The dosage is the main component BaTiO 3 Dosage 0~2wt%; SrCO 3 The dosage is the main component BaTiO 3 Dosage 0~2wt%; Al 2 O 3 The dosage is the main component BaTiO 3 Dosage: 0.2~1wt%; MnCO 3 The dosage is the main component BaTiO 3 Dosage 0~0.5wt%; Co 2 O 3 The dosage is the main component BaTiO 3 The dosage is 0~0.3wt%.
5. The temperature-stable capacitor porcelain powder with a core-shell structure according to claim 1, It is characterized in that The glass powder is a cooling agent, and the amount of the Li-B-Si glass compound is the main component BaTiO 3 0.05~0.3wt% of dosage; The amount of the Bi-B glass compound is the main component BaTiO 3 The dosage is 0.05-0.3wt%; the mass ratio of Li:B:Si in the Li-B-Si glass compound is 31:46:
23.
6. The temperature-stable capacitor porcelain powder with a core-shell structure according to claim 5, It is characterized in that The preparation method of the Li-B-Si glass compound is: 1) Weigh LiCO in proportion 3 Powder, B 2 O 3 Powder, SiO 2 The powder is added into the ball mill and mixed evenly by wet ball milling; 2) Drying the anhydrous ethanol on the uniformly mixed powder, sending the powder into a heating furnace for calcination, and then subjecting the glass material to wet ball milling and drying in sequence to obtain Li-B-Si glass powder.
7. The temperature-stable capacitor porcelain powder with a core-shell structure according to claim 5, It is characterized in that The preparation method of the Bi-B glass compound is: 1) Weigh Bi in proportion 2 O 3 Powder, B 2 O 3 The powder is added into the ball mill and mixed evenly by wet ball milling; 2) Drying the anhydrous ethanol on the uniformly mixed powder, sending the powder into a heating furnace for calcination, and then subjecting the glass material to wet ball milling and drying in sequence to obtain Bi-B glass powder.
8. The temperature-stable capacitor porcelain powder with a core-shell structure according to claim 1, It is characterized in that The mass ratio of Bi:B in the Bi-B glass compound is 89:
11.
9. A method for preparing a temperature-stable capacitor ceramic powder having a core-shell structure as claimed in any one of claims 1 to 7, It is characterized in that The following steps are involved: Step 1: Weigh the main crystal phase BaTiO according to the dosage ratio 3 The powder is ground by wet vibration ball milling until the particle size D 50 Reach 700-800 μm to obtain slurry A; Step 2: Weigh the modifier according to the dosage ratio and grind it by wet vibration ball milling until the particle size is D 50 Reach 200-300 μm to obtain slurry B; Step 3: Weigh the glass powder according to the proportion and grind it by wet vibration ball milling until the particle size is D 50 Reach 200-300 μm to obtain slurry C; Step 4: Mix slurry B and slurry C, add slurry A after vibration ball milling, continue vibration ball milling to obtain ceramic slurry, and then dry and screen the ceramic slurry in sequence to obtain a temperature-stable capacitor ceramic powder with a core-shell structure.
10. A temperature-stable capacitor porcelain powder with a core-shell structure as claimed in any one of claims 1 to 7 or a temperature-stable capacitor porcelain powder with a core-shell structure prepared by the preparation method of claim 9 for use in preparing capacitors.
Citation Information
Patent Citations
High-performance BaTiO3-based ceramic dielectric material with core-shell structure and preparation method thereof
CN112174658A
Dielectric material for barium titanate-based X8R type multilayer ceramic capacitor and preparation method
CN112479705A
TiO2 (at) SiO2 (at) BaTiO3 composite ceramic powder material as well as preparation method and application thereof
CN115565781A
Ultralow-temperature sintered X7R dielectric material, preparation method and product prepared from ultralow-temperature sintered X7R dielectric material
CN117185803A
Secondary hydrothermal crystallization preparation method of nano-modified barium titanate-based formula powder with core-shell structure
CN117361611A
Cited By
Direct-current bias characteristic X7R ceramic dielectric material and preparation method thereof
CN122187484A